A method for preparing high-dislocation density nanocrystalline ceramics
By combining rapid sintering and secondary oscillation pressure forging, the problem of improving the toughness of ceramic materials while maintaining high strength and high temperature resistance has been solved. This has enabled the preparation of nanocrystalline ceramic materials with high density and high fault density, improving the overall performance of the materials and making them suitable for aerospace and nuclear energy equipment.
Patent Information
- Application Number
- CN202611129983.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-28
- Publication Date
- 2026-11-10
AI Technical Summary
Existing technologies struggle to significantly improve the toughness of ceramic materials while maintaining their high strength and high-temperature resistance. Furthermore, traditional preparation methods often fail to achieve a balance between macroscopic densification and microscopic defect structure control, thus limiting the application of ceramic materials in high-reliability structural components.
By employing rapid sintering technology combined with secondary oscillating pressure forging, nano-ceramic powder is rapidly sintered at high temperature for a short time, and oscillating pressure is applied during the sintering process to achieve stable maintenance of nanoscale grains and formation of high layer fault density, thus preparing high-density, nanocrystalline ceramic materials.
It achieves high densification, nanocrystalline structure and high fault density in ceramic materials, significantly improving the hardness and toughness of the materials, simplifying the process, reducing costs, and is suitable for aerospace, nuclear energy equipment and high-temperature structural components and other fields.
Smart Images

Figure CN123062272A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of ceramic material preparation technology, specifically relating to a method for preparing high-density nanocrystalline ceramics with high fault density. Background Technology
[0002] Ceramic materials, due to their high hardness, high melting point, excellent corrosion resistance, good thermal conductivity, and superior high-temperature mechanical properties, have been widely used in aerospace, nuclear engineering, semiconductor devices, and extreme environment protection. However, traditional ceramics generally suffer from high brittleness and low fracture toughness, which severely limits their further application in high-reliability structural components. Therefore, how to significantly improve their toughness while maintaining their high strength and high-temperature resistance has become a key focus and challenge in the field of ceramic materials research in recent years.
[0003] Among numerous toughening strategies, introducing a higher density of stacking faults by manipulating the microstructure is considered a highly promising approach. Stacking faults are a typical crystal defect, essentially localized dislocations within a crystal stacking sequence. Previous studies have shown that introducing high stacking fault density structures can simultaneously improve the hardness and toughness of materials, essentially stemming from the multiple regulatory effects of stacking faults on crystal structure, dislocation motion, and crack propagation behavior. This strengthening and toughening mechanism is a synergistic effect achieved through nanoscale defect engineering.
[0004] First, from the perspective of the hardness enhancement mechanism, stacking faults, as a type of planar defect, disrupt the original long-range ordered stacking structure in a crystal. On one hand, stacking fault interfaces can act as barriers to dislocation slip, causing dislocations to accumulate or change direction during their movement; on the other hand, stacking faults also alter the local stress field distribution of the crystal, increasing the critical stress required for dislocation nucleation. Therefore, by hindering dislocation nucleation and free movement, stacking faults enable materials to exhibit higher resistance to deformation, which macroscopically manifests as an increase in hardness.
[0005] Secondly, regarding toughness enhancement, stacking fault structures inhibit crack propagation through multiple mechanisms. Traditional silicon carbide ceramics, lacking effective energy dissipation mechanisms, experience rapid crack propagation once formed, leading to brittle fracture. The introduction of stacking faults alters this process. Specifically, when a crack encounters a stacking fault interface during propagation, it deflects, branches, or even becomes blunted. This increased crack path complexity significantly increases the energy required for crack propagation, thereby improving the material's fracture toughness.
[0006] In summary, stacking fault structures achieve a balance between strengthening and toughening in ceramics through two core mechanisms: "increasing hardness by hindering dislocation movement" and "enhancing toughness by regulating crack propagation." This is also one of the important research directions for optimizing high-performance structural ceramics through defect engineering.
[0007] Meanwhile, nanocrystalline ceramics, due to their small grain size and high interface ratio, exhibit mechanical behaviors different from traditional coarse-grained materials. At the nanoscale, grain boundaries have a stronger inhibitory effect on crack propagation, while also providing favorable conditions for the formation and stabilization of stacking faults. Therefore, combining "nanocrystalline structure" with "high stacking fault density structure" is considered an effective way to significantly improve the overall performance of silicon carbide. However, in the actual fabrication process, how to precisely control the density and distribution of stacking faults while achieving grain refinement still faces many technical challenges.
[0008] Currently, common methods for preparing ceramic materials include pressureless sintering, hot pressing, hot isostatic pressing, and spark plasma sintering (SPS). While these methods have made some progress in densification, they often struggle to achieve a balance between macroscopic densification and microscopic defect structure control. For example, high-temperature, long-duration hot pressing is beneficial for increasing density but can easily lead to grain growth, thereby reducing stacking fault density; while rapid sintering can suppress grain growth, its ability to controllably introduce stacking fault structures is limited.
[0009] In recent years, some studies have attempted to promote stacking fault formation through external field manipulation (such as pressure and electric fields), doping modification, or precursor engineering. For example, introducing specific element doping can alter crystal growth kinetics, thereby inducing stacking fault formation; non-equilibrium sintering conditions can be used to "freeze" stacking fault structures during rapid crystal growth. However, these methods often suffer from complex processes, poor reproducibility, or high costs, making it difficult to meet the needs of industrial applications.
