A fluorine coating system for rotational molding and a method of applying the same
By designing a fluorinated coating system with intermediate and topcoat components, the problem of poor coating adhesion in the spin coating process was solved, resulting in a coating with high chemical resistance and high adhesion strength, suitable for corrosion protection applications in chemical, pharmaceutical and other industrial equipment.
Patent Information
- Application Number
- CN202611213750.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2025-12-18
- Filing Date
- 2026-08-11
- Publication Date
- 2026-11-10
AI Technical Summary
Existing fluorinated coatings exhibit poor adhesion in rotary coating processes, leading to easy peeling of the coating in negative pressure applications and a short lifespan.
A fluoropolymer coating system consisting of an intermediate component and a topcoat component is adopted. The intermediate component includes a curing crosslinking aid, a binder, an antioxidant, a heat stabilizer, and a surfactant. The topcoat component is a fluoropolymer coating powder. By controlling the mass ratio and particle size of each component, a three-dimensional network structure is formed to enhance adhesion.
It improves the adhesion strength and chemical resistance of the coating, extends the service life of the coating, and the coating is not easy to peel off at high temperatures. It is suitable for anti-corrosion lining of industrial equipment such as chemical and pharmaceutical products.
Smart Images

Figure CN123063012A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of fluorinated coatings, specifically relating to a fluorinated coating system for rotational molding and its application method. Background Technology
[0002] Hot-melt fluorinated powder coatings, such as modified polytetrafluoroethylene (PFA), perfluoroethylene propylene (FEP), and ethylene-tetrafluoroethylene copolymer, have excellent heat resistance, chemical resistance, weather resistance, electrical insulation, high-frequency characteristics, flame retardancy, and thermal stability. They are widely used in many fields such as chemical, mechanical, electrical, medical, food, and semiconductor industries.
[0003] Powder coating processes mainly include electrostatic spraying and fluidized bed dip coating. For internal wall anti-corrosion and wear-resistant coatings of hollow products, rotary coating is required. Rotary coating, also known as rotational molding, is a molding process in which metered fluoropolymer powder is added to a liner and rotated along two perpendicular axes while being heated. Under the influence of gravity and heat, the plastic material is gradually and evenly coated, melted, and adhered to the entire surface of the inner cavity, forming the final product after cooling.
[0004] Fluorine-containing coatings, due to the high surface energy of fluorine, have problems such as poor adhesion to substrates such as metals, glass, and ceramics, and poor resistance to stress cracking. Therefore, an intermediate layer is needed to create a transition layer between the topcoat and the substrate to enhance adhesion.
[0005] Because the spin coating process requires fluorinated coatings to have good flowability, a relatively large particle size is needed, typically 200-500 micrometers. This results in a relatively thick coating, ranging from 2mm to 8mm. When the coating thickness is high, peeling is more likely to occur during application, especially under negative pressure conditions, thus requiring stronger adhesion. Summary of the Invention
[0006] To address the problems of poor adhesion and short lifespan of existing fluorinated coatings, this invention provides a fluorinated coating system for rotational molding and its application method.
[0007] To achieve the above objectives, the present invention adopts the following technical solution: A fluoropolymer coating system for rotational molding comprises an intermediate component and a topcoat component. The intermediate component consists of a curing and crosslinking aid, a binder, an antioxidant, a heat stabilizer, a surfactant, and fluoropolymer coating powder. The topcoat component is fluoropolymer coating powder. In the fluoropolymer coating system, the mass ratio of the intermediate component to the topcoat component is 1:1-2.
[0008] The intermediate components include a main component and additives. The main component consists of fluorinated coatings and adhesives, and the additives include curing and crosslinking aids, antioxidants, heat stabilizers, and surfactants.
[0009] The main component contains 10-50 wt% binder, preferably 10-30 wt%, more preferably 20 wt%; 0.3-1 wt% curing and crosslinking aid, preferably 0.7 wt%; 0.01-0.1 wt% antioxidant, preferably 0.05 wt%; 0.1-0.5 wt% heat stabilizer, preferably 0.3 wt%; and 0.01-0.05 wt% surfactant, preferably 0.03 wt%.
[0010] Preferably, the fluorinated coating powder in the intermediate component has the same composition as the fluorinated coating powder in the topcoat component, and the fluorinated coating powder is one of modified polytetrafluoroethylene (PFA), perfluoroethylene propylene (FEP), or ethylene-tetrafluoroethylene copolymer (ETFE) powder. The pure fluorinated coating powder in the intermediate component needs to be consistent with the composition of the topcoat fluorinated coating to achieve application matching and enhance adhesion.
[0011] Preferably, the fluoropolymer coating powder has high thermal stability and chemical resistance, and a particle size of 150-500 μm. The relatively high particle size gives the fluoropolymer coating good flowability and makes it easy to level during processing.
