A high-temperature, high-pressure resin-modified fiber-reinforced composite plugging particle for oil-based drilling fluids

By using materials such as aluminate cement, latex, basalt fiber, and graphite to prepare composite plugging particles, and then spraying modified phenolic resin on the surface, the problem of easy failure of plugging materials in deep water and ultra-deep wells under high temperature and high pressure was solved, achieving a stable sealing effect. This method is suitable for plugging operations in deep water high temperature fractured formations.

CN123063148APending Publication Date: 2026-11-10YANGTZE UNIVERSITY +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611309573.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-27
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing plugging materials are difficult to maintain a stable sealing structure under high temperature and high pressure environments, especially in deep water and ultra-deep wells. Conventional materials are prone to softening, pulverizing or failing, and cannot meet the long-term plugging requirements of high temperature and high pressure fractured formations in deep water in the South China Sea.

Method used

Aluminate cement is used as the main pressure-bearing skeleton, combined with high-temperature latex, basalt fiber and elastic graphite. Composite plugging particles are prepared by stirring, molding, curing, crushing and screening. The surface is then sprayed with modified phenolic resin to form a partitioned synergistic structure of pressure-bearing core and resin-impregnated oleophilic layer.

Benefits of technology

Under conditions of 230 ℃ and 5 MPa, the composite plugging particles form a stable particle bridge in the cracks, reducing the risk of damage to the plugging structure. They have good morphological integrity and load-bearing capacity, and are suitable for plugging operations in deep, ultra-deep and deep-water high-temperature fractured formations.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

This invention discloses a high-temperature, high-pressure resin-modified fiber-reinforced composite plugging particle for oil-based drilling fluids and its preparation method, belonging to the technical field of plugging materials for petroleum drilling engineering. The particle uses aluminate cement as the main pressure-bearing skeleton, combined with high-temperature latex, basalt fiber, elastic graphite, and polytetrafluoroethylene to form a cement-based pressure-bearing core. Then, through thin-layer spraying with organosilicon-modified phenolic resin, surface drying, pre-curing, and high-temperature curing, a resin-cement interlocking transition structure is formed on the particle surface. The resulting particle exhibits high temperature resistance, high pressure resistance, breakage resistance, good oil phase wettability, and high sealing stability, making it suitable for plugging operations of oil-based drilling fluids in deep, ultra-deep, and deep-water fractured formations.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the technical field of oilfield chemistry and plugging materials in petroleum drilling engineering, specifically relating to a high-temperature and high-pressure resistant resin-modified fiber-reinforced composite plugging particle for oil-based drilling fluids and its preparation method. Background Technology

[0002] Currently, my country's oil and gas exploration and development is continuously expanding into deeper, ultra-deep, and deep-water areas, significantly increasing the complexity of temperature, pressure, and fractures encountered in the drilling formations. Taking the BY block in the South China Sea as an example, some ultra-deep wells have bottom-hole temperatures reaching 230℃ and bottom-hole pressures reaching 5MPa, with natural fractures, drilling-induced fractures, and high-permeability channels developing together. Under pressure differentials, drilling fluid rapidly leaks along fractures and high-permeability channels, which can, in severe cases, lead to a drop in wellbore fluid column pressure, wellbore instability, stuck pipe, and even well control risks, adversely affecting the safety and continuity of drilling operations. Therefore, whether plugging materials can rapidly form a stable sealing structure in high-temperature, high-pressure, and complex fracture environments has become a critical issue that urgently needs to be addressed in deep-water and ultra-deep drilling engineering.

