A modified water-based pencil paint, a pencil with a 3D textured surface, and a rolling molding method thereof.
By combining modified water-based pencil paint with transparent polyethylene film, the problems of cracking and adhesion to molds during the hot pressing process of water-based pencil paint are solved, achieving clear and deep 3D textures and a good tactile feel.
Patent Information
- Application Number
- CN202611444608.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-17
- Publication Date
- 2026-11-10
AI Technical Summary
In existing technologies, water-based pencil paint is prone to cracking and sticking to the mold during high-temperature hot pressing, and it is difficult to achieve clear and appropriately deep 3D textures.
Modified water-based pencil paint, containing a specific ratio of plasticizer and water-based base paint, is combined with a transparent polyethylene film as an isolation medium and hot-pressed to ensure the flexibility and anti-adhesion of the paint film.
It improves the flexibility of the paint film, avoids cracking and sticking to the mold, forms a clear and deep 3D texture, and enhances the anti-slip feel and visual effect of the product.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] This application belongs to the field of stationery manufacturing technology, and relates to a modified water-based pencil paint, a pencil with a 3D textured surface, and a rolling molding method thereof. Background Technology
[0002] In the stationery manufacturing industry, the surface decoration of pencil barrels is mostly limited to flat printing, hot stamping, or glossy coating. In recent years, with the increasing demand from consumers for personalized and high-quality writing instruments, pencil products with 3D grids or raised textures have begun to appear on the market. These products aim to enhance the three-dimensional visual effect, grip feel, and anti-slip performance of the pencil barrel through embossed textures.
[0003] However, the main technical challenges currently facing the creation of 3D textures on the surface of wooden pen barrels are as follows: (1) Problems with paint film cracking and peeling. After the conventional water-based pencil paint is fully dried and cross-linked, the paint film has high hardness but insufficient flexibility. When a high-temperature hot press roller is used to apply mechanical extrusion to the surface of the pen barrel to form a 3D texture, the paint film is very prone to micro-cracks due to stress concentration, and may even peel off the entire piece from the wooden pen barrel, seriously affecting the appearance and durability of the product.
[0004] (2) Hot pressing paint adhesion and mold contamination problems. During the hot pressing process, the roller mold is in direct contact with the paint surface at high temperature. The softened water-based pencil paint is very easy to adhere to the surface of the roller mold. This not only causes the paint surface of the pen barrel to become rough, lose its gloss, and become blurred after embossing, but also the adhered residual paint will quickly contaminate the mold, forcing the production line to stop frequently for cleaning, making it impossible to carry out continuous industrial mass production.
[0005] (3) The contradiction between texture depth and clarity. If the paint film thickness on the pen barrel surface is insufficient or the design of the texture of the roller mold is inappropriate, the paint film material cannot fully fill the texture cavity when extruded, resulting in insufficient 3D relief depth and weak three-dimensionality. If the texture lines of the roller mold are too fine, it will easily cause the paint film to crack. If the lines are too thick, the imprint will not be obvious, making it difficult to balance texture clarity and paint film integrity.
[0006] Therefore, there is an urgent need to develop a modified water-based pencil paint and roll forming method that can avoid hot pressing cracking, adhere to the mold, and achieve clear 3D texture on the pencil barrel surface. Summary of the Invention
[0007] To address the shortcomings of existing technologies, the purpose of this application is to provide a modified water-based pencil paint, a pencil with a 3D textured surface, and a rolling molding method thereof. By using the modified water-based pencil paint in conjunction with a specific hot pressing molding method, it is possible to ensure that the paint film is flexible and does not crack, and that the pencil does not stick to the mold during the hot pressing process, enabling continuous industrial production. At the same time, it ensures that the embossing on the pencil barrel surface is clear, the depth is moderate, and the visual and tactile effects are excellent.
[0008] To achieve this objective, the present application adopts the following technical solution: In a first aspect, this application provides a modified water-based pencil paint, which comprises the following components by weight: 70-85 parts by weight of water-based base paint; Plasticizer 2-4 parts by weight; Other additives: 10-25 parts by weight; The water-based base paint includes water-based acrylic emulsions and / or water-based polyurethane emulsions.
