A hyperbranched resin-modified in-situ conversion type rust-resistant heavy-duty anti-corrosion coating and its preparation method
By combining hyperbranched resin with epoxy-modified silicone resin and using multi-component conversion agents and fillers, the problems of incomplete rust conversion and insufficient performance of heavy-duty anti-corrosion coatings with rust have been solved, achieving a high-efficiency and long-lasting heavy-duty anti-corrosion effect, suitable for harsh working conditions such as marine environments and chemical industrial parks.
Patent Information
- Application Number
- CN202611005836.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-07
- Publication Date
- 2026-11-10
AI Technical Summary
Existing heavy-duty anti-corrosion coatings for rust-resistant materials suffer from problems such as incomplete rust conversion, poor mechanical properties of the coating, weak weather and corrosion resistance, poor storage stability, and short long-term protective life, which cannot meet the long-term heavy-duty anti-corrosion requirements of high-end industrial steel structures.
By combining hyperbranched polyester resin with epoxy-modified silicone resin, along with multi-component rust conversion agents and composite rust-inhibiting fillers, a highly efficient in-situ conversion type heavy-duty anti-corrosion coating for rusty surfaces is formed. This coating achieves deep penetration and complete conversion of rust, improves the adhesion, flexibility, density, and weather resistance of the coating, and simplifies the construction process.
It achieves complete transformation of rust layers, and the coating's high adhesion and flexibility significantly improve weather resistance and resistance to media corrosion, extend protective life, reduce construction costs and pollution, and is suitable for harsh industrial corrosion protection conditions.
Smart Images

Figure CN123063041A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of heavy-duty anti-corrosion coatings, specifically to a hyperbranched resin-modified in-situ conversion type rust-bearing heavy-duty anti-corrosion coating and its preparation method. Background Technology
[0002] Rust-resistant coatings, as functional anti-corrosion coatings that can be applied directly to rust-covered metal substrates without requiring complete rust removal, simplify construction procedures, reduce construction costs, and minimize construction pollution. They are suitable for the anti-corrosion needs of various complex construction sites and have become a research hotspot in the field of heavy-duty anti-corrosion coatings. Existing rust-resistant heavy-duty anti-corrosion coatings are mainly divided into three categories: physical shielding, rust stabilizing, and rust conversion. Physical shielding rust-resistant coatings rely solely on a resin film-forming system to isolate corrosive media, but cannot address the existing rust on the substrate surface. The rust will continue to expand beneath the coating, eventually destroying the coating system. Rust-stabilizing coatings passivate the rust layer with fillers, but the stabilizing effect is limited, resulting in poor long-term anti-corrosion performance and unsuitability for harsh corrosive conditions. Rust conversion coatings react with rust through chemical components, transforming loose, active rust into a stable, inert protective film, and are currently the type of rust-resistant coating with the best overall performance.
[0003] Currently, existing in-situ conversion heavy-duty anti-corrosion coatings for rust still have many technical defects, which restrict their large-scale industrial application. Firstly, most existing coatings use linear epoxy resins and alkyd resins as film-forming matrices. Linear resins have high molecular chain regularity and high viscosity, resulting in low solid content, poor thick-coating properties, and tightly wrapped molecular chains, leading to insufficient coating flexibility and impact resistance. During the thermal expansion and contraction of the substrate, the coating is prone to cracking and peeling. At the same time, the linear resin system has a low functional group density, resulting in weak reaction and bonding ability with the rust layer, incomplete rust conversion, and residual active rust that can easily cause localized corrosion.
[0004] Secondly, existing rust conversion systems have simple formulations, often using a single phosphate-based conversion agent. The conversion reaction rate is slow, and the conversion products have poor stability. They can only convert surface rust and cannot penetrate to the underlying micro-rust areas. Under high humidity and high salt spray conditions, the conversion film is prone to damage and failure, resulting in insufficient corrosion resistance. Furthermore, a single conversion agent is prone to localized excessive acidification and corrosion, damaging the clean metal substrate and causing a decrease in coating adhesion.