[0003] Particulate plugging materials (LCMs) construct a particle skeleton by bridging, embedding, and accumulating within fractures. The interlocking contact between particles forms a pressure-bearing chain, thereby reducing drilling fluid loss and improving the pressure-bearing capacity of the lost formation. However, in high-temperature environments of 180–230 °C, conventional walnut shell, rubber particles, and ordinary resin-based plugging materials are prone to thermal degradation, softening and deformation, brittle cracking and pulverization, or interfacial bonding failure. Specifically, plant fiber and walnut shell materials are prone to carbonization and strength reduction under prolonged high temperatures; rubber materials are prone to softening, creep, or loss of elastic support; and ordinary resin particles may become brittle due to thermal aging and break under high pressure and fluid erosion. These changes weaken the embedding, interlocking, and stress transfer capabilities between particles, causing the formed bridging structure to loosen, collapse, or leak back, making it difficult to maintain a stable pressure-bearing sealing layer in fractures over the long term. Existing plugging particles generally fail to simultaneously achieve high-temperature resistance, structural strength, toughness, fracture embedding capacity, and erosion resistance, especially failing to meet the long-term plugging requirements of high-temperature, high-pressure fractured formations in the deep waters of the South China Sea. Therefore, developing new plugging particles with stronger temperature and pressure resistance, toughness, and erosion resistance has become an urgent need for the oil and gas extraction industry. Currently, many high-temperature, high-pressure plugging materials rely on high-strength inorganic materials for constructing the pressure-bearing framework. Considering temperature resistance, pressure bearing capacity, and economic benefits, using high-temperature aluminate cement as the main framework material has significant advantages.

[0004] To balance economic efficiency, high-temperature resistance, pressure bearing capacity, and sealing structure stability, this invention selects refractory cement, high-temperature latex, high-temperature resistant fibers, elastic graphite, and polytetrafluoroethylene (PTFE) as the main raw materials for composite plugging particles. The refractory cement is aluminate cement, which is not easily decomposed under high-temperature conditions and possesses high early strength and structural stability, serving as the main skeleton of the plugging particles and providing the primary pressure bearing capacity. The high-temperature latex, a heat-resistant polymer material, can form a continuous flexible phase within the cement matrix, improving the brittleness of the particles and enhancing their toughness, impact resistance, and thermal shock resistance. The high-temperature resistant fibers are basalt fibers with a length of 1–2 mm, possessing a high melting point and good heat resistance, forming a fiber-reinforced network within the particles and enhancing their pressure bearing capacity in cracks. Elastic graphite, with its flexibility, heat resistance, and deformability, can fill the tiny pores within the cement block particles, improving the density of the plugging particles. PTFE, with its stable carbon-fluorine chain structure, high-temperature resistance, and corrosion resistance, can enhance the corrosion resistance of the plugging particles in acidic underground environments.

[0005] Compared with traditional walnut shells, rubber granules, and ordinary resin-based sealing materials, this invention uses aluminate cement to construct a high-temperature resistant and pressure-bearing skeleton, and uses high-temperature latex and basalt fiber to synergistically toughen and crack-resistant materials. It combines elastic graphite and polytetrafluoroethylene to improve pore filling and interface sealing performance, so that the composite particles have the advantages of high temperature resistance, high pressure resistance, breakage resistance, and erosion resistance. At the same time, after the cement-based pressure-bearing particles are formed and screened, modified phenolic resin is applied by atomized spraying, so that the resin forms a film on the surface and penetrates into the surface pores, forming a partitioned synergistic structure of pressure-bearing core and resin-impregnated oleophilic layer.

[0006] In summary, the high-temperature resistant composite plugging particles provided by this invention not only maintain good morphological integrity and load-bearing capacity in high-temperature and high-pressure drilling environments, but also form stable particle bridges and pressure-bearing chains in fractures, reducing the risk of damage and backflow of the plugging structure under pressure fluctuations and fluid erosion. The raw materials used in this material are readily available, the preparation process is simple, and the production cost is controllable. It is suitable for plugging operations in deep, ultra-deep, and deep-water high-temperature fractured formations, and has good engineering application value and promising prospects for widespread application. Summary of the Invention

[0007] This invention relates to the field of oil drilling plugging materials technology, specifically a high-temperature resistant, high-pressure-bearing fiber-reinforced composite plugging particle and its preparation method. The plugging particle uses aluminate cement (CA-50 type) as the main pressure-bearing skeleton, introduces high-temperature latex to improve material toughness, reinforces the particle's crack resistance with basalt fibers of 1-2 mm length, and enhances the particle's filling and sealing properties, wear resistance, and high-temperature stability through elastic graphite and polytetrafluoroethylene (PTFE, average particle size 200 nm). The plugging particle was tested at 230 °C and 5 MPa using 0.5 mm, 1.5 mm, 3.5 mm, and 5.0 mm crack devices, with cumulative leakage consistently below 20 mL. The prepared cement-based specimen, tested on a universal testing machine, showed a compressive strength of up to 15.8 MPa. The material has widely available raw materials, a simple preparation process, and controllable production costs, making it suitable for plugging operations in deep, ultra-deep, and deep-water high-temperature fractured formations.