[0009] The modified water-based pencil paint provided in this application is based on water-based base paint with the addition of a specific proportion of plasticizer. The plasticizer molecules can fully insert between the polymer chains of the water-based base paint, weaken the interaction force between the resin chains, significantly reduce the glass transition temperature of the resulting modified water-based pencil paint after film formation, improve the plastic deformation ability of the paint film, and significantly improve the flexibility and thermoplastic elongation of the paint film after drying. This ensures that the paint film remains continuous and intact even when deeply recessed during high-temperature and high-pressure rolling.
[0010] The water-based base paint has a weight ratio of 70 to 85 parts, for example, 72 parts, 74 parts, 76 parts, 78 parts, 80 parts, 82 parts, or 84 parts.
[0011] The plasticizer is present in parts by weight of 2 to 4 parts by weight, for example, 2.2 parts by weight, 2.5 parts by weight, 2.8 parts by weight, 3 parts by weight, 3.3 parts by weight, 3.6 parts by weight, or 3.8 parts by weight.
[0012] The other additives are present in parts by weight of 10 to 25, for example, 12, 15, 18, 20, 22 or 24 parts by weight.
[0013] In some specific embodiments, the solid content of the aqueous acrylic emulsion is 20-40%, such as 22%, 24%, 26%, 28%, 30%, 32%, 34%, 36%, 38%, or 40%.
[0014] In this application, the aqueous acrylic emulsion can be derived from commercially available products or can be prepared in-house, and the preparation method is not particularly limited.
[0015] In some specific embodiments, the solid content of the aqueous polyurethane emulsion is 20-40%, such as 22%, 24%, 26%, 28%, 30%, 32%, 34%, 36%, 38%, or 40%.
[0016] In this application, the aqueous polyurethane emulsion can be derived from commercially available products or can be prepared in-house, and the preparation method is not particularly limited.
[0017] In some specific embodiments, the plasticizer includes triethyl citrate and / or dibutyl phthalate.
[0018] In some specific embodiments, the other additives include any one or a combination of at least two of colorants, film-forming aids, defoamers, or leveling agents.
[0019] In some specific embodiments, the content of colorant, film-forming aid, defoamer and leveling agent in the modified water-based pencil paint is independently 0.1 to 10 parts by weight, for example, 0.5 parts by weight, 1 part by weight, 2 parts by weight, 4 parts by weight, 6 parts by weight, 8 parts by weight or 10 parts by weight, etc.
[0020] In this application, the colorant is an aqueous colorant, selectable from one or more of aqueous pigment pastes, aqueous color pigments, and aqueous dispersions of pigment powders; wherein the aqueous pigment paste includes aqueous red pigment paste, aqueous titanium white pigment paste, aqueous carbon black pigment paste, aqueous iron oxide yellow pigment paste, aqueous phthalocyanine blue pigment paste, etc. Exemplarily, the coloring substance of the aqueous red pigment paste can be selected from iron oxide red, quinacridone red, azo red, diketopyrrolopyrrole red, etc. The coloring substance of the aqueous titanium white pigment paste can be selected from rutile titanium dioxide, anatase titanium dioxide, etc. The coloring substance of the aqueous carbon black pigment paste can be selected from high-pigment carbon black, medium-pigment carbon black, low-pigment carbon black, iron oxide black, etc. The coloring substance of the aqueous iron oxide yellow pigment paste can be selected from synthetic α-iron oxide yellow, natural iron oxide yellow, etc. The coloring substance of the aqueous phthalocyanine blue pigment paste can be selected from β-phthalocyanine blue, α-phthalocyanine blue, ε-phthalocyanine blue, etc.
[0021] In this application, the film-forming aid may be selected from one or more of the following: dodecyl alcohol ester, dipropylene glycol butyl ether, dipropylene glycol methyl ether, and propylene glycol phenyl ether.
[0022] In this application, the defoamer may be selected from one or more of mineral oil defoamers, silicone defoamers, polyether-modified silicone defoamers, and nonionic defoamers.
[0023] In this application, the leveling agent may be selected from one or more of the following: silicone leveling agents (such as polyether-modified polysiloxane), acrylic leveling agents, fluorinated acrylate leveling agents, etc.