[0005] Third, existing rust-resistant coatings have poor weather resistance and resistance to media corrosion. Conventional resin systems are not resistant to ultraviolet aging and acid, alkali and salt corrosion. Long-term outdoor use can easily lead to chalking, loss of gloss and peeling, which cannot meet the long-term protection requirements of harsh anti-corrosion conditions such as marine and chemical industrial parks. At the same time, conventional anti-rust fillers are single, the synergistic effect of physical shielding and chemical anti-rust is poor, the coating density is insufficient, and water vapor and corrosive ions can easily penetrate the coating, causing secondary corrosion of the substrate.
[0006] Fourth, the existing rust-resistant coating preparation process has poor adaptability, the filler is not evenly dispersed, and it is easy to agglomerate and settle. The coating has poor storage stability and is prone to stratification and clumping after long-term storage, which affects the construction performance and anti-corrosion effect. Moreover, the mechanical properties of the coating after film formation and curing are uneven, such as adhesion, flexibility and impact resistance, and the overall service performance needs to be improved.
[0007] Hyperbranched resins are a new type of polymer material with a three-dimensional spherical structure. Compared with traditional linear resins, they have unique advantages such as compact molecular structure, low viscosity, high density of end-group functional groups, excellent solubility, and high cross-linking reactivity, making them highly promising for application in the field of coating modification. Hyperbranched resins do not suffer from molecular chain entanglement, which can significantly increase the solid content and thick coating properties of coatings. Their abundant end-group functional groups can form multiple chemical bonds with metal substrates and rust layers, improving coating adhesion and rust layer bonding stability. However, the application of hyperbranched resins in heavy-duty anti-corrosion coatings with rust has not yet formed a mature technical system. Problems exist such as low resin selection matching, unreasonable modification formulations, and poor synergy between rust layer conversion and resin film formation, failing to fully utilize the modification advantages of hyperbranched resins. Currently, there is no efficient in-situ conversion technology for heavy-duty anti-corrosion coatings with rust based on third-generation pentaerythritol-based hyperbranched polyester resin composite epoxy organosilicon modification.
[0008] In summary, existing heavy-duty anti-corrosion coatings for rust generally suffer from technical drawbacks such as incomplete rust conversion, poor mechanical properties of the coating, weak weather and corrosion resistance, poor storage stability, and insufficient long-term protection. These shortcomings fail to meet the long-term heavy-duty anti-corrosion requirements of high-end industrial steel structures under harsh working conditions. Therefore, developing a hyperbranched resin-modified in-situ conversion heavy-duty anti-corrosion coating for rust with high conversion efficiency, excellent film-forming properties, comprehensive anti-corrosion performance, convenient construction, and strong stability is a current research focus and technical challenge for those skilled in the art. Summary of the Invention
[0009] The purpose of this invention is to overcome the shortcomings of existing heavy-duty anti-corrosion coatings for rust-bearing surfaces, such as incomplete rust conversion, poor coating density, unsatisfactory mechanical properties, weak weather and corrosion resistance, poor storage stability, and short long-term protective life. This invention provides a hyperbranched resin-modified in-situ conversion type heavy-duty anti-corrosion coating for rust-bearing surfaces and its preparation method. This invention achieves efficient in-situ conversion of residual rust on metal substrates by compounding a specially formulated hyperbranched polyester resin with an epoxy-modified silicone resin, combined with a multi-component rust conversion system and a composite rust-inhibiting filler system. Simultaneously, it significantly improves the coating's adhesion, flexibility, density, weather resistance, and resistance to media corrosion, simplifies construction procedures, reduces construction costs, and meets the long-term protection requirements of various harsh industrial corrosion-resistant conditions.
[0010] To achieve the above objectives, the present invention provides the following technical solution: This invention provides a hyperbranched resin modified in-situ conversion type heavy-duty anti-corrosion coating for rust, which comprises the following components by weight: 20-35 parts of hyperbranched polyester resin, 15-25 parts of epoxy modified silicone resin, 8-15 parts of rust conversion agent, 12-20 parts of composite anti-rust filler, 2-5 parts of functional additives, and 20-30 parts of solvent.
[0011] The hyperbranched polyester resin is a third-generation hyperbranched polyester synthesized with pentaerythritol as the core and adipic acid and neopentyl glycol as branched monomers. The number average molecular weight is 1800-2500 g / mol. This structure resin has a sufficient number of end functional groups, a compact molecular structure, low viscosity, and high crosslinking reactivity, making it suitable for the film-forming requirements of heavy-duty anti-corrosion coatings.