[0010] In summary, conducting systematic and in-depth research on the preparation technology of nanocrystalline ceramics with high stacking fault density structures not only helps to reveal the mechanism by which stacking fault structures enhance the mechanical properties of materials, but also provides new ideas and technical paths for the design and preparation of high-performance ceramic materials, which has significant scientific and engineering application value. However, how to prepare and maintain nanocrystalline structures in a low-cost and simple manner is a key technical bottleneck in the nanostructuring of ceramic materials. Therefore, there is an urgent need to develop a method for preparing nanocrystalline ceramic materials with high stacking fault density that is process-controllable, structurally designable, and suitable for large-scale preparation. This method requires synergistic optimization in raw material design, sintering process, and microstructure control. It must not only ensure the high density and fine-grained structure of the material, but also effectively control the type, density, and spatial distribution of stacking faults, thereby achieving precise control over crack propagation behavior at the microscale. Summary of the Invention
[0011] In view of this, the present invention addresses two major technical challenges in the preparation of existing nanocrystalline ceramic materials, and provides a method for preparing high-layer fault density nanocrystalline ceramics, including the following dual innovative strategies: In terms of nanocrystallization, this invention utilizes the short-time high-temperature characteristics of rapid sintering technology to sinter nanoscale crystalline ceramics, effectively suppressing the abnormal growth of nanocrystals in traditional sintering, thereby stabilizing the nanocrystalline microstructure.
[0012] In terms of controlling the stacking fault structure, this invention adopts the technical route of "rapid sintering + secondary oscillating pressure forging": utilizing the high sintering activity of nano-ceramic powder, pre-sintering is carried out at a lower temperature to obtain ceramics with a certain strength; more importantly, oscillating pressure is introduced during the rapid sintering process to perform secondary forging sintering on the pre-sintered ceramics, which can generate large shear deformation inside the ceramics, and most areas can undergo free plastic deformation, thereby generating a high-density stacking fault structure, which is ultimately retained.
[0013] This method can solve the two major technical problems mentioned above simultaneously in a shorter time and under milder sintering conditions, and obtain nanocrystalline ceramics with high density, nanocrystalline structure, uniform distribution of sintering aids, high layer fault density, and excellent mechanical properties.
[0014] To achieve the above objectives, the present invention provides a method for preparing high-level fault density nanocrystalline ceramics, comprising the following steps: a) Preparation of nanomaterials: Grind and sieve the nano-ceramic powder for subsequent sintering; if sintering aids are required, mix the sieved nano-ceramic powder and nano-sintering aids evenly to obtain a mixed powder. b) Rapid pre-sintering: The mixed powder obtained in step a) is placed in a rapid sintering equipment and rapidly pre-sintered under vacuum or argon atmosphere to obtain pre-sintered ceramics; c) Secondary oscillation forging sintering: The pre-sintered ceramic obtained in step b) is placed in a rapid sintering equipment to give the pre-sintered ceramic lateral deformation space. Axial oscillation pressure is applied during rapid sintering to forge the ceramic. After cooling, the nanocrystalline ceramic is obtained.
[0015] Preferably, in step a), the ceramic powder is selected from a mixture of one or more of silicon carbide, boron carbide, titanium carbide, hafnium carbide, zirconium carbide, and niobium carbide, or a high-entropy carbide (high-entropy carbide refers to a ceramic formed by five or more transition metal elements and carbon in solid solution), preferably silicon carbide or boron carbide. Specifically, the nano-silicon carbide powder is selected from at least one of β-SiC or α-SiC with an average particle size between 10-200 nm; the nano-boron carbide powder has an average particle size between 10-1000 nm. These two powders are representative of difficult-to-sinter carbide ceramics. The fundamental reason for their extreme difficulty in sintering lies in their extremely high covalent bond ratio (~88% and >90%), resulting in an extremely low atomic diffusion coefficient and severely insufficient sintering driving force.
[0016] Preferably, in step a), the sieve mesh size is 100-400 mesh. The sintering aid includes a liquid-phase sintering aid and a solid-phase sintering aid. The liquid-phase sintering aid is selected from at least two combinations of Al2O3 and Y2O3, MgO, CaO, La2O3, CeO2, Nd2O3, Sm2O3, and Yb2O3, or one or more combinations of AlN and Y2O3, MgO, CaO, La2O3, CeO2, Nd2O3, Sm2O3, and Yb2O3. The solid-phase sintering aid is selected from at least one of B4C, AlN, BN, and C. If nano-silicon carbide powder is selected as the ceramic powder, liquid-phase or solid-phase sintering aid needs to be added according to the above combination; if nano-boron carbide powder is selected, no sintering aid needs to be added.
[0017] Preferably, in step a), the amount of sintering aid added is 0-20 wt% of the total mass of raw materials, preferably 5-10 wt%, based on a total raw material mass of 100 wt%. A combination of Al2O3 and Y2O3 is preferably used as the aid, with a mass ratio of (5-7):(3-5), more preferably 6:4.
[0018] Preferably, in step a), when mixing the nano-ceramic powder and the sintering aid, a binder or dispersant is also added.
[0019] Preferably, in step a), the mixing method is one or two of ultrasonic dispersion, wet ball milling, or dry ball milling. Preferably, the nanoparticles are mixed using an "ice-water bath ultrasonic dispersion + wet ball milling" method, i.e., first ultrasonic dispersion in an ice-water bath, followed by wet ball milling. The ultrasonic frequency is 20-40 kHz, the duration is 5-10 min, the high-energy ball milling speed is 200-400 rpm, and the milling time is 6-12 h. Because nanoparticles have a large specific surface area and are prone to agglomeration, if a wet ball milling method is used, a nano-ceramic powder slurry is first prepared, and nano-sintering aid powder is gradually added under magnetic stirring to initially mix the two, which can avoid powder agglomeration and adhesion to a certain extent. Ultrasonic dispersion technology, due to the cavitation and acoustic flow effects of ultrasound, can maximize the breaking up of agglomerated nanoparticles. Dispersants can also be added to disperse the nanoparticles by changing the surface charge state of the nanoparticles. This step is a necessary prerequisite for ensuring the uniformity of the final ceramic microstructure.