[0012] Preferably, the binder in the intermediate component is composed of nitrogen-containing binders, such as PAI (polyamide-imide) or PI (polyimide) powder, with a particle size of 0.5-20.5 micrometers. The presence of nitrogen in PAI or PI can effectively form hydrogen bonds with the substrate surface, enhancing adhesion strength. Furthermore, PAI or PI has high thermal stability, which allows it to enhance adhesion without degrading at the high processing temperatures of fluoropolymer coatings. Excessive PAI or PI content can lead to thermal stability issues with the main material, while insufficient content results in inadequate adhesion.
[0013] The synergistic effect of the curing crosslinking aid and the bonding aid enables the fluorinated coating to form a three-dimensional network structure, thereby improving adhesion, heat resistance, density, chemical resistance, and crack resistance. The topcoat component is a pure fluorinated coating, effectively resisting the corrosive effects of chemical media. The coating system, composed of intermediate and topcoat components, can be applied to various industrial chemical-resistant and corrosion-resistant lining equipment in chemical, pharmaceutical, and pesticide industries.
[0014] Preferably, the curing and crosslinking aid in the intermediate component is triallyl isocyanurate (TAIC), which not only plays a three-dimensional network crosslinking role, but also forms a matched melt-mixed structure with nitrogen-containing adhesives, further enhancing the adhesion.
[0015] Preferably, the antioxidant in the intermediate component is composed of aromatic amines, such as dinaphthylamine. Fluoropolymer coatings are processed at high temperatures and require long sintering times, which easily leads to degradation of the polymer components. Therefore, adding antioxidants can help the polymer melt while maintaining high thermal stability. Low antioxidant content is ineffective, while excessive content will generate bubbles.
[0016] Preferably, the heat stabilizer in the intermediate component is composed of metal oxide additives such as zinc oxide, aluminum oxide, copper oxide, tin oxide, chromium trioxide, and antimony trioxide (Sb₂O₃). These metal oxide additives absorb the HF generated during thermal degradation and act as heat stabilizers during the melting process of the PFA coating, slowing down or preventing the rapid degradation of the molecular chains.
[0017] Preferably, the surfactant in the intermediate component is a nonionic surfactant: Triton X-100 (octylphenol polyoxyethylene ether). Nonionic surfactants can help disperse various added inorganic additives in organic polymers and prevent mixing and agglomeration.
[0018] Preferably, the method for preparing the intermediate component includes the following steps: (1) First, mix the various additives according to the mass ratio, and then dilute them in the aqueous phase to prepare the additive mixture; (2) Blend the main components according to their mass ratio; (3) Using spray drying, the auxiliary agent mixture is added to the main component mixture and dried into powder to obtain the intermediate component.
[0019] This invention also provides a method for applying the above-mentioned fluorine coating system, comprising the following steps: (1) Roughen the inner surface of the pre-constructed equipment workpiece and clean it by blowing; (2) Seal off all inlets and outlets of the equipment workpiece, leaving only one feeding port, and then perform tooling welding to fix the workpiece on the three-dimensional rotating platform of the sintering furnace. (3) Calculate the amount of intermediate component and topcoat component to be fed based on the melt density of fluorine coating, the surface area of the inner wall of the equipment workpiece, and the coating thickness; (4) Start the three-dimensional rotation and heat the sintering furnace to the preset temperature. After the temperature is balanced, put the intermediate component into the feeding port. After sintering for a period of time, put the top coating component into the furnace and keep it at the preset temperature for a specified time. (5) Turn off the heating and slowly cool down. When the temperature of the sintering furnace drops below 100°C, turn off the rotation. When the entire workpiece cools down to room temperature, disassemble the tooling and remove the workpiece from the equipment. (6) The workpiece is smoothed and polished to obtain a smooth and flat equipment lining.
[0020] Defect detection is performed using a thickness gauge and a high-voltage electrostatic spark leak detector. The overall coating should meet the requirements of good leveling, uniform thickness, smoothness without bubbles, and no obvious defects.
[0021] The preset temperature in step (4) is related to the type of fluoropolymer coating. For ETFE, it is approximately 300℃; for PFA, it is approximately 380℃; and for FEP, it is approximately 370℃. The sintering time and holding time are 30-120 minutes, and the sintering time is adjusted according to the amount of material fed. The sintering thickness of the topcoat component is generally 3-8 mm. The sintering thickness of the intermediate component is 1.5-4 mm.
[0022] The beneficial effects of this invention are: This invention provides a fluoropolymer coating system for equipment corrosion protection lining that has high chemical resistance and strong adhesion to the substrate. When applied, it can simultaneously provide resistance to chemical media and resistance to peeling, thereby improving the lifespan of the equipment corrosion protection coating.