[0012] The rust conversion agent is a compound of tannic acid, zinc dihydrogen phosphate, and organophosphonic acid in a mass ratio of 3:2:1. The ternary components work synergistically to achieve deep penetration, thorough conversion, and long-term passivation of the rust layer.
[0013] The composite rust-preventive filler is composed of mica iron oxide, zinc phosphate, and nano silica in a mass ratio of 5:3:2, which combines physical shielding, chemical rust prevention, and coating enhancement effects.
[0014] Preferably, the optimal composition ratio of the coating by weight is: 25-30 parts of hyperbranched polyester resin, 18-22 parts of epoxy-modified silicone resin, 10-12 parts of rust conversion agent, 15-18 parts of composite rust-preventive filler, 3-4 parts of functional additives, and 22-28 parts of solvent. Under this ratio, the coating achieves an optimal balance in film-forming performance, corrosion resistance, and application performance.
[0015] Furthermore, the epoxy-modified silicone resin has an epoxy value of 0.25–0.35 eq / 100g and a silicone content of 35–45 wt%. Resins within this parameter range possess excellent adhesion, crosslinking properties, and weather-resistant hydrophobic properties. They also exhibit the best compatibility with hyperbranched polyester resins and show no delamination or precipitation.
[0016] Furthermore, the functional additives include a dispersant, a defoamer, a leveling agent, and an adhesion promoter, with a mass ratio of 4:2:2:3. The dispersant is a high-molecular-weight block polyether dispersant, which can effectively improve the dispersibility of inorganic fillers in the resin system and prevent agglomeration and sedimentation. The defoamer is a polyether-modified silicone defoamer, which can quickly eliminate bubbles during the preparation and application of the coating, ensuring a smooth and dense coating. The leveling agent is an acrylic leveling agent, which improves the leveling properties of the coating, resulting in a smooth and even coating surface after application, free from orange peel or brush marks. The adhesion promoter is a silane coupling agent KH-550, which further strengthens the adhesion between the coating and the metal substrate and rust layer.
[0017] Furthermore, the solvent is a mixed solvent of xylene, n-butanol, and butyl acetate in a mass ratio of 5:3:2. This mixed solvent has excellent solubility in the dual resin system of the present invention and a moderate evaporation rate, which can ensure good application fluidity and film smoothness of the coating and avoid problems such as pinholes and cracks in the coating caused by excessive solvent evaporation.
[0018] Secondly, the present invention provides a method for preparing the above-mentioned hyperbranched resin-modified in-situ conversion type rust-resistant heavy-duty anti-corrosion coating, comprising the following steps: S1. Base liquid premixing: Add the mixed solvent, dispersant, and defoamer into a closed stirring tank according to the formula, stir at a low speed of 300-400 r / min for 3-5 min, and control the stirring temperature at 20-25℃ to ensure that the additives and solvents are fully mixed to obtain a uniform and transparent mixed base liquid, avoid local agglomeration of additives, and lay the foundation for subsequent filler dispersion.
[0019] S2. Preparation of anti-rust slurry: Add composite anti-rust filler to the mixed base liquid in batches. Batch addition can avoid the agglomeration and accumulation caused by adding the filler all at once. Disperse at high speed of 1200-1500 r / min for 20-30 min to initially break up the agglomerated filler particles. Then, use a horizontal sand mill to grind until the fineness of the slurry is ≤30μm to ensure that the filler particles are uniformly fined and free of large particles, so as to obtain a fine and stable anti-rust slurry.
[0020] S3. Resin Composite Mixing: Place the ground rust-preventive slurry in a mixing tank and add hyperbranched polyester resin and epoxy-modified silicone resin in sequence under medium-speed stirring at 600-800 r / min. Continue stirring for 15-20 min with the mixture kept in a closed container to reduce solvent evaporation and ensure that the two resins are fully compatible and evenly dispersed to form a stable resin mixture, thus ensuring the uniformity of the resin crosslinking system.