[0024] Secondly, this application provides a method for preparing modified water-based pencil paint as described in the first aspect, the method comprising: mixing water-based base paint and other additives, and then adding a plasticizer and mixing to obtain the modified water-based pencil paint.
[0025] Thirdly, this application provides a method for rolling a pencil with a 3D textured surface, the rolling method comprising the following steps: (1) The modified water-based pencil paint as described in the first aspect is applied to the surface of a planed wooden pencil shaft, and after drying, a pencil shaft with a dry paint film layer is obtained. (2) Print graphic markings on the surface of the pen barrel with the dry paint film layer obtained in step (1) to form a planar graphic layer; (3) The pen barrel after printing the graphic logo in step (2) is sent into the hot press roller printing machine. A layer of transparent polyethylene film is inserted between the roller of the hot press roller printing machine and the pen barrel. The transparent polyethylene film is flatly covered on the dry paint film layer of the pen barrel. The roller rolls the pen barrel under heating and pressure, so that the dry paint film layer on the surface of the pen barrel is deformed to form a 3D texture pattern corresponding to the 3D texture on the surface of the roller. (4) Remove the pencil barrel after rolling in step (3) from the hot pressing area, and cut and sharpen it in sequence to obtain a pencil with a 3D texture on the surface, thus completing the rolling forming method.
[0026] The rolling molding method for a pencil with a 3D textured surface provided in this application first coats the modified water-based pencil paint described in the first aspect onto the surface of the wooden pencil shaft. After drying, a pencil shaft with a dry paint film layer is obtained. The modified water-based pencil paint described in the first aspect of this application can impart excellent thermoplastic deformation ability and crack resistance to the dry paint film layer. Then, graphic markings are printed on the surface of the pencil shaft with the dry paint film layer obtained in step (1) to form a planar graphic layer. The pencil shaft printed in step (2) is then sent into a hot press roller printing machine. A layer of transparent polyethylene film is inserted between the roller and the pencil shaft for physical isolation. The polyethylene film can cover the paint surface of the pencil shaft smoothly. The roller rolls the pencil shaft under heating and pressure, so that the dry paint film on the surface of the pencil shaft is removed. The paint film layer deforms to form a 3D texture pattern corresponding to the 3D texture on the roller surface. In this process, the transparent polyethylene film acts as a key isolation and polishing medium. On the one hand, it prevents the softened water-based base paint from directly contacting the high-temperature metal roller, thus eliminating the phenomenon of paint sticking. On the other hand, the smooth surface of the polyethylene film plays a "pressing / polishing" role on the paint surface during hot pressing, making the edge of the embossed grid extremely smooth and dense, while achieving the dual effects of "anti-sticking demolding" and "hot pressing polishing of the paint surface". Finally, the pen barrel after step (3) is removed from the hot pressing area and cut and sharpened in sequence to complete the rolling forming of the 3D texture on the surface of the pen barrel. The 3D texture of the pen barrel paint surface after being removed from the hot pressing area is clear and deep and has no micro-cracks.
[0027] In some specific embodiments, the thickness of the dry paint film layer in step (1) is 45~60 μm, for example, it can be 46μm, 48 μm, 50 μm, 52 μm, 54 μm, 56 μm or 58 μm, etc.
[0028] In this application, the thickness of the dry paint film layer in step (1) is 45~60 μm, which is thicker than the conventional paint film thickness (25~35 μm), thus providing sufficient extrusion deformation for subsequent hot pressing, making the embossing deeper and sharper; in order to achieve this thicker dry paint film layer, 1~2 coating processes can be added in the coating process, and the coating method can be dip coating or spray coating.
[0029] In some specific embodiments, the printing of graphic markings in step (2) is performed on a screen printing machine or a pad printing machine.
[0030] In this application, the graphic and textual identifiers mentioned in step (2) include, but are not limited to, brand logos, barcodes, etc., and can be adjusted according to customer needs.
[0031] In some specific embodiments, the surface of the roller in step (3) is engraved with a diamond-shaped grid pattern.
[0032] In this application, the roller in step (3) is the core component of the hot press roller printing machine. The roller is preferably a metal roller with a heating rod inside, which can strictly control the heating temperature.