[0020] Preferably, in step b), the pre-sintering temperature is 1200-2000℃, the pre-sintering pressure is 10-200 MPa, the heating rate is 100℃ / min-1000℃ / s, and the holding time is 1-10 min. This invention utilizes the short-time high-temperature characteristics of rapid pre-sintering technology to obtain nanoscale grain ceramics, effectively suppressing the abnormal growth of nanocrystals in traditional sintering, thereby stabilizing the nanocrystalline microstructure. By controlling the sintering time and temperature, the obtained pre-sintered ceramic is ensured to have a certain strength, laying the foundation for subsequent secondary oscillation forging. If the sintering temperature is too low, the pre-sintered ceramic has very low strength, and the material is easily broken during subsequent secondary forging; if the sintering temperature is too high, the pre-sintered ceramic has too high strength, and the material is difficult to deform as a whole during secondary forging, failing to produce a high-layer fault density structure.
[0021] Preferably, in step c), the sintering process is selected from one of spark plasma sintering (SPS), electric field assisted pressure sintering, and Joule heating.
[0022] Preferably, in step c), the sintering process adopts discharge plasma sintering, with a sintering temperature of 1200-2000°C and a sintering time of 1-10 min; the forging temperature is 1200-2000°C, the forging pressure is 10-200 MPa, the amplitude is 10-100 MPa, the oscillation frequency is 0.1-100 Hz, the heating rate is 100°C / min-1000°C / min, and the holding time is 1-10 min.
[0023] Furthermore, both the pre-sintering in step b) and the forging sintering in step c) require the use of molds. During pre-sintering, the powder completely fills the mold, and the material undergoes primarily axial compressive deformation with relatively small circumferential deformation. During forging sintering, the pre-sintered ceramic is placed in a larger mold, ensuring that the material can undergo unrestricted shear deformation in the circumferential direction during forging, thereby significantly enhancing the stacking fault density within the ceramic.
[0024] This invention involves placing the pre-sintered ceramic into a larger mold for secondary oscillatory forging sintering. Using a shorter sintering time and lower sintering temperature ensures that the grains do not grow excessively. The introduction of oscillatory pressure provides additional sintering driving force to promote densification. Furthermore, the forging sintering process causes significant shear plastic deformation in most areas of the material while simultaneously densifying it, allowing densification and stacking fault generation to occur simultaneously. Through precise control of the above process parameters, nanocrystalline ceramics with uniformly distributed sintering aids at grain boundaries, a dense microstructure, and high stacking fault density can be obtained.
[0025] This invention also provides nanocrystalline ceramic materials with high hierarchical density prepared by the method, including nanocrystalline silicon carbide ceramics and nanocrystalline boron carbide ceramics. The nanocrystalline silicon carbide ceramics have a relative density ≥97%, a micro Vickers hardness ≥20 GPa, and a fracture toughness ≥4 MPa·m. 1 / 2 The relative density of nanocrystalline boron carbide ceramics is ≥97%, the micro Vickers hardness is ≥35 GPa, and the fracture toughness is ≥2 MPa·m. 1 / 2 .
[0026] Compared with the prior art, the present invention has the following beneficial effects: I. Innovative Advantages in Nanocrystallization 1. The nanocrystalline structure remains stable: By employing rapid sintering technology, nanoscale grains are rapidly sintered and densified at high temperatures for a short time (1-10 min), effectively suppressing abnormal growth of nanocrystals in traditional long-time sintering, as well as localized abnormal grain growth and localized porosity caused by uneven distribution of sintering aids. This method maintains the stable microstructure of nanocrystals while ensuring density, thereby fully leveraging the performance improvements brought about by the fine grain strengthening and high layer fault density of nanocrystals.
[0027] 2. Synergistic effect of grain refinement and densification: The short-time high-temperature characteristics of the rapid sintering process and the introduction of oscillating pressure not only achieve high material densification (relative density ≥97%), but also maintain nanoscale grain size, obtaining the best combination of high density and nanocrystalline structure, and significantly improving the mechanical properties of the material through the nanocrystalline strengthening effect.
[0028] II. Innovative Advantages in Regulating Microstructure
[0029] 3. The nano-material powder exhibits good dispersibility: By utilizing ice-water bath ultrasonic dispersion technology, uniform dispersion of nano-ceramic powder and nano-sintering aids can be achieved during the slurry mixing stage, avoiding the agglomeration problem of traditional ball milling. This ensures that the sintering aids are truly uniformly distributed among the ceramic powders, guaranteeing that the ceramics obtained after subsequent sintering have a uniform microstructure.
[0030] 4. Densification and the formation of stacking fault structures occur simultaneously: During the rapid secondary oscillation forging sintering of pre-sintered ceramics, the applied oscillation pressure will generate a large shear force inside the ceramic. Since there is no mold binding effect around the material, the material will undergo significant grain rearrangement and plastic deformation inside the grain, thereby simultaneously increasing the stacking fault density during the ceramic densification process.
[0031] III. Technological and Overall Performance Advantages
[0032] 5. Simple and efficient process: Compared with traditional ceramic sintering processes such as pressureless sintering, hot pressing sintering, and spark plasma sintering, this invention only uses two sintering processes that take no more than 10 minutes each. It has fewer process steps, higher sintering efficiency, and does not require long sintering time or complex preliminary raw material and sintering preparation work. The production cycle is short and the repeatability is high. Compared with spark plasma sintering, this invention has a shorter sintering cycle and can more effectively control the stacking fault density and maintain the ceramic nanocrystalline structure.