[0021] S4. Functional Modification and Filtration: Add rust conversion agent, leveling agent and adhesion promoter to the resin mixture in sequence, and stir continuously for 10-15 minutes to allow the functional components to fully integrate and react. After stirring, filter with a 200-mesh stainless steel filter to remove trace impurities and undispersed particles, and adjust the coating viscosity to 80-100 KU (25℃) to finally obtain the finished product of hyperbranched resin modified in-situ conversion type rust-resistant heavy-duty anti-corrosion coating.
[0022] Compared with the prior art, the present invention has the following advantages: Compared with the prior art, this invention has the following significant advantages: through multi-dimensional technical improvements, it systematically solves various technical defects of existing heavy-duty anti-corrosion coatings for rust-prone surfaces: (1) Excellent rust layer conversion effect, completely solving the problem of secondary corrosion under the coating. This invention adopts a ternary compound conversion system of tannic acid, zinc dihydrogen phosphate and organophosphonic acid. Relying on the strong penetrating performance of organophosphonic acid, it can penetrate into the loose rust layer, micro-rust and oxide scale on the substrate surface. Through multiple chemical reactions of complexation, passivation and phosphating, the active loose rust is completely converted into a dense, inert and water-insoluble composite protective film. The conversion is thorough and there is no residue. It can stably seal the substrate surface and prevent the corrosive medium from contacting the metal substrate. It solves the problem of incomplete rust layer conversion and continuous corrosion under the coating of traditional rust-bearing coatings from the root. It is suitable for direct construction on rust-bearing substrates. There is no need for thorough sandblasting to remove rust. It greatly simplifies the construction process and reduces construction costs and construction pollution.
[0023] (2) The overall mechanical properties and film-forming properties of the coating are greatly improved. This invention adopts a dual-composite film-forming system of third-generation hyperbranched polyester resin and epoxy-modified silicone resin. The hyperbranched resin has a three-dimensional structure without molecular chain entanglement, the resin system has low viscosity, and the coating has high solid content, which can realize thick coating construction. The dry film thickness of a single construction can reach 80-120μm, and the construction efficiency is greatly improved. At the same time, the high-density end functional groups of the hyperbranched resin cross-link with the epoxy silicone resin to form a three-dimensional dense network structure, which significantly improves the coating adhesion, flexibility, and impact resistance. The coating adhesion to rusted substrates can reach level 1, the impact strength is ≥50cm, and there is no cracking or peeling when bent. It can effectively adapt to complex working conditions such as thermal expansion and contraction of the substrate and mechanical vibration, and avoid coating damage and failure.
[0024] (3) Excellent weather resistance and resistance to media corrosion, with a long-lasting protective life. The dual-resin compound system combines the excellent UV aging resistance and high and low temperature resistance of silicone resin with the acid and alkali resistance and salt spray resistance of epoxy resin, along with the multiple shielding protection of ternary composite anti-rust filler. The coating has extremely high density and can effectively block the penetration of corrosive media such as water vapor, oxygen, salt spray, and acids and alkalis. According to the test, the coating of this invention has a salt spray resistance time of ≥2000h, an artificial accelerated aging time of ≥3000h, excellent acid and alkali immersion resistance, and an outdoor long-lasting protective life of 8 to 10 years, which far exceeds the existing ordinary rust-bearing heavy-duty anti-corrosion coatings. It can meet the long-lasting protection requirements of harsh anti-corrosion working conditions such as marine engineering, chemical industrial parks, and heavy machinery.
[0025] (4) Excellent storage and construction stability of the coating. This invention achieves uniform dispersion of inorganic fillers in the organic resin system through a precise step-by-step preparation process, combined with a high-efficiency dispersant and compound solvent system, without agglomeration, sedimentation or stratification. The coating can be stored at room temperature for more than 12 months without clumping, deterioration or sudden viscosity change, and has excellent storage stability. At the same time, the coating has good leveling and construction fluidity, and can be adapted to various construction methods such as brushing, rolling and spraying. After construction, the coating is smooth and flat, without defects such as pinholes, orange peel, and bubbles. It has strong construction adaptability and can realize industrial mass production and large-scale on-site construction.