[0033] In some specific embodiments, the width of the raised lines in the 3D texture of the roller surface in step (3) is 0.5~0.8 mm, for example, it can be 0.55 mm, 0.6 mm, 0.65 mm or 0.75 mm, etc.
[0034] In some specific embodiments, the recessed gap between the lines in the 3D texture of the roller surface in step (3) is 0.5~0.8 mm, for example, it can be 0.55 mm, 0.6 mm, 0.65 mm or 0.75 mm, etc.
[0035] As a preferred technical solution of this application, the thickness of the dry paint film layer in step (1) is limited to 45~60 μm, and the width of the raised lines in the 3D texture of the roller surface and the gap between the recesses in the 3D texture of the roller surface are limited to 0.5~0.8 mm, so as to achieve a deep and sharp 3D texture (such as rhombus / honeycomb) embossing, which greatly improves the anti-slip feel and texture of the product.
[0036] In some specific embodiments, the thickness of the polyethylene film in step (3) is 0.02~0.04 mm, for example, it can be 0.022 mm, 0.025 mm, 0.028 mm, 0.032 mm, 0.035 mm or 0.038 mm, etc.
[0037] In some specific embodiments, the heating temperature in step (3) is 110~130℃, for example, it can be 112℃, 115℃, 118℃, 122℃, 125℃ or 128℃, etc.
[0038] In some specific embodiments, the pressure applied in step (3) is 0.3~0.5 MPa, for example, it can be 0.32 MPa, 0.35 MPa, 0.38 MPa, 0.42 MPa, 0.45 MPa or 0.48 MPa, etc.
[0039] Thirdly, this application provides a pencil with a 3D textured surface, the pencil being manufactured using the rolling forming method described in the second aspect.
[0040] Compared with the prior art, this application has the following advantages: (1) Flexible and crack-free paint film: By compounding a specific proportion of plasticizer in water-based base paint, the glass transition temperature of the paint film is significantly reduced, the plastic deformation capacity of the paint film is improved, and the paint film remains continuous and intact when hot-pressed deep indentation is ensured. (2) The paint film surface is smooth, and it is easy to demold during hot pressing without residual paint pollution: During the hot pressing process, a transparent polyethylene film is introduced between the roller mold and the paint surface of the pen barrel as a heat medium barrier layer. This not only completely eliminates the phenomenon of paint sticking, but also uses the flat surface of the polyethylene film to play a "polishing" effect on the paint surface during hot pressing, making the edge of the grid after embossing extremely smooth and dense. (3) Clear and three-dimensional embossing: By matching the high-thickness paint film coating with the specific mold line gap, a deep and sharp 3D grid (such as rhombus / honeycomb) embossing is achieved, which greatly improves the anti-slip feel and texture of the product. Detailed Implementation
[0041] The technical solution of this application will be further described below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely to help understand this application and should not be regarded as specific limitations on this application.
[0042] The detailed information of some of the raw materials involved in the following specific implementation method is shown below: (1) Waterborne acrylic emulsion: solid content is 30%, from Qingdao Jintaibang, brand name is 03438; (2) Water-based red pigment paste: from Suzhou Shiming Technology, brand name SIP3071; (3) Film-forming aid: from Shanghai Tikem, brand name 34590-94-8; (4) Leveling agent: from Shanghai Snow, brand name SN-7020; (5) Transparent polyethylene film: from Qingdao Jintaibang, brand name 03473.
[0043] Examples 1-4 and Comparative Examples 1-2 Examples 1-4 and Comparative Examples 1-2 each provide a modified water-based pencil paint, the components of which are shown in Table 1. In Table 1, the amount of each component is in "parts by weight". Table 1 The preparation methods of the modified water-based pencil paint provided in Examples 1-4 and Comparative Examples 1-2 include: firstly, weighing water-based base paint, adding water-based colorant, film-forming aid and leveling agent and mixing them, then slowly adding plasticizer to the system, and stirring at 800 rpm for 20 min using a disperser to obtain the modified water-based pencil paint.