[0023] This invention introduces triallyl isocyanurate (TAIC), forming a three-dimensional network structure with stronger adhesion. It can also form a compatible melt-mixed structure with nitrogen-containing adhesives, further enhancing adhesion.
[0024] The fluoropolymer coating system provided by this invention can be applied to rotational molding. Through the combination of specific composition and particle size, the binder and fluoropolymer coating have a certain phase separation during the rotational coating process, forming a transition layer, which improves the adhesion and service life of the coating. Attached Figure Description
[0025] Figure 1 This is a schematic diagram of the structure of a three-dimensional rotary sintering furnace.
[0026] Figure 2 It is a fluorine coating powder for surface coating.
[0027] Figure 3 It is an intermediate component powder. Detailed Implementation
[0028] Example The fluorinated coating powder PFA powder used in this embodiment of the invention has a melt index of 10-30 g / 10 min and an average particle size D50 of 200 μm, and is produced by Shandong Dongyue Future Hydrogen Energy Materials Co., Ltd. Other materials such as triallyl isocyanate (TAIC), polyimide (PI, average particle size 5-30 μm), dinaphthylamine, antimony trioxide, and Triton X-100 are also commercially available products.
[0029] A schematic diagram of the three-dimensional rotary sintering furnace used in this embodiment is shown below. Figure 1 As shown, this equipment has: The sintering furnace is equipped with a three-dimensional rotating platform and its related components; The controllable sintering temperature range can reach the specified temperature from room temperature, with uniform temperature control and a set temperature fluctuation of no more than 10℃. It is equipped with a gas or electric heating system and a circulating air system; Equipped with an exhaust gas absorption device to meet the requirements for safety and environmental protection regarding the toxicity of gases released at high temperatures.
[0030] Preparation process of intermediate components: (1) First, mix triallyl isocyanate (TAIC), dinaphthylamine, antimony trioxide and Triton X-100 in proportion, and then dilute them in the aqueous phase to prepare an auxiliary agent mixture; the content of auxiliary agent in the auxiliary agent mixture is 10wt%.
[0031] (2) Apply fluoropolymer coating powder (PFA powder, such as topcoat fluoropolymer coating powder) to the surface. Figure 2 (as shown) and PI powder were physically mixed together at room temperature using a three-dimensional mixer in a certain proportion; (3) Using spray drying, the additive mixture is added to the polymer mixture and dried into powder at 120°C. Finally, the water content is controlled to be less than 0.3wt% to obtain intermediate component powder.
[0032] Following the above preparation process, the content of each component was adjusted as shown in Table 1 to obtain the intermediate components of Examples 1-6. The actual powder image of the intermediate component obtained in Example 3 is shown below. Figure 3 As shown.
[0033] Table 1. Composition of intermediate component powders obtained in Examples 1-6
[0034] Note: The intermediate components are mainly composed of PFA powder and PI, and the content of other functional additives is a percentage of the total content of PFA and PI.
[0035] The intermediate components of Examples 1-6 were subjected to performance tests, and the test methods are as follows: The intermediate powder was prepared into a plate with a thickness of 2 mm and a length and width of 100 mm using a flat vulcanizing machine, and then cut into strips with a width of 20 mm and a length of 100 mm for testing.
[0036] Media permeability test: After soaking the sample in 35wt% hydrochloric acid at room temperature for 7 days, its mechanical strength loss, color and foaming changes were evaluated.
[0037] High-temperature stability test: After sintering the sample at 260℃ for 4 hours, its embrittlement degree was evaluated.
[0038] Adhesion test: The substrate is carbon steel, smooth and un-sandblasted, with the surface sanded. The sample is placed on the substrate and sintered at 380℃ until it melts and bonds, thus forming the coating. The test is performed using the 90° peel method.
[0039] The test results are summarized in Table 2.
[0040] Table 2 Performance testing methods for intermediate components obtained in Examples 1-6 .
[0041] Example 7 The intermediate component and the corresponding topcoat powder of Example 3 were used Figure 1 The three-dimensional rotary sintering furnace shown is used for roll coating, which includes the following steps: (1) Roughen the inner surface of the pre-constructed equipment workpiece (roughness Ra=4μm) and clean it; (2) Seal off all inlets and outlets of the equipment workpiece, leaving only one feeding port, and then perform tooling welding to fix the workpiece on the three-dimensional rotating platform of the sintering furnace. (3) Calculate the amount of intermediate component and topcoat component to be fed based on the melt density of fluorine coating, the surface area of the inner wall of the equipment workpiece and the coating thickness; the amount of intermediate component to be fed is 6 kg / m²; the amount of topcoat component to be fed is 6 kg / m².