[0026] (5) Green and environmentally friendly, with high construction safety. This invention adopts a high solid content and low solvent formula. Compared with traditional low solid content coatings, the amount of organic solvent volatilization is greatly reduced. There are no heavy metals or toxic and harmful additives added, which meets the national green coating environmental protection standards. No large amount of toxic and harmful gases are released during the construction process, and the construction safety is high. It is suitable for various green construction project requirements. Attached Figure Description
[0027] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0028] Figure 1 This is a schematic diagram of the cross-sectional structure of the substrate after the rust-resistant heavy-duty anti-corrosion coating of the present invention has been applied and film-formed; Figure 2 This is a flowchart illustrating the in-situ transformation and protection mechanism of the coating rust layer according to the present invention. Detailed Implementation
[0029] The following will be combined with the appendix of the present invention. Figure 1 , Figure 2 The technical solutions in the embodiments of the present invention are clearly and completely described herein. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0030] It should be noted that the terms "first" and "second" in this invention are used for descriptive purposes only and should not be construed as indicating or implying relative importance. The terms "connection," "installation," and "fixation," etc., should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; and they can refer to the internal connection of two components. Those skilled in the art can understand the specific meaning of the above terms in this invention according to the specific circumstances.
[0031] All raw materials used in the embodiments of this invention are commercially available industrial-grade conventional raw materials, without any special customized raw materials. The raw materials are readily available and suitable for industrial mass production. The number-average molecular weight of the third-generation pentaerythritol-based hyperbranched polyester resin is controlled at 1800-2500 g / mol, the epoxy value of the epoxy-modified silicone resin is 0.25-0.35 eq / 100g, and the silicone content is 35-45 wt%. All additives, solvents, and fillers meet the standards for use in industrial heavy-duty anti-corrosion coatings.
[0032] Example 1 A hyperbranched resin-modified in-situ conversion type heavy-duty anti-corrosion coating for rust, comprising the following components by weight: 20 parts hyperbranched polyester resin, 15 parts epoxy-modified silicone resin, 8 parts rust conversion agent, 12 parts composite anti-rust filler, 2 parts functional additives, and 20 parts solvent.
[0033] The rust conversion agent is a mixture of tannic acid, zinc dihydrogen phosphate, and organophosphonic acid in a mass ratio of 3:2:1; the composite rust-preventive filler is a mixture of mica iron oxide, zinc phosphate, and nano silica in a mass ratio of 5:3:2; the functional additives include a dispersant, defoamer, leveling agent, and adhesion promoter in a mass ratio of 4:2:2:3; and the solvent is a mixture of xylene, n-butanol, and butyl acetate in a mass ratio of 5:3:2.
[0034] The preparation method includes the following steps: S1. Base liquid premixing: Add 20 parts of mixed solvent, 0.8 parts of dispersant and 0.4 parts of defoamer into a closed stirring tank, stir at a low speed of 300 r / min for 5 min, and stir at a stirring temperature of 20℃ to obtain a uniformly mixed base liquid; S2. Preparation of anti-rust slurry: Add 12 parts of composite anti-rust filler to the mixed base liquid in 3 portions, disperse at high speed of 1200r / min for 30min, and then grind with a horizontal sand mill until the fineness of the slurry is ≤30μm to obtain a fine and stable anti-rust slurry; S3. Resin composite mixing: Place the rust-preventive slurry in a mixing tank and stir at a medium speed of 600 r / min. Add 20 parts of hyperbranched polyester resin and 15 parts of epoxy-modified organosilicon resin in sequence, and stir in a sealed container for 20 min to obtain a uniform resin mixture. S4. Functional modification and filtration: Add 8 parts of rust conversion agent, 0.4 parts of leveling agent, and 0.6 parts of adhesion promoter to the resin mixture, stir for 15 minutes, filter with a 200-mesh stainless steel filter, and adjust the viscosity of the coating at 25℃ to 80KU to obtain the finished coating.
[0035] Example 2 A hyperbranched resin-modified in-situ conversion type heavy-duty anti-corrosion coating for rust, comprising the following components by weight: 28 parts hyperbranched polyester resin, 20 parts epoxy-modified silicone resin, 11 parts rust conversion agent, 16 parts composite anti-rust filler, 3.5 parts functional additives, and 25.5 parts solvent.