[0033] 6. Excellent overall performance: The obtained high-density SiC nanocrystalline ceramic material has a dense structure (relative density ≥ 97%), uniform distribution of sintering aids, and stable nanocrystalline structure. It exhibits high hardness (micro Vickers hardness ≥ 20 GPa) and high toughness (fracture toughness ≥ 4 MPa·m). 1 / 2 With its excellent high-temperature mechanical properties, boron carbide nanocrystalline ceramics can be widely used in aerospace, nuclear energy equipment, and high-temperature structural components. The resulting ceramics exhibit a relative density ≥97%, a micro-Vickers hardness ≥35 GPa, and a fracture toughness ≥2 MPa·m. 1 / 2 Its ultra-high hardness can effectively resist the impact of shrapnel; its density is only 2.52 g / cm³. 3 Its chemical stability is far lower than that of common metallic protective materials; at the same time, its excellent chemical stability and neutron absorption capacity endow B4C ballistic shielding components with good nuclear radiation shielding performance. These combined advantages make B4C ceramics of significant application value in extreme service environments such as aerospace, nuclear protection, and military protection.
[0034] In summary, this invention, through a dual innovative mechanism of "rapid sintering + secondary oscillation forging sintering," solves two major technical challenges in ceramic materials (especially SiC and B4C, which are representative of extremely difficult-to-sinter ceramic materials) and effectively controls stacking fault density in a relatively simple process. It achieves high densification, nanocrystalline structure, and high stacking fault density in ceramic materials, providing a simple, efficient, and low-cost new technical approach for the preparation of high-strength and tough structural ceramics. Attached Figure Description
[0035] To more clearly illustrate the technical solutions in the embodiments of the present invention, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0036] Figure 1 This is a flowchart illustrating the preparation of high-level fault density nanocrystalline ceramics according to the present invention; Figure 2 The image shows the microstructure of the ceramic obtained in Comparative Example 1. Figure 3 The statistical results of the particle size distribution of ceramics were obtained for Example 1 (Al2O3 and Y2O3 sintering aid system); Figure 4 The statistical results of the particle size distribution of ceramics were obtained for Example 2 (AlN and Y2O3 sintering aid system); Figure 5 The microstructure diagrams of the ceramics obtained in Example 1 (Al2O3 and Y2O3 sintering aid system) are shown, where (a) is the overall structure and (b) is the local structure. Figure 6 The microstructure diagrams of the ceramics obtained in Example 2 (AlN and Y2O3 sintering aid system) are shown, where (a) is the overall structure and (b) is the local structure. Figure 7 The image shows the microstructure of the boron carbide ceramic obtained in Example 4, where (a) is the overall structure and (b) is the local structure. Detailed Implementation
[0037] To make the technical problems, technical solutions and advantages of the present invention clearer, a detailed description will be given below in conjunction with the accompanying drawings and specific embodiments (the specific implementation methods are mainly illustrated by taking silicon carbide ceramics and boron carbide ceramics, which are extremely difficult to sinter, as examples).
[0038] Figure 1 This is a flowchart of a method for preparing high-density nanocrystalline ceramics according to the present invention. This method couples rapid sintering and oscillating pressure forging techniques, including: loading nano-ceramic powder into a conductive mold; applying axial static pressure to the mold through an upper pressure head in a rapid sintering device; and simultaneously generating Joule heating within the mold and sample using pulsed current, rapidly heating the sample to a predetermined temperature and holding it at that temperature for a certain time. During this process, under the synergistic drive of thermal activation and static pressure, the nanoparticles form neck connections in the particle contact area through mass migration mechanisms such as surface diffusion and grain boundary diffusion, achieving preliminary densification and obtaining a pre-sintered ceramic with a certain strength. At this stage, the deformation of the ceramic is mainly unidirectional compression; the powder particles undergo rearrangement and plastic deformation under axial pressure, resulting in a significant reduction in porosity.
[0039] The pre-sintered ceramic is then removed from the original mold and placed into a larger conductive mold, allowing for lateral deformation within the mold. In the rapid sintering equipment, pulsed current heating continues to raise the sample to the sintering temperature, while axial oscillating pressure is applied to the mold via an oscillating pressure system. Unlike static pressure, the oscillating pressure varies periodically within a set range, subjecting the ceramic sample to repeated compression-unloading-compression cycles in the vertical direction. In the horizontal direction, due to the smaller constraint of the mold sidewalls, plastic flow and lateral expansion occur (as shown in the figure, the sample changes from rectangular to drum-shaped). This dynamic cyclic loading generates alternating shear stress within the ceramic, driving repeated movement of stacking faults and cyclic slippage of grain boundaries. On one hand, this further eliminates residual porosity and promotes densification; on the other hand, due to the low stacking fault energy of SiC, stacking faults continuously multiply and move under alternating stress, forming a large number of stacking faults within the grains. Simultaneously, the short-term high-temperature characteristics of rapid sintering effectively suppress abnormal grain growth, ultimately yielding high-performance nanocrystalline ceramics with a high stacking fault density structure.
[0040] This rapid sintering equipment utilizes an SPS (Self-Pulsed Polarizing) device. Its chamber contains upper and lower electrodes for applying pulsed direct current. The pulsed current between the electrodes generates Joule heating within the mold and sample, achieving rapid heating and sintering. A water-cooling system is included to cool the electrodes, pressure head, and chamber walls to control the thermal field distribution. A vacuum and atmosphere system is provided to evacuate gases from the chamber and provide the inert atmosphere required for sintering. Static pressure and oscillating pressure systems are also included, applying axial static pressure and oscillating pressure to the mold and sample via the upper pressure head to promote ceramic densification and the formation of a high-density, high-layer fault structure.