[0042] (4) Start the three-dimensional rotation and heat the sintering furnace to the preset temperature of 380-400℃. After the temperature is balanced, add the intermediate component from the feeding port. After sintering for 50 minutes, add the top coating component and keep it at the preset temperature for 40 minutes. (5) Turn off the heating and slowly cool down. When the temperature of the sintering furnace drops below 100°C, turn off the rotation. When the entire workpiece cools down to room temperature, disassemble the tooling and remove the workpiece from the equipment. (6) The workpiece is smoothed and polished to obtain a smooth and flat equipment lining.
[0043] Defect detection was performed using a thickness gauge and a high-voltage electrostatic spark leak detector. The overall coating showed good leveling properties, uniform thickness, smoothness, and no bubbles or obvious defects. The sintered thickness of the topcoat component was 6 mm. The coating's 90° adhesion strength was measured to be over 30 N / cm.
Claims
1. A fluoropolymer coating system for rotational molding, characterized in that, It consists of an intermediate component and a topcoat component. The intermediate component is composed of a curing and crosslinking aid, a binder, an antioxidant, a heat stabilizer, a surfactant, and fluorinated coating powder. The topcoat component is fluorinated coating powder.
2. The fluoropolymer coating system for rotational molding according to claim 1, characterized in that, The intermediate components include a main component and additives. The main component consists of a fluorinated coating and a binder. The additives include a curing and crosslinking aid, an antioxidant, a heat stabilizer, and a surfactant. The binder content in the main component is 10-50 wt%, preferably 10-30 wt%, more preferably 20 wt%. The curing and crosslinking aid accounts for 0.3-1 wt% of the main component's mass, preferably 0.7 wt%. The antioxidant accounts for 0.01-0.1 wt% of the main component's mass, preferably 0.05 wt%. The heat stabilizer accounts for 0.1-0.5 wt% of the main component's mass, preferably 0.3 wt%. The surfactant accounts for 0.01-0.05 wt% of the main component's mass, preferably 0.03 wt%.
3. The fluoropolymer coating system for rotational molding according to claim 1, characterized in that, The fluorinated coating powder in the intermediate component has the same composition as the fluorinated coating powder in the topcoat component, and the fluorinated coating powder is one of modified polytetrafluoroethylene, perfluoroethylene propylene, or ethylene-tetrafluoroethylene copolymer powder.
4. The fluoropolymer coating system for rotational molding according to claim 1, characterized in that, The particle size of the fluoropolymer coating powder is 150-500 μm.
5. The fluoropolymer coating system for rotational molding according to claim 1, characterized in that, The binder in the intermediate component is an nitrogen-containing binder with a particle size of 0.5-20.5 μm. Preferably, the binder is polyamide-imide or polyimide.
6. The fluoropolymer coating system for rotational molding according to claim 1, characterized in that, The curing and crosslinking aid in the intermediate component is triallyl isocyanurate.
7. The fluoropolymer coating system for rotational molding according to claim 1, characterized in that, The antioxidant in the intermediate component is an aromatic amine, preferably dinaphthylamine.
8. The fluoropolymer coating system for rotational molding according to claim 1, characterized in that, The heat stabilizer in the intermediate component is one or more of zinc oxide, aluminum oxide, copper oxide, tin oxide, chromium trioxide, and antimony trioxide. Preferably, the surfactant in the intermediate component is a nonionic surfactant, and more preferably octylphenol polyoxyethylene ether.
9. The fluorine coating system according to any one of claims 1-8, characterized in that, The preparation method of the intermediate component includes the following steps: (1) First, mix the various additives according to the mass ratio, and then dilute them in the aqueous phase to prepare the additive mixture; (2) Blend the main components according to their mass ratio; (3) Using spray drying, the auxiliary agent mixture is added to the main component mixture and dried into powder to obtain the intermediate component.
10. The method of applying the fluoropolymer coating system according to any one of claims 1-8, characterized in that, Includes the following steps: (1) Roughen the inner surface of the pre-constructed equipment workpiece and clean it by blowing; (2) Seal off all inlets and outlets of the equipment workpiece, leaving only one feeding port, and then perform tooling welding to fix the workpiece on the three-dimensional rotating platform of the sintering furnace. (3) Calculate the amount of intermediate component and topcoat component to be fed based on the melt density of fluorine coating, the surface area of the inner wall of the equipment workpiece, and the coating thickness; (4) Start the three-dimensional rotation and heat the sintering furnace to the preset temperature. After the temperature is balanced, put the intermediate component into the feeding port. After sintering for a period of time, put the top coating component into the furnace and keep it at the preset temperature for a specified time. (5) Turn off the heating and slowly cool down. When the temperature of the sintering furnace drops below 100°C, turn off the rotation. When the entire workpiece cools down to room temperature, disassemble the tooling and remove the workpiece from the equipment. (6) The workpiece is smoothed and polished to obtain a smooth and flat equipment lining.