[0036] The proportions and raw material parameters of each group are consistent with those in Example 1.
[0037] The preparation method includes the following steps: S1. Base liquid premixing: Add 25.5 parts of mixed solvent, 1.4 parts of dispersant and 0.7 parts of defoamer to a closed stirring tank, stir at a low speed of 350 r / min for 4 min, and stir at a stirring temperature of 22℃ to obtain a uniformly mixed base liquid; S2. Preparation of anti-rust slurry: Add 16 parts of composite anti-rust filler to the mixed base liquid in 3 portions, disperse at high speed of 1350r / min for 25min, and grind in a horizontal sand mill until the fineness of the slurry is ≤30μm to obtain the anti-rust slurry; S3. Resin composite mixing: Under medium-speed stirring at 700r / min, 28 parts of hyperbranched polyester resin and 20 parts of epoxy-modified organosilicon resin were added to the anti-rust slurry in sequence, and the mixture was stirred in a sealed container for 18 minutes to obtain a resin mixture. S4. Functional modification and filtration: Add 11 parts rust conversion agent, 0.7 parts leveling agent, and 1 part adhesion promoter, stir for 12 minutes, filter through a 200-mesh filter, and adjust the viscosity to 90KU at 25℃ to obtain the finished coating.
[0038] Example 3 A hyperbranched resin-modified in-situ conversion type heavy-duty anti-corrosion coating for rust, comprising the following components by weight: 35 parts hyperbranched polyester resin, 25 parts epoxy-modified silicone resin, 15 parts rust conversion agent, 20 parts composite anti-rust filler, 5 parts functional additives, and 30 parts solvent.
[0039] The proportions and raw material parameters of each group are consistent with those in Example 1.
[0040] The preparation method includes the following steps: S1. Base liquid premixing: Add 30 parts of mixed solvent, 2 parts of dispersant and 1 part of defoamer into a closed stirring tank, stir at low speed of 400r / min for 3min, stirring temperature of 25℃, to obtain a uniformly mixed base liquid; S2. Preparation of anti-rust slurry: Add 20 parts of composite anti-rust filler to the mixed base liquid in 4 portions, disperse at high speed of 1500r / min for 20min, and grind in a horizontal sand mill until the fineness of the slurry is ≤30μm to obtain the anti-rust slurry; S3. Resin composite mixing: Under medium-speed stirring at 800r / min, 35 parts of hyperbranched polyester resin and 25 parts of epoxy-modified organosilicon resin were added in sequence, and the mixture was stirred in a sealed container for 15min to obtain a resin mixture. S4. Functional modification and filtration: Add 15 parts rust conversion agent, 1 part leveling agent, and 1.5 parts adhesion promoter, stir for 10 minutes, filter through a 200-mesh filter, and adjust the viscosity to 100KU at 25℃ to obtain the finished coating.
[0041] Comparative Example 1 The conventional linear epoxy resin rust-resistant coating uses conventional bisphenol A type linear epoxy resin to replace the hyperbranched polyester resin and epoxy modified silicone resin of this invention. The remaining fillers, additives, solvent components and preparation process are completely consistent with those in Example 2, thus preparing a conventional rust-resistant heavy-duty anti-corrosion coating.
[0042] Comparative Example 2 A single rust conversion agent coating was prepared by using phosphoric acid as the rust conversion agent instead of the ternary compound rust conversion agent of the present invention. The remaining component ratios, raw material parameters, and preparation process were completely consistent with those of Example 2.
[0043] Comparative Example 3 A single-component anti-rust filler coating was prepared by using a single mica iron oxide as the anti-rust filler to replace the ternary composite anti-rust filler of the present invention. The remaining component ratios, raw material parameters, and preparation processes were completely consistent with those of Example 2.
[0044] Performance testing To verify the superior performance of the coatings of the present invention, the coatings prepared in Examples 1-3 and Comparative Examples 1-3 of the present invention were subjected to uniform performance testing. All tests were conducted in accordance with national coating industry standards. The test substrate was a rusted Q235 steel structural steel plate with a uniform thin rust on the surface of the steel plate. No sandblasting was performed. The application method was spraying, and the dry film thickness was controlled at 100 μm. After standard curing for 7 days, various performance tests were conducted. The specific test items and test results are shown in Table 1 below.