[0008] The present invention achieves its above-mentioned objectives through the following technical solutions.

[0009] This invention provides a high-temperature, high-pressure-bearing fiber-reinforced composite plugging particle suitable for deep, ultra-deep, and deep-water high-temperature fractured formations. The materials used in this invention include refractory cement, high-temperature latex, high-temperature fiber, elastic graphite, polytetrafluoroethylene, and water. It is prepared using methods of mixing, molding, curing, crushing, and sieving, with each component proportioned based on the mass of the refractory cement.

[0010] Refractory cement (aluminate cement) 100 parts 35-45 parts water 10-20 parts of high-temperature latex High-temperature fiber (1-2 mm basalt fiber) 0.5-1.5 parts 0.3 to 0.8 parts of elastic graphite Polytetrafluoroethylene (PTFE, average particle size 200 nm) 0.1–0.2 parts By compounding within the above-mentioned content range, composite plugging particles with high temperature resistance, high pressure resistance, breakage resistance, and adaptability to multi-scale cracks can be obtained.

[0011] Preferably, based on 400 g of refractory cement, 140-180 g of water, 40-80 g of high-temperature latex, 2-6 g of basalt fiber with a length of 1-2 mm, 1.2-3.2 g of elastic graphite and 0.4-0.8 g of polytetrafluoroethylene are added.

[0012] The first step is to weigh water and high-temperature latex according to the formula ratio, slowly add the high-temperature latex to the water, and place the slurry cup on the stirrer and stir at a speed of 300-500 r / min to make the high-temperature latex evenly dispersed in the water to form a uniform latex dispersion.

[0013] The second step involves slowly adding aluminate cement, basalt fiber, elastic graphite, and polytetrafluoroethylene sequentially into the slurry cup while maintaining a stirring speed of 300–500 r / min, according to the formula ratio. Rapid, one-time pouring should be avoided during the addition of each component to reduce powder agglomeration and ensure uniform dispersion of the basalt fiber in the slurry.

[0014] The third step is to increase the speed of the mixer to 800-1000 r / min after all the raw materials have been added, and continue mixing for 5-8 minutes to fully mix the cement, latex, fiber, graphite and polytetrafluoroethylene to obtain a uniform, stable composite cement paste with good fluidity.

[0015] The fourth step is to pour the well-mixed composite cement paste into the concrete mold and use a vibrator to thoroughly compact it to remove air bubbles and voids trapped inside the paste. After compaction, the surface of the mold is smoothed to improve the density, structural integrity, and mechanical strength of the cement specimen.

[0016] The fifth step involves placing the mold containing the composite cement slurry in a 90°C constant temperature hydration curing device for 48 hours. After curing, the mold is removed and allowed to cool to room temperature before demolding to obtain a high-temperature resistant fiber-reinforced composite cement block.

[0017] The sixth step is to place the cured composite cement block into a crushing and grinding equipment for crushing and grinding. Then, according to the actual crack sealing requirements, the crushed particles are placed into a vibrating screen for grading and screening to obtain high-temperature and high-pressure resistant composite plugging particles within the required particle size range.

[0018] Step 7: Select a silicone-modified phenolic resin. The resin solution should have the fluidity to atomize and wet the pores on the surface of the particles at 25 ℃. Add the particles to a roller coating device or a fluidized bed device, keeping the particles continuously tumbling or fluidized; spray the resin solution onto the particles using an atomization pressure of 0.2–0.5 MPa, applying 2–5 thin-layer coatings, continuing to roll and surface dry for 5–15 minutes after each coating.