[0044] Application Example 1 A method for rolling a 3D textured pencil surface includes the following steps: (1) The modified water-based pencil paint provided in Example 1 was sprayed onto the surface of the planed wooden pencil shaft. After the paint was applied, the pencil shaft was dried completely in the drying tunnel so that the average thickness of the dry paint film on the surface of the pencil shaft reached 50 μm, thus obtaining a pencil shaft with a dry paint film layer. (2) The pen barrel with dry paint film layer obtained in step (1) is put into the pad printing machine as needed to complete the graphic printing operation of the brand logo and barcode, etc., to form a flat graphic layer; (3) The pen barrel printed in step (2) is sent into a hot press roller printing machine. The core component of the hot press roller printing machine is a metal engraving roller with a heating rod inside. The surface of the metal engraving roller is engraved with a diamond grid pattern, wherein the width of the raised lines and the gap between the lines are both 0.65 mm. As the pen barrel enters the roller imprinting area, a roll of transparent polyethylene film with a thickness of 0.03 mm is simultaneously fed by the film supply machine. The transparent polyethylene film is flatly covered on the red paint surface of the pen barrel, between the roller and the pen barrel. The heating temperature of the roller is set to 120°C, and the roller applies a mechanical pressure of 0.4 MPa to roll over the pen barrel, causing the dry paint film layer on the surface of the pen barrel to soften instantly and undergo plastic flow, and to sink inward along with the underlying wood fibers to form a clear diamond grid. (4) Remove the pen barrel after pressing in step (3) from the hot pressing area. The transparent polyethylene film is rolled up by the film winding machine (the transparent polyethylene film can be reused or continuously tensioned and rolled up). The paint surface of the pen barrel after leaving the hot pressing area is dense and bright red, with clear and deep diamond patterns and no micro-cracks. Then, the pen barrel enters the cutting machine for flat cutting at both ends and enters the sharpening machine for sharpening the lead core. Finally, after passing the inspection, it is packaged and put into storage.
[0045] Application Example 2 A method for rolling a 3D textured pencil surface includes the following steps: (1) The modified water-based pencil paint provided in Example 2 was sprayed onto the surface of the planed wooden pencil shaft. After the coating was completed, the pencil shaft was completely dried in the drying tunnel so that the average thickness of the dry paint film on the surface of the pencil shaft reached 45 μm, thus obtaining a pencil shaft with a dry paint film layer. (2) The pen barrel with dry paint film layer obtained in step (1) is put into the pad printing machine as needed to complete the graphic printing operation of the brand logo and barcode, etc., to form a flat graphic layer; (3) The pen barrel printed in step (2) is sent into a hot press roller printing machine. The core component of the hot press roller printing machine is a metal engraving roller with a heating rod inside. The surface of the metal engraving roller is engraved with a reverse diamond grid pattern, wherein the width of the raised lines and the gap between the lines are both 0.8 mm. As the pen barrel enters the roller imprinting area, a roll of transparent polyethylene film with a thickness of 0.03 mm is simultaneously fed by the film supply machine. The transparent polyethylene film is flatly covered on the red paint surface of the pen barrel, between the roller and the pen barrel. The heating temperature of the roller is set to 110°C, and the roller applies a mechanical pressure of 0.5 MPa to roll over the pen barrel, causing the dry paint film layer on the surface of the pen barrel to soften instantly and undergo plastic flow, and sink inward along with the underlying wood fibers to form a clear diamond grid. (4) Remove the pen barrel after pressing in step (3) from the hot pressing area. The transparent polyethylene film is rolled up by the film winding machine (the transparent polyethylene film can be reused or continuously tensioned and rolled up). The paint surface of the pen barrel after leaving the hot pressing area is dense and bright red, with clear and deep diamond patterns and no micro-cracks. Then, the pen barrel enters the cutting machine for flat cutting at both ends and enters the sharpening machine for sharpening the lead core. Finally, after passing the inspection, it is packaged and put into storage.