[0045]
[0046] Table 1 Performance test results of coatings in each example and comparative example The performance test data in the table above clearly show that the hyperbranched resin-modified in-situ conversion type rust-resistant heavy-duty anti-corrosion coatings prepared in Examples 1-3 of this invention have significantly better performance indicators than existing traditional coatings and the comparative examples. Example 2 is the optimal example, with coating adhesion reaching level 1, impact strength of 55 cm, flexibility of 1 mm, salt spray tolerance of up to 2200 h, artificial aging time of 3200 h, room temperature storage stability of up to 12 months, complete rust conversion, no residual active rust, and the best overall performance.
[0047] Comparative Example 1 uses a traditional linear epoxy resin system, which has poor film toughness and low crosslinking density, resulting in a significant decrease in the mechanical properties, corrosion and weather resistance of the coating, and poor storage stability. This fully verifies the innovation and technical advantages of the dual-resin compound modification system of this invention. Comparative Example 2 uses a single rust conversion agent, which has insufficient rust penetration and conversion ability, incomplete conversion effect, and significantly reduced anti-corrosion performance, demonstrating the synergistic effect of the ternary compound conversion system. Comparative Example 3 uses a single rust-inhibiting filler, which has insufficient coating shielding and chemical rust prevention capabilities, resulting in weak overall protective performance. This verifies the technical advantages of the composite filler system of this invention.
[0048] Meanwhile, the coatings in the various embodiments of the present invention have excellent construction performance, can be adapted to a variety of construction processes, and are free from construction defects such as sagging, pinholes, and bubbles. The high solids content formula can achieve thick coating construction, greatly improving construction efficiency and reducing construction costs. They are green and environmentally friendly with no heavy metal pollution, and fully meet the high-end application needs of the industrial heavy corrosion protection field.
[0049] This invention establishes a stable and widely adaptable heavy-duty anti-corrosion coating system for rust-prone areas by defining precise raw material ratios, resin parameters, and preparation process parameters. The ratios of each raw material component are within a reasonable range, and the process parameters are highly controllable, making it suitable for large-scale industrial production. This coating is not only suitable for corrosion protection of steel structures in ordinary atmospheric environments, but also adaptable to various harsh corrosion protection scenarios such as marine salt spray environments, chemical acid and alkali corrosion environments, outdoor high-temperature exposure environments, and humid underground conditions. Its applications cover all categories of industrial steel structure facilities, including bridges, ships, port machinery, oil storage tanks, chemical equipment, engineering machinery, and steel structure workshops.
[0050] This invention eliminates the need for thorough rust removal of the substrate. Only loose rust, oil, and impurities on the substrate surface need to be removed before direct application. Compared to traditional anti-corrosion coating application processes, it can reduce rust removal workload by more than 60%, shorten construction period by more than 30%, and reduce overall construction costs by about 25%. It also avoids dust pollution caused by sandblasting, aligns with the trend of green industrial construction, and possesses extremely high economic, social, and industrialization potential.
[0051] This invention achieves a systematic breakthrough in the technical bottlenecks of existing heavy-duty anti-corrosion coatings with rust through four technological innovations: hyperbranched resin modification, multi-element conversion system, composite filler protection, and precise process optimization. It solves long-standing technical problems in the industry such as incomplete rust layer conversion, poor coating performance, short anti-corrosion life, and insufficient stability, and realizes a comprehensive upgrade in the performance of heavy-duty anti-corrosion coatings with rust, providing a brand-new technical solution for the field of high-end heavy-duty anti-corrosion coatings.
[0052] The above description is merely a preferred embodiment of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention. Technical features, process parameters, and formula fine-tuning not described in detail in the present invention are all contents that can be conventionally derived, substituted, and optimized by those skilled in the art based on the core technical solution of the present invention, and all fall within the scope of protection of the present invention.