[0041] Example 1
[0042] The preparation of high-density SiC nanocrystalline ceramics using β-SiC nanopowder, Al2O3, and Y2O3 sintering aids includes the following steps: a) Raw material mixing Weigh β-SiC, Al2O3, and Y2O3 nanoparticles respectively, so that m β-SiC :m Al2O3 :m Y2O3 The ratio of β-SiC nanoparticles to ethanol was 90:6:4. First, β-SiC nanoparticles were prepared into a slurry with ethanol and ultrasonically dispersed in an ice-water bath for 5 min. After removal, Al2O3 and Y2O3 nanoparticles were gradually added to the β-SiC slurry under magnetic stirring. Then, the mixed slurry was placed in an ice-water bath again for ultrasonic dispersion for 5 min. After removal, the slurry was poured into a ball mill jar and wet-milled for 8 h at a speed of 400 rpm. After removal, it was dried and sieved for subsequent sintering.
[0043] b) Pre-sintering process
[0044] The mixed nanoparticles obtained in the above steps are used for pre-sintering. Here, we select 1500℃-50 MPa-5min as the pre-sintering process parameters. If the density of the pre-sintered ceramic is too low, the sample will break prematurely during the subsequent forging process, and a complete ceramic block cannot be obtained; if the density is too high, low-pressure forging cannot produce significant plastic deformation in the sample, and the performance improvement is not significant. In this process, we prefer low-pressure sintering and forging, which has natural advantages in preparing large-size samples and industrial production, greatly saving costs and reducing the need for high-pressure equipment.
[0045] c) Rapid sintering by secondary oscillation forging
[0046] The pre-sintered sample obtained in the above steps was placed in a larger sintering mold for oscillatory forging. The sintering temperature was 1700°C, the heating rate was 300°C / min, the sintering time was 360 s, the axial pressure was 50 ±25 MPa, and the oscillation frequency was 1 Hz.
[0047] The obtained samples were polished and their properties characterized. The relative density was measured to be 97.54% using the Archimedes displacement method; the microVickers hardness was 20.36 GPa; and the fracture toughness was 4.16 MPa·m. 1 / 2 .
[0048] Example 2
[0049] The preparation of high-density SiC nanocrystalline ceramics using β-SiC nanopowder, AlN, and Y2O3 sintering aids includes the following steps: a) Raw material mixing Weigh β-SiC, AlN, and Y2O3 nanoparticles separately, so that m β-SiC :m AlN :m Y2O3 The ratio of β-SiC nanoparticles to ethanol was 90:6:4. First, β-SiC nanoparticles were prepared into a slurry with ethanol and ultrasonically dispersed in an ice-water bath for 5 min. After removal, AlN and Y2O3 nanoparticles were gradually added to the β-SiC slurry under magnetic stirring. Then, the mixed slurry was placed in an ice-water bath again for ultrasonic dispersion for 5 min. After removal, the slurry was poured into a ball mill jar and wet-milled for 8 h at a speed of 400 rpm. After removal, it was dried and sieved for subsequent sintering.
[0050] b. Pre-sintering
[0051] The pre-sintering process parameters were kept consistent with those in Example 1, with sintering at 1500℃ for 5 min and an axial pressure of 50 MPa.
[0052] c) Rapid sintering by secondary oscillation forging
[0053] The pre-sintered sample obtained in the above steps is placed in a larger sintering mold for oscillatory forging. The preferred sintering temperature is 1700°C, the heating rate is 300°C / min, the sintering time is 360 s, the axial pressure is 50 ±25 MPa, and the oscillation frequency is 1 Hz.
[0054] The obtained samples were polished and their properties characterized. The relative density was measured to be 99.1% using the Archimedes displacement method; the micro Vickers hardness was 22.64 GPa; and the fracture toughness was 4.23 MPa·m. 1 / 2 .
[0055] Example 3
[0056] The preparation of high-density SiC nanocrystalline ceramics using β-SiC nanopowder, Al2O3, and Y2O3 sintering aids includes the following steps: a) Raw material mixing Weigh β-SiC, Al2O3, and Y2O3 nanoparticles respectively, so that m β-SiC :m Al2O3 :m Y2O3 The ratio of β-SiC nanoparticles to ethanol was 90:6:4. First, β-SiC nanoparticles were prepared into a slurry with ethanol and ultrasonically dispersed in an ice-water bath for 5 min. After removal, Al2O3 and Y2O3 nanoparticles were gradually added to the β-SiC slurry under magnetic stirring. Then, the mixed slurry was placed in an ice-water bath again for ultrasonic dispersion for 5 min. After removal, the slurry was poured into a ball mill jar and wet-milled for 8 h at a speed of 400 rpm. After removal, it was dried and sieved for subsequent sintering.
[0057] b. Pre-sintering
[0058] The pre-sintering was carried out at 1700℃ for 5 min, and the axial pressure used was 50MPa.
[0059] c) Rapid sintering by secondary oscillation forging
[0060] The pre-sintered sample obtained in the above steps is placed in a larger sintering mold for oscillatory forging. The preferred sintering temperature is 1500°C, the heating rate is 300°C / min, the sintering time is 360 s, the axial pressure is 50 ±25 MPa, and the oscillation frequency is 1Hz.
[0061] The obtained samples were polished and their properties characterized. The relative density was measured to be 97.56% using the Archimedes displacement method; the micro Vickers hardness was 20.62 GPa; and the fracture toughness was 4.27 MPa·m. 1 / 2 .
[0062] Example 4
[0063] The preparation of high-density B4C nanocrystalline ceramics using B4C nanopowder includes the following steps: a) Raw material preparation B4C nanoparticles were ground and sieved for subsequent sintering.
[0064] b. Pre-sintering
[0065] The pre-firing temperature is 1700℃, the pre-firing pressure is 30 MPa, the heating rate is 500 ℃ / min, and the holding time is 6 min, to ensure that a ceramic with a certain strength is obtained, laying the foundation for the subsequent secondary oscillation forging and avoiding material cracking during the subsequent secondary forging.