[0046] Application Example 3 A method for rolling a 3D textured pencil surface includes the following steps: (1) The modified water-based pencil paint provided in Example 3 was sprayed onto the surface of the planed wooden pencil shaft. After coating, the pencil shaft was completely dried in the drying tunnel so that the average thickness of the dry paint film on the surface of the pencil shaft reached 55 μm, thus obtaining a pencil shaft with a dry paint film layer. (2) The pen barrel with dry paint film layer obtained in step (1) is put into the pad printing machine as needed to complete the graphic printing operation of the brand logo and barcode, etc., to form a flat graphic layer; (3) The pen barrel printed in step (2) is sent into a hot press roller printing machine. The core component of the hot press roller printing machine is a metal engraving roller with a heating rod inside. The surface of the metal engraving roller is engraved with reverse diamond grid patterns, wherein the width of the raised lines and the gap between the lines are both 0.5 mm. As the pen barrel enters the roller imprinting area, a roll of transparent polyethylene film with a thickness of 0.03 mm is simultaneously fed by the film supply machine. The transparent polyethylene film is flatly covered on the red paint surface of the pen barrel, between the roller and the pen barrel. The heating temperature of the roller is set to 130°C, and the roller applies a mechanical pressure of 0.3 MPa to roll over the pen barrel, causing the dry paint film layer on the surface of the pen barrel to soften instantly and undergo plastic flow, and to sink inward along with the underlying wood fibers to form a clear diamond grid. (4) Remove the pen barrel after pressing in step (3) from the hot pressing area. The transparent polyethylene film is rolled up by the film winding machine (the transparent polyethylene film can be reused or continuously tensioned and rolled up). The paint surface of the pen barrel after leaving the hot pressing area is dense and bright red, with clear and deep diamond patterns and no micro-cracks. Then, the pen barrel enters the cutting machine for flat cutting at both ends and enters the sharpening machine for sharpening the lead core. Finally, after passing the inspection, it is packaged and put into storage.
[0047] Application Example 4 A method for rolling a 3D texture on a pencil surface, which differs from Application Example 1 only in that the modified water-based pencil paint provided in Example 4 is used instead of the modified water-based pencil paint provided in Example 1, while the other materials, parameters and steps are the same as in Application Example 1.
[0048] Application Example 5 A rolling molding method for 3D texture on the surface of a pencil is different from Application Example 1 only in that the average thickness of the dry paint film on the surface of the pencil barrel in step (1) is 35 μm. Other materials, parameters and steps are the same as in Application Example 1.
[0049] Application Example 6 A rolling molding method for 3D texture on the surface of a pencil, which differs from Application Example 1 only in that the width of the raised lines and the gap between the lines in step (3) are both 0.45 mm. Other materials, parameters and steps are the same as in Application Example 1.
[0050] Application Example 7 A rolling molding method for 3D texture on the surface of a pencil, which differs from Application Example 1 only in that the width of the raised lines and the gap between the lines in step (3) are both 0.85 mm. Other materials, parameters and steps are the same as in Application Example 1.
[0051] Comparative Application Example 1 A method for rolling a 3D texture on a pencil surface, which differs from Application Example 1 only in that the modified water-based pencil paint provided in Comparative Example 1 is used instead of the modified water-based pencil paint provided in Example 1, while the other materials, parameters and steps are the same as in Application Example 1.
[0052] By observing the surface of the pencil shaft obtained in Example 4 under a magnifying glass, it was found that the paint film at the edge of the diamond grid depression on the surface of the pencil shaft showed obvious mesh-like microcracks, and the paint film was easy to peel off during the abrasion resistance test.
[0053] Comparative Application Example 2 A method for rolling a 3D texture on the surface of a pencil, which differs from Application Example 1 only in that, in step (3), a transparent polyethylene film is not conveyed while the pencil barrel enters the roller imprinting area. Other materials, parameters and steps are the same as in Application Example 1.
[0054] After hot-pressing five pencils using the rolling molding method provided in Comparative Application Example 2, red resin residue began to adhere to the surface of the metal roller mold, and the surface of the subsequently pressed pencil barrels showed signs of fuzzing, stringing, and loss of gloss.
[0055] Performance testing: (1) Paint film appearance: Under a magnifying glass, observe whether the 3D rhomboid mesh texture on the surface of the final pencil is clear, whether there are obvious mesh microcracks on the paint film at the concave edge of the rhomboid mesh, and whether the paint film is easy to peel off when further abrasion test is conducted. The abrasion test method is the roller method.