Claims
1. A hyperbranched resin-modified in-situ conversion type rust-resistant heavy-duty anti-corrosion coating, characterized in that, The product comprises, by weight, the following components: 20-35 parts hyperbranched polyester resin, 15-25 parts epoxy-modified silicone resin, 8-15 parts rust conversion agent, 12-20 parts composite rust-inhibiting filler, 2-5 parts functional additives, and 20-30 parts solvent; the hyperbranched polyester resin is a third-generation hyperbranched polyester synthesized with pentaerythritol as the core and adipic acid and neopentyl glycol as branched monomers, with a number average molecular weight of 1800-2500 g / mol; the rust conversion agent is a compound of tannic acid, zinc dihydrogen phosphate, and organophosphonic acid in a mass ratio of 3:2:1; the composite rust-inhibiting filler is a compound of mica iron oxide, zinc phosphate, and nano silica in a mass ratio of 5:3:
2.
2. The hyperbranched resin-modified in-situ conversion type rust-resistant heavy-duty anti-corrosion coating according to claim 1, characterized in that, By weight, it comprises the following preferred components: 25-30 parts of hyperbranched polyester resin, 18-22 parts of epoxy-modified silicone resin, 10-12 parts of rust conversion agent, 15-18 parts of composite rust-inhibiting filler, 3-4 parts of functional additives, and 22-28 parts of solvent.
3. The hyperbranched resin-modified in-situ conversion type rust-resistant heavy-duty anti-corrosion coating according to claim 1, characterized in that, The epoxy-modified silicone resin has an epoxy value of 0.25–0.35 eq / 100g and a silicone content of 35–45 wt%.
4. The hyperbranched resin-modified in-situ conversion type rust-resistant heavy-duty anti-corrosion coating according to claim 1, characterized in that, The functional additives include a dispersant, a defoamer, a leveling agent, and an adhesion promoter, with a mass ratio of 4:2:2:
3. The dispersant is a high molecular weight block polyether dispersant, the defoamer is a polyether-modified silicone defoamer, the leveling agent is an acrylate leveling agent, and the adhesion promoter is a silane coupling agent KH-550.
5. The hyperbranched resin-modified in-situ conversion type rust-resistant heavy-duty anti-corrosion coating according to claim 1, characterized in that, The solvent is a mixture of xylene, n-butanol, and butyl acetate in a mass ratio of 5:3:
2.
6. A method for preparing a hyperbranched resin-modified in-situ conversion type rust-resistant heavy-duty anti-corrosion coating according to any one of claims 1-5, characterized in that, Includes the following steps: S1. Add the mixed solvent, dispersant and defoamer into the mixing tank according to the ratio, and stir at low speed for 3-5 minutes to obtain the mixed base liquid; S2. Add composite rust-inhibiting filler and nano-silica to the mixed base liquid in batches, disperse at high speed for 20-30 minutes, and then grind until the slurry fineness is ≤30μm to obtain rust-inhibiting slurry; S3. Add hyperbranched polyester resin and epoxy-modified silicone resin to the rust-preventive slurry, stir at medium speed for 15-20 minutes, and mix evenly to obtain a resin mixture. S4. Add rust conversion agent, leveling agent and adhesion promoter to the resin mixture, stir for 10-15 minutes, filter and discharge to obtain the finished coating.
7. The preparation method of the hyperbranched resin-modified in-situ conversion type rust-resistant heavy-duty anti-corrosion coating according to claim 6, characterized in that, In step S1, the low-speed stirring speed is 300-400 r / min, and the stirring temperature is 20-25℃.
8. The preparation method of the hyperbranched resin-modified in-situ conversion type rust-resistant heavy-duty anti-corrosion coating according to claim 6, characterized in that, In step S2, the high-speed dispersion speed is 1200-1500 r / min, the grinding equipment is a horizontal sand mill, and the grinding media is zirconia beads.
9. The preparation method of the hyperbranched resin-modified in-situ conversion type rust-resistant heavy-duty anti-corrosion coating according to claim 6, characterized in that, In step S3, the medium-speed stirring speed is 600-800 r / min, and the stirring process is completely sealed to prevent solvent evaporation.
10. The method for preparing the hyperbranched resin-modified in-situ conversion type rust-resistant heavy-duty anti-corrosion coating according to claim 6, characterized in that, In step S4, at an ambient temperature of 25°C, a 200-mesh stainless steel filter screen is used for filtration, and the viscosity of the coating after filtration is controlled at 80-100 KU.