[0019] Step 8: Pre-cure the sprayed granules at 60–90 °C for 0.5–2 h, then cure them at 140–180 °C for 1–4 h. Keep the granules loose during curing to prevent them from sticking together. After cooling, lightly sieve and weigh the cured granules (m1). Calculate the weight gain rate (R) of the cured resin according to R = (m1 − m0) / m0 × 100%. Preferably, R should be controlled at 3–6%.

[0020] The manufacturing process of resin-modified fiber-reinforced composite leak-sealing particles is as follows: Figure 1 As shown The aluminate cement is a high-temperature resistant inorganic material used as the main pressure-bearing skeleton of the composite plugging particles; The high-temperature latex described herein has the functions of heat resistance, toughening, and improving the interfacial bonding performance of cementitious matrix; The basalt fibers are 1-2 mm in length and are added at a rate of 0.5%-1.5% of the mass of aluminate cement to enhance the crack resistance, impact resistance, and bridging properties of the particles. The elastic graphite described herein has the functions of high temperature resistance, flexible filling and improved particle sealing performance; The polytetrafluoroethylene mentioned above is PTFE micro powder with an average particle size of 200 nm, which has high temperature resistance, corrosion resistance, and friction reduction and wear resistance properties; The amount of elastic graphite added is 0.3% to 0.8% of the mass of aluminate cement, and the amount of polytetrafluoroethylene added is 0.1% to 0.2% of the mass of aluminate cement. The amount of water added is 35% to 45% of the mass of aluminate cement, and the amount of high-temperature latex added is 10% to 20% of the mass of aluminate cement; preferably, the amount of water added is 40% and the amount of high-temperature latex added is 15%.

[0021] The sprayed silicone-modified phenolic resin has the functions of high temperature resistance, improving the oil phase wettability of particle surface, and improving particle erosion resistance and sealing stability.

[0022] Compared with the prior art, the present invention has at least the following beneficial effects: (1) The present invention uses refractory cement (aluminate cement) as the main pressure-bearing skeleton, which overcomes the problems of walnut shells, rubber particles and ordinary resin-based sealing materials being easy to soften, pulverize and weaken under high temperature conditions, so that the sealing particles can still maintain good structural integrity and load-bearing capacity under high temperature environment of 230℃.

[0023] (2) The synergistic effect of high-temperature latex and basalt fiber with a length of 1-2 mm can improve the brittleness of cement-based materials, inhibit the generation and propagation of cracks, improve the toughness, impact resistance and thermal shock resistance of plugging particles, and reduce the risk of particle breakage under high pressure extrusion and fluid scouring.

[0024] like Figure 2 At different magnifications, it can be observed that the particle surface maintains a clear continuous matrix without obvious cracks.

[0025] (3) Elastic graphite and polytetrafluoroethylene with an average particle size of 200 nm synergistically fill the micropores inside the cement matrix and improve the contact and sealing performance between the particles and the crack wall, so that the formed sealing layer has good density, wear resistance and anti-backflow stability.

[0026] (4) The plugging particles prepared by the present invention have good adaptability to multi-scale cracks. When the plugging test was carried out on cracks of 0.5 mm, 1.5 mm, 3.5 mm and 5.0 mm at 230 ℃ and 5 MPa, the cumulative leakage was controlled below 20 mL, which can meet the high temperature and high pressure plugging requirements of cracks of different widths.

[0027] (4) such as Figure 3 As shown, the composite cement-based specimen prepared by this invention has a compressive strength of up to 15.8 MPa as tested by a universal testing machine. At the same time, the raw materials used are widely available and cost-controllable, the preparation process is simple, and it is easy to carry out particle crushing, screening and large-scale production, which has good engineering application and promotion value.