[0056] (2) Hot pressing paint adhesion phenomenon: After hot pressing 5 pencils, observe whether there is red resin residue on the surface of the metal roller mold, and whether the surface of the subsequently pressed pencil barrels shows fuzzing, stringing and loss of gloss.
[0057] The pencils provided in Test Cases 1-7 and Comparative Application Examples 1-2 were tested according to the above test method. The test results are shown in Table 2. Table 2 According to the data in Table 2: The 3D texture of the paint film formed on the surface of the pencils provided in Application Examples 1 to 7 is clear and does not stick to the mold during the hot pressing process; while the paint film on the edge of the diamond grid recess on the barrel surface of the pencil provided in Comparative Application Example 1 shows obvious mesh microcracks and the paint film is easy to peel off during the abrasion resistance test; the paint film of the pencil provided in Comparative Application Example 2 sticks to the mold during the hot pressing process.
[0058] The above description is only a specific embodiment of this application, but the protection scope of this application is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in this application fall within the protection and disclosure scope of this application.
Claims
1. A modified water-based pencil paint, characterized in that, The modified water-based pencil paint comprises the following components by weight: 70-85 parts by weight of water-based base paint; Plasticizer 2-4 parts by weight; Other additives: 10-25 parts by weight; The water-based base paint includes water-based acrylic emulsions and / or water-based polyurethane emulsions.
2. The modified water-based pencil paint according to claim 1, characterized in that, The solid content of the aqueous acrylic emulsion is 20-40%; And / or, the solid content of the aqueous polyurethane emulsion is 20-40%.
3. The modified water-based pencil paint according to claim 1 or 2, characterized in that, The plasticizers include triethyl citrate and / or dibutyl phthalate.
4. The modified water-based pencil paint according to any one of claims 1 to 3, characterized in that, The other additives include any one or a combination of at least two of the following: colorants, film-forming aids, defoamers, or leveling agents.
5. A method for preparing modified water-based pencil paint as described in any one of claims 1 to 4, characterized in that, The preparation method includes: mixing water-based base paint and other additives, then adding plasticizer and mixing to obtain the modified water-based pencil paint.
6. A method for rolling a pencil with a 3D textured surface, characterized in that, The roll forming method includes the following steps: (1) Apply the modified water-based pencil paint as described in any one of claims 1 to 4 to the surface of a planed wooden pencil shaft, and dry it to obtain a pencil shaft with a dry paint film layer. (2) Print graphic markings on the surface of the pen barrel with the dry paint film layer obtained in step (1) to form a planar graphic layer; (3) The pen barrel after printing the graphic logo in step (2) is sent into the hot press roller printing machine. A layer of transparent polyethylene film is inserted between the roller of the hot press roller printing machine and the pen barrel. The transparent polyethylene film is flatly covered on the dry paint film layer of the pen barrel. The roller rolls the pen barrel under heating and pressure, so that the dry paint film layer on the surface of the pen barrel is deformed to form a 3D texture pattern corresponding to the 3D texture on the surface of the roller. (4) Remove the pencil barrel after rolling in step (3) from the hot pressing area, and cut and sharpen it in sequence to obtain a pencil with a 3D texture on the surface, thus completing the rolling forming method.
7. The roll forming method according to claim 6, characterized in that, The thickness of the dry paint film layer in step (1) is 45~60 μm.
8. The roll forming method according to claim 6 or 7, characterized in that, The surface of the roller in step (3) is engraved with a reverse diamond grid pattern; And / or, the width of the raised lines in the 3D texture of the roller surface in step (3) is 0.5~0.8 mm; And / or, the recessed gaps between lines in the 3D texture of the roller surface described in step (3) are 0.5~0.8 mm; And / or, the thickness of the transparent polyethylene film in step (3) is 0.02~0.04 mm.
9. The roll forming method according to any one of claims 6 to 8, characterized in that, The heating temperature in step (3) is 110~130℃; And / or, the pressure applied in step (3) is 0.3~0.5 MPa.
10. A pencil with a 3D textured surface, characterized in that, The pencil is manufactured using the rolling forming method as described in any one of claims 6 to 9.