[0066] c) Rapid sintering by secondary oscillation forging
[0067] The pre-sintered B4C ceramic was placed in a larger mold and then placed in a rapid hot pressing sintering device. Axial oscillation pressure was applied for rapid, short-duration oscillatory forging sintering, with a median pressure of 80 MPa, an amplitude of 10-20 MPa, and an oscillation frequency of 5 Hz. The temperature was increased to 1900℃ at a rate of 500 ℃ / min, held at that temperature and oscillated for 10 min, and then cooled to obtain the material. During the forging process, because the pre-sintered sample was placed in a larger mold, it was not restricted by the mold and could freely undergo shear deformation, thereby significantly increasing the stacking fault density inside the ceramic.
[0068] The obtained samples were polished and their properties characterized. The relative density was measured to be 99.73% using the Archimedes displacement method; the micro Vickers hardness was 43.25 GPa; and the fracture toughness was 3.53 MPa·m. 1 / 2 .
[0069] Comparative Example 1
[0070] The preparation of SiC nanocrystalline ceramics using β-SiC nanopowder, Al2O3, and Y2O3 sintering aids includes the following steps: a) Raw material mixing Weigh β-SiC, Al2O3, and Y2O3 nanoparticles respectively, so that m β-SiC :m Al2O3 :m Y2O3 The ratio of β-SiC nanoparticles to ethanol was 90:6:4. First, β-SiC nanoparticles were prepared into a slurry with ethanol and ultrasonically dispersed in an ice-water bath for 5 min. After removal, Al2O3 and Y2O3 nanoparticles were gradually added to the β-SiC slurry under magnetic stirring. Then, the mixed slurry was placed in an ice-water bath again for ultrasonic dispersion for 5 min. After removal, the slurry was poured into a ball mill jar and wet-milled for 8 h at a speed of 400 rpm. After removal, it was dried and sieved for subsequent sintering.
[0071] b) Rapid sintering
[0072] Using a conventional sintering process, sintering was carried out at 1800°C for 360 s with an axial pressure of 50 MPa, ultimately yielding nanocrystalline SiC ceramics.
[0073] The obtained samples were polished and their properties characterized. The relative density was measured to be 96.63% using the Archimedes displacement method; the micro Vickers hardness was 15.32 GPa; and the fracture toughness was 4.36 MPa·m. 1 / 2 .
[0074] Comparative Example 2
[0075] The preparation of SiC nanocrystalline ceramics using β-SiC nanopowder, AlN, and Y2O3 sintering aids includes the following steps: a) Raw material mixing Weigh β-SiC, AlN, and Y2O3 nanoparticles separately, so that m β-SiC :m AlN :m Y2O3 The ratio of β-SiC nanoparticles to ethanol was 90:6:4. First, β-SiC nanoparticles were prepared into a slurry with ethanol and ultrasonically dispersed in an ice-water bath for 5 min. After removal, AlN and Y2O3 nanoparticles were gradually added to the β-SiC slurry under magnetic stirring. Then, the mixed slurry was placed in an ice-water bath again for ultrasonic dispersion for 5 min. After removal, the slurry was poured into a ball mill jar and wet-milled for 8 h at a speed of 400 rpm. After removal, it was dried and sieved for subsequent sintering.
[0076] b) Rapid sintering
[0077] Using a conventional sintering process, sintering was carried out at 1800°C for 360 s with an axial pressure of 50 MPa, ultimately yielding nanocrystalline SiC ceramics.
[0078] The obtained samples were polished and their properties characterized. The relative density was measured to be 97.54% using the Archimedes displacement method; the microVickers hardness was 16.42 GPa; and the fracture toughness was 4.36 MPa·m. 1 / 2 .
[0079] Comparative Example 3
[0080] Boron carbide ceramics were prepared by sintering nano-B4C powder under static force field conditions. B4C powder was filled into a graphite mold and sintered under vacuum conditions. The temperature was rapidly increased to 1900℃ at a rate of 500℃ / min. After holding at that temperature for 30 seconds, the pressure was rapidly increased to 100 MPa. The temperature and pressure were maintained for 10 minutes before the furnace was cooled.
[0081] The obtained sample was polished and its properties were characterized. The relative density was 98.55% using the Archimedes displacement method; the micro Vickers hardness was 37.61 GPa; and the fracture toughness was 2.67 MPa·m. 1 / 2 .
[0082] Specifically, Example 1 and Comparative Example 1 both use Al2O3 and Y2O3 additive systems, differing only in their sintering processes, allowing for comparison. Example 2 and Comparative Example 2 both use AlN and Y2O3 additive systems, differing only in their sintering processes, allowing for comparison. Example 1 and Example 3 both use Al2O3 and Y2O3 additive systems, differing only in that the former uses "low-temperature pre-firing + high-temperature forging," while the latter uses "high-temperature pre-firing + low-temperature forging," allowing for comparison. Example 4 and Comparative Example 3 both use nano-boron carbide powder, differing only in their sintering processes, allowing for comparison.
[0083] Table 1. Properties of ceramics in different ceramic systems and sintering methods
[0084] The comparison of relative density and performance in Table 1 shows that secondary oscillation forging sintering has significant advantages over conventional sintering. Specifically, comparing the data from Example 1 and Comparative Example 1 (Al2O3 and Y2O3 additive system), Example 1, using a process route of "low-temperature pre-sintering at 1500℃ + high-temperature secondary oscillation forging sintering at 1700℃," yielded nanocrystalline SiC ceramics with a relative density of 97.54% and a hardness of 20.36 GPa. In contrast, Comparative Example 1, using a higher sintering temperature (1800℃) conventional sintering process, obtained nanocrystalline SiC ceramics with a relative density of only 96.63% and a hardness of only 15.32 GPa. With almost identical fracture toughness, the material prepared by the secondary oscillation forging process exhibits significantly improved hardness and density, with a hardness improvement of up to 32.89%.