[0028] (5) such as Figure 4 As shown, the present invention performs oil phase static contact angle tests on unmodified particles and resin-coated modified particles, and the results are as follows. Figure 4 As shown in the figure. Under the same test conditions, the oil droplet profile on the surface of unmodified cement-based particles was higher, and the contact angle was denoted as θ1; the oil droplet spreading range on the surface of resin-coated modified particles was increased, and the contact angle was denoted as θ2, with θ2 < θ1. This result indicates that the modified phenolic resin thin layer can reduce the wetting resistance of the oil phase on the particle surface and improve the wetting ability of the particle surface for the continuous oil phase of oil-based drilling fluid. The specific value of the contact angle should be based on the results of parallel tests on the same batch of samples. Attached image description: Figure 1 This is a flow chart illustrating the preparation process of the resin-modified fiber-reinforced composite plugging particles of the present invention.

[0029] Figure 2 These are surface microstructure images of the composite plugging particles prepared according to the present invention at different magnifications.

[0030] Figure 3 This is a uniaxial compression test curve of the composite cement-based specimen of the present invention after high-temperature hydration curing.

[0031] Figure 4 This is a comparison of the static contact angle of the oil phase before and after the cement-based sealing particles of the present invention are sprayed with organosilicon-modified phenolic resin.

[0032] in, Figure 4 In the figure, θ1 represents the static contact angle of the oil phase on the surface of cement-based particles without resin coating, and θ2 represents the static contact angle of the oil phase on the surface of particles after coating with silicone-modified phenolic resin, and θ2 < θ1. Detailed implementation method: The present invention will be further described below with reference to specific embodiments, but the scope of protection of the present invention is not limited to the following embodiments. Unless otherwise specified, the amounts of each component in the following embodiments are by mass, and the stirring, molding, curing, crushing and screening equipment used are all commonly used equipment in the art.

[0033] The refractory cement used in the following examples is aluminate cement (CA-50 type), the basalt fiber length is 1-2 mm, the polytetrafluoroethylene is PTFE micro powder with an average particle size of 200 nm, and the elastic graphite is a high-temperature resistant flexible graphite material.

[0034] Example 1:

[0035] High-temperature resistant and high-pressure-bearing fiber-reinforced composite plugging particles are prepared using the following steps: High-temperature resistant and high-pressure-bearing fiber-reinforced composite plugging particles are prepared using the following steps: The first step is to weigh 160 g of water and 60 g of high-temperature latex, add them to the slurry cup in sequence, place the slurry cup on the stirrer, and stir at a speed of 300-500 r / min to make the high-temperature latex evenly dispersed in the water to form a stable latex dispersion.

[0036] In the second step, while maintaining a rotation speed of 300–500 r / min, slowly add 400 g of aluminate cement (CA-50 type), 4 g of basalt fibers with a length of 1–2 mm, 2.2 g of elastic graphite, and 0.6 g of polytetrafluoroethylene (PTFE, average particle size 200 nm) to the slurry cup in sequence. Continuous stirring is maintained during the addition of each solid component to prevent powder agglomeration and fiber entanglement.

[0037] The third step is to increase the speed of the mixer to 800-1000 r / min after all the raw materials have been added, and continue mixing for 5-8 minutes to ensure that the components are fully mixed and a uniform and stable composite cement paste is obtained.

[0038] The fourth step is to pour the obtained composite cement slurry into the cement test block mold, and use a vibrator to vibrate it to remove air bubbles and voids inside the slurry. After vibration, the surface of the test mold is smoothed to ensure the density and structural integrity of the cement test block.

[0039] The fifth step involves placing the mold containing the composite cement slurry in a 90°C constant temperature hydration curing device for 48 hours. After curing, the mold is removed, cooled to room temperature, and demolded to obtain a high-temperature resistant fiber-reinforced composite cement block.

[0040] The sixth step is to place the cured composite cement block into a crushing and grinding equipment for crushing and grinding, and then vibrate and screen the resulting particles according to the target crack width to obtain high temperature and high pressure resistant composite plugging particles within the required particle size range.

[0041] Step 7: Remove surface dust from the sieved particles and dry them at 80 ℃ for 1 h. After cooling, weigh the particles before spraying (m0). Add the dried particles to a roller coating device and keep them continuously tumbling during the spraying process to ensure that all surfaces of the particles are evenly exposed.

[0042] Step 8: Select a silicone-modified phenolic resin liquid with atomized spray flowability and spray it onto the continuously tumbling particle surface under an atomization pressure of 0.3 MPa. Apply three thin layers using a small amount multiple times, continuing to tumble and surface dry for 10 minutes after each application. This allows the resin to spread evenly and partially penetrate the open pores on the particle surface, avoiding excessive application that could cause particle adhesion or the formation of a thick, closed shell.

[0043] Step 9: Pre-cure the sprayed granules at 80 ℃ for 1 h, then raise the temperature to 160 ℃ for 2 h; keep the granules loose during curing. After cooling to room temperature, perform light sieving to remove a small amount of adherent granules, obtaining high-temperature and high-pressure composite plugging granules sprayed with organosilicon-modified phenolic resin. Weigh the cured granules (m1) and calculate the resin curing weight gain rate according to R = (m1 - m0) / m0 × 100%; control R between 3% and 6% by adjusting the spraying amount.

[0044] Example 2:

[0045] The following steps were used to prepare high-temperature resistant and high-pressure-bearing fiber-reinforced composite plugging particles with a low dosage formulation: The first step is to weigh 140 g of water and 40 g of high-temperature latex, add them to the slurry cup in sequence, place the slurry cup on the stirrer, and stir at 300 r / min to make the high-temperature latex evenly dispersed in the water to form a stable latex dispersion.

[0046] In the second step, while maintaining a rotation speed of 300 r / min, slowly add 400 g of aluminate cement (CA-50 type), 2 g of basalt fibers with a length of 1-2 mm, 1.2 g of elastic graphite, and 0.4 g of polytetrafluoroethylene (PTFE, average particle size 200 nm) to the slurry cup in sequence. Continuous stirring is maintained during the addition of each solid component to prevent powder agglomeration and fiber entanglement.

[0047] The third step is to increase the speed of the mixer to 800 r / min after all the raw materials have been added, and continue mixing for 5 minutes to ensure that the components are fully mixed and a uniform and stable composite cement paste is obtained.

[0048] The fourth step is to pour the obtained composite cement slurry into the cement test block mold, and use a vibrator to fully vibrate it to remove air bubbles and voids inside the slurry. After vibration, the surface of the test mold is smoothed.

[0049] The fifth step involves placing the mold containing the composite cement slurry in a 90°C constant temperature hydration curing device for 48 hours. After curing, the mold is removed, cooled to room temperature, and demolded to obtain a high-temperature resistant fiber-reinforced composite cement block.

[0050] The sixth step is to place the cured composite cement block into a crushing and grinding equipment for crushing and grinding, and then perform vibrating sieving according to the target particle size range to obtain high temperature and high pressure resistant composite plugging particles.

[0051] Step 7: Remove surface dust from the sieved particles and dry them at 80 ℃ for 1 h. After cooling, weigh the particles before spraying (m0). Add the dried particles to a roller coating device and keep them continuously tumbling during the spraying process to ensure that all surfaces of the particles are evenly exposed.

[0052] Step 8: Select a silicone-modified phenolic resin liquid with atomized spray flowability and spray it onto the continuously tumbling particle surface under an atomization pressure of 0.3 MPa. Apply three thin layers using a small amount multiple times, continuing to tumble and surface dry for 10 minutes after each application. This allows the resin to spread evenly and partially penetrate the open pores on the particle surface, avoiding excessive application that could cause particle adhesion or the formation of a thick, closed shell.

[0053] Step 9: Pre-cure the sprayed granules at 80 ℃ for 1 h, then raise the temperature to 160 ℃ for 2 h; keep the granules loose during curing. After cooling to room temperature, perform light sieving to remove a small amount of adherent granules, obtaining high-temperature and high-pressure composite plugging granules sprayed with organosilicon-modified phenolic resin. Weigh the cured granules (m1) and calculate the resin curing weight gain rate according to R = (m1 - m0) / m0 × 100%; control R between 3% and 6% by adjusting the spraying amount.