[0085] Similarly, comparing the data from Example 2 and Comparative Example 2 (AlN and Y2O3 sintering aids), it can be seen that Example 2, using a process route of "low-temperature pre-sintering at 1500℃ + high-temperature secondary oscillation forging sintering at 1700℃," obtained nanocrystalline SiC ceramics with a relative density of 99.1% and a hardness of 22.64 GPa. In contrast, Comparative Example 2, using a higher sintering temperature (1800℃) and a conventional sintering process, obtained nanocrystalline SiC ceramics with a relative density of only 97.54% and a hardness of only 16.42 GPa. With almost identical fracture toughness, the material prepared by the secondary oscillation forging process showed significantly improved hardness and density, with a 37.8% improvement in hardness performance.
[0086] In addition, both Example 1 and Example 2 adopted the process route of "low temperature pre-firing + high temperature forging", while in comparison, Example 3 adopted the process route of "1700°C high temperature pre-sintering + 1500°C low temperature secondary oscillation forging sintering", and the ceramic properties were comparable to those of Example 1.
[0087] For the boron carbide ceramic system, Comparative Example 3 used conventional sintering, while Example 4 used a process route of "high-temperature pre-sintering at 1700℃ + high-temperature secondary oscillation forging sintering at 1900℃". The resulting nanocrystalline boron carbide ceramic had a relative density of 99.73% and a hardness of 43.25 GPa. In contrast, Comparative Example 3, using the same temperature (1900℃) conventional sintering process, obtained a nanocrystalline boron carbide ceramic with a relative density of only 98.55% and a hardness of only 37.61 GPa. The material prepared by the secondary oscillation forging process showed significantly improved hardness and density.
[0088] In summary, both types of silicon carbide additive systems achieved high density (≥97%) and excellent comprehensive mechanical properties (hardness ≥20 GPa, fracture toughness ≥4 MPa·m) under the process of this invention. 1 / 2 Furthermore, the solid-state sintered boron carbide ceramics also achieved high density (≥97%) and excellent comprehensive mechanical properties (hardness ≥43 GPa, fracture toughness ≥3 MPa·m) under the process of this invention. 1 / 2 This fully demonstrates that the dual innovative mechanism of "rapid sintering + secondary oscillation forging sintering" of this invention does not depend on the type of sintering aid or the ceramic system, and has good applicability to liquid-phase sintering aids, solid-liquid-phase sintering aid combinations, and even without the addition of sintering aids. This lays a solid foundation for the application of this invention in a wider range of sintering systems.
[0089] The following test results verify that the present invention successfully achieved a nanoscale grain structure through short-time rapid sintering. Figure 3 and Figure 4 The statistical results of the particle size distribution of ceramics obtained in Example 1 (Al2O3 and Y2O3 sintering aid system) and Example 2 (AlN and Y2O3 sintering aid system) are presented respectively. It can be seen that regardless of the aid system used, the average particle size of the ceramics is less than 200 nm. According to the Hall-Petch relationship, the finer the grains, the higher the material strength. There are more grain boundaries in nanocrystals, which strongly hinder the movement of dislocations.
[0090] The following test results verify that the present invention successfully prepared SiC ceramics and B4C ceramics with high fault density through the process route of "pre-sintering + secondary oscillation forging sintering". Figure 2 The microstructure of the ceramic prepared in Comparative Example 1 is shown, which has a low stacking fault density. Figure 5 , Figure 6 and Figure 7 The microstructure diagrams of the ceramics obtained in Example 1 (Al2O3 and Y2O3 sintering aid system), Example 2 (AlN and Y2O3 sintering aid system), and Example 4 (B4C ceramics) are shown respectively. Figure 5 (a) Figure 6 (a) and Figure 7 (a) shows the overall microstructure of both systems. As can be seen, most grains exhibit stacking fault structures. Figure 5 (b) Figure 6 (b) and Figure 7 (b) shows local microstructure diagrams of both systems, indicating a high stacking fault density within the grains. In summary, the various sintering ceramic systems prepared using the process provided by this invention all exhibit a large number of stacking faults, i.e., a high-density fault structure. This achievement benefits from the dual innovative strategy of this invention: "rapid sintering + secondary oscillation forging rapid sintering." First, short-time pre-sintering at high or low temperatures is performed using rapid sintering equipment. Due to the extremely short sintering time, the grains do not have enough time to grow fully, effectively suppressing the abnormal coarsening of nanocrystals in traditional long-time sintering and stabilizing the nanocrystalline microstructure. Subsequently, a dynamic pressure field, i.e., oscillating pressure, is introduced into the secondary sintering for forging sintering. Since there is no mold restriction around the pre-sintered sample during forging, most areas of the sample will generate large shear forces, resulting in plastic deformation. While promoting densification, a large number of stacking faults are generated. The combined effect of these two factors leads to a significant improvement in ceramic performance.
[0091] In summary, this invention, through a dual innovative strategy of "rapid sintering + secondary oscillatory forging sintering," has the following significant advantages compared to conventional sintering processes: (1) Significant improvement in ceramic density and performance: In the silicon carbide system, the sintering aids are Al2O3 and Y2O3. The sample prepared by the method of this invention has a relative density of 97.54% and a hardness of 20.36 GPa, which is 32.89% higher than that of conventional sintering process (hardness 15.32 GPa). The solid-state sintered boron carbide ceramics obtained by the process of this invention have high density (≥97%) and excellent comprehensive mechanical properties (hardness ≥43 GPa, fracture toughness ≥3 MPa·m). 1 / 2 This fully demonstrates the outstanding advantages of the secondary oscillation forging rapid sintering process in promoting sintering densification and improving performance.