[0054] Example 3:

[0055] The high-dosage formulation of high-temperature resistant and high-pressure-bearing fiber-reinforced composite plugging particles was prepared using the following steps: The first step is to weigh 180 g of water and 80 g of high-temperature latex, add them to the slurry cup in sequence, place the slurry cup on the stirrer, and stir at 500 r / min to make the high-temperature latex evenly dispersed in the water to form a stable latex dispersion.

[0056] In the second step, while maintaining a rotation speed of 500 r / min, slowly add 400 g of aluminate cement (CA-50 type), 6 g of basalt fibers with a length of 1-2 mm, 3.2 g of elastic graphite, and 0.8 g of polytetrafluoroethylene (PTFE, average particle size 200 nm) to the slurry cup in sequence. Continuous stirring is maintained during the addition of each solid component to prevent powder agglomeration and fiber entanglement.

[0057] The third step is to increase the speed of the mixer to 1000 r / min after all the raw materials have been added, and continue mixing for 8 minutes to ensure that the components are fully mixed and a uniform and stable composite cement paste is obtained.

[0058] The fourth step is to pour the obtained composite cement slurry into the cement test block mold, and use a vibrator to fully vibrate it to remove air bubbles and voids inside the slurry. After vibration, the surface of the test mold is smoothed.

[0059] The fifth step involves placing the mold containing the composite cement slurry in a 90°C constant temperature hydration curing device for 48 hours. After curing, the mold is removed, cooled to room temperature, and demolded to obtain a high-temperature resistant fiber-reinforced composite cement block.

[0060] The sixth step is to place the cured composite cement block into a crushing and grinding equipment for crushing and grinding, and then perform vibrating sieving according to the target particle size range to obtain high temperature and high pressure resistant composite plugging particles.

[0061] Step 7: Remove surface dust from the sieved particles and dry them at 80 ℃ for 1 h. After cooling, weigh the particles before spraying (m0). Add the dried particles to a roller coating device and keep them continuously tumbling during the spraying process to ensure that all surfaces of the particles are evenly exposed.

[0062] Step 8: Select a silicone-modified phenolic resin liquid with atomized spray flowability and spray it onto the continuously tumbling particle surface under an atomization pressure of 0.3 MPa. Apply three thin layers using a small amount multiple times, continuing to tumble and surface dry for 10 minutes after each application. This allows the resin to spread evenly and partially penetrate the open pores on the particle surface, avoiding excessive application that could cause particle adhesion or the formation of a thick, closed shell.

[0063] Step 9: Pre-cure the sprayed granules at 80 ℃ for 1 h, then raise the temperature to 160 ℃ for 2 h; keep the granules loose during curing. After cooling to room temperature, perform light sieving to remove a small amount of adherent granules, obtaining high-temperature and high-pressure composite plugging granules sprayed with organosilicon-modified phenolic resin. Weigh the cured granules (m1) and calculate the resin curing weight gain rate according to R = (m1 - m0) / m0 × 100%; control R between 3% and 6% by adjusting the spraying amount.

[0064] Example 4:

[0065] The high-temperature resistant and high-pressure-bearing fiber-reinforced composite plugging particles with a medium-to-high dosage formulation were prepared using the following steps: The first step is to weigh 168 g of water and 72 g of high-temperature latex, add them to the slurry cup in sequence, place the slurry cup on the stirrer, and stir at 400 r / min to make the high-temperature latex evenly dispersed in the water to form a stable latex dispersion.

[0066] In the second step, while maintaining a rotation speed of 400 r / min, slowly add 400 g of aluminate cement (CA-50 type), 4.8 g of basalt fibers with a length of 1-2 mm, 2.8 g of elastic graphite, and 0.8 g of polytetrafluoroethylene (PTFE, average particle size 200 nm) to the slurry cup in sequence. Continuous stirring is maintained during the addition of each solid component to prevent powder agglomeration and fiber entanglement.

[0067] The third step is to increase the speed of the mixer to 900 r / min after all the raw materials have been added, and continue mixing for 6 minutes to ensure that the components are fully mixed and a uniform and stable composite cement paste is obtained.

[0068] The fourth step is to pour the obtained composite cement slurry into the cement test block mold, and use a vibrator to fully vibrate it to remove air bubbles and voids inside the slurry. After vibration, the surface of the test mold is smoothed.