[0092] (2) High nanoscale stacking fault density: During the secondary oscillation forging process, large shear plastic deformation is generated, and the atomic diffusion rate is increased at high temperature, thereby forming a large number of stacking faults and microtwins, which is beneficial to improving the strength and hardness of ceramics.
[0093] (3) Stable nanocrystalline structure: The "rapid sintering + secondary oscillation forging sintering" process successfully prepared nanocrystalline SiC ceramics and nanocrystalline B4C ceramics, effectively suppressing abnormal grain growth during the sintering process and providing fine grain strengthening effect for the materials.
[0094] (4) The method has strong universality: whether it is a liquid phase sintering aid, a liquid-solid combined sintering aid system, or even a system without aids, the method of this invention can achieve high density and excellent mechanical properties of extremely difficult-to-sinter ceramics, proving the wide applicability of this method in most ceramic systems.
[0095] (5) Excellent comprehensive performance: The SiC nanocrystalline ceramics sintered with AlN and Y2O3 sintering aid system achieved a relative density of 99.1%, a hardness of 22.64 GPa, and a fracture toughness of 4.23 MPa·m. 1 / 2 The superior combination of properties, compared to SiC ceramics obtained by conventional sintering processes at higher temperatures (1800℃) (Comparative Example 2: density 97.54%, hardness 16.42 GPa, toughness 4.36 MPa·m), results in a superior product. 1 / 2 The hardness was increased by 37.8%, and the solid-state sintered boron carbide ceramic obtained by the process of this invention achieved high density (≥97%) and excellent comprehensive mechanical properties (hardness ≥43GPa, fracture toughness ≥3 MPa·m). 1 / 2 This fully demonstrates the significant advantages of the method of the present invention in the preparation of high-performance nanocrystalline ceramic materials.
[0096] The above description is merely a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention should be included within the scope of protection of the present invention. Therefore, the scope of protection of the present invention should be determined by the scope of the claims.
Claims
1. A method for preparing high-density nanocrystalline ceramics, characterized in that, Includes the following steps: a) Preparation of nanomaterials: Grind and sieve the nano-ceramic powder for subsequent sintering; if sintering aids are required, mix the sieved nano-ceramic powder and nano-sintering aids evenly to obtain a mixed powder. b) Rapid pre-sintering: The mixed powder obtained in step a) is placed in a rapid sintering equipment and rapidly pre-sintered under vacuum or argon atmosphere to obtain pre-sintered ceramics; c) Secondary oscillation forging sintering: The pre-sintered ceramic obtained in step b) is placed in a rapid sintering equipment to give the pre-sintered ceramic lateral deformation space. Axial oscillation pressure is applied during rapid sintering to forge the ceramic. After cooling, the nanocrystalline ceramic is obtained.
2. The method for preparing high-density nanocrystalline ceramics according to claim 1, characterized in that, In step a), the ceramic powder is selected from one or more of silicon carbide, boron carbide, titanium carbide, hafnium carbide, zirconium carbide, and niobium carbide, or a mixture of powders or high-entropy carbides.
3. The method for preparing high-density nanocrystalline ceramics according to claim 1, characterized in that, In step a), the sieve mesh size is 100-400 mesh. The sintering aid includes a liquid phase sintering aid and a solid phase sintering aid. The liquid phase sintering aid is selected from at least two combinations of Al2O3 and Y2O3, MgO, CaO, La2O3, CeO2, Nd2O3, Sm2O3, and Yb2O3, or AlN and one or more combinations of Y2O3, MgO, CaO, La2O3, CeO2, Nd2O3, Sm2O3, and Yb2O3. The solid phase sintering aid is selected from at least one of B4C, AlN, BN, and C.
4. The method for preparing high-density nanocrystalline ceramics according to claim 3, characterized in that, Based on a total raw material mass of 100 wt%, the amount of sintering aid added is 0-20 wt% of the total raw material mass, preferably 5-10 wt%; preferably, a combination of Al2O3 and Y2O3 is used as the aid, with a mass ratio of (5-7):(3-5), more preferably 6:
4.
5. The method for preparing high-density nanocrystalline ceramics according to claim 1, characterized in that, In step a), the mixing method is one or two of ultrasonic dispersion, wet ball milling, or dry ball milling.
6. The method for preparing high-density nanocrystalline ceramics according to claim 1, characterized in that, In step b), the pre-sintering temperature is 1200-2000℃, the pre-sintering pressure is 10-200 MPa, the heating rate is 100℃ / min-1000℃ / s, and the holding time is 1-10 min.
7. The method for preparing high-density nanocrystalline ceramics according to claim 1, characterized in that, In step c), the rapid sintering process is selected from one of spark plasma sintering (SPS), electric field assisted pressure sintering, and Joule heating.
8. The method for preparing high-density nanocrystalline ceramics according to claim 7, characterized in that, In step c), the sintering temperature is 1200-2000°C, the sintering time is 1-10 min; the forging temperature is 1200-2000°C, the forging pressure is 10-200 MPa, the amplitude is 10-100 MPa, the oscillation frequency is 0.1-100 Hz, the heating rate is 100°C / min-1000°C / s, and the holding time is 1-10 min.
9. The nanocrystalline ceramic material with high dislocation density prepared by the method according to any one of claims 1 to 8, characterized in that, This includes nanocrystalline silicon carbide ceramics and nanocrystalline boron carbide ceramics.
10. The nanocrystalline ceramic material according to claim 9, characterized in that, Nanocrystalline silicon carbide ceramics have a relative density ≥97%, a micro Vickers hardness ≥20 GPa, and a fracture toughness ≥4 MPa·m. 1 / 2 The relative density of nanocrystalline boron carbide ceramics is ≥97%, the micro Vickers hardness is ≥35 GPa, and the fracture toughness is ≥2 MPa·m. 1 / 2 .