[0069] The fifth step involves placing the mold containing the composite cement slurry in a 90°C constant temperature hydration curing device for 48 hours. After curing, the mold is removed, cooled to room temperature, and demolded to obtain a high-temperature resistant fiber-reinforced composite cement block.

[0070] The sixth step is to place the cured composite cement block into a crushing and grinding equipment for crushing and grinding, and then perform vibrating sieving according to the target particle size range to obtain high temperature and high pressure resistant composite plugging particles.

[0071] Step 7: Remove surface dust from the sieved particles and dry them at 80 ℃ for 1 h. After cooling, weigh the particles before spraying (m0). Add the dried particles to a roller coating device and keep them continuously tumbling during the spraying process to ensure that all surfaces of the particles are evenly exposed.

[0072] Step 8: Select a silicone-modified phenolic resin liquid with atomized spray flowability and spray it onto the continuously tumbling particle surface under an atomization pressure of 0.3 MPa. Apply three thin layers using a small amount multiple times, continuing to tumble and surface dry for 10 minutes after each application. This allows the resin to spread evenly and partially penetrate the open pores on the particle surface, avoiding excessive application that could cause particle adhesion or the formation of a thick, closed shell.

[0073] Step 9: Pre-cure the sprayed granules at 80 ℃ for 1 h, then raise the temperature to 160 ℃ for 2 h; keep the granules loose during curing. After cooling to room temperature, perform light sieving to remove a small amount of adherent granules, obtaining high-temperature and high-pressure composite plugging granules sprayed with organosilicon-modified phenolic resin. Weigh the cured granules (m1) and calculate the resin curing weight gain rate according to R = (m1 - m0) / m0 × 100%; control R between 3% and 6% by adjusting the spraying amount.

[0074] Example aluminate cement / g Water / g High-temperature latex / g Basalt fiber / g Elastic graphite / g PTFE / g Example 1 400 160 60 4.0 2.2 0.6 Example 2 400 140 40 2.0 1.2 0.4 Example 3 400 180 80 6.0 3.2 0.8 Example 4 400 168 72 4.8 2.8 0.8 Performance evaluation:

[0075] The composite cement blocks, uncoated granules, and silicone-modified phenolic resin coated granules prepared in Example 1 were selected for evaluation of compressive strength, oil phase wettability, surface microstructure, erosion resistance, and high-temperature and high-pressure crack sealing performance. Examples 2-4 illustrate that the same process can be used to complete molding, curing, crushing, screening, resin thin-layer spraying, and segmented curing within the component range described in this invention.

[0076] Compressive strength test:

[0077] The composite cement blocks prepared in Example 1 and cured at 90 °C for 48 h were subjected to uniaxial compression tests on a universal testing machine. The load was continuously applied until the specimen failed, and the maximum load was recorded. The compressive strength was calculated based on the area of ​​the specimen subjected to pressure. The test results showed that the compressive strengths of the composite cement blocks in Examples 1-4 reached 15.8, 15.8, 15.7, and 15.7 MPa, respectively, indicating that this material can provide high skeleton strength and load-bearing capacity for the plugging particles.

[0078] Table 2 Compressive strength of composite cement blocks in Examples 1-4

[0079] sample Maintenance temperature / ℃ Maintenance time / h Compressive strength / MPa Example 1 90 48 15.8 Example 2 90 48 15.8 Example 3 90 48 15.7 Example 4 90 48 15.7 High-temperature and high-pressure crack sealing performance test:

[0080] The plugging particles obtained in Examples 1-4 were matched in particle size according to the test crack width and formulated into plugging slurry. Crack plugging tests were conducted using a high-temperature and high-pressure plugging instrument. The test temperature was set at 230 ℃, the test pressure was set at 5 MPa, and the crack widths were set at 0.5 mm, 1.5 mm, 3.5 mm, and 5.0 mm, respectively. The cumulative leakage under each crack condition was recorded during the test, and the results are shown in Table 3.

[0081] Table 3. High-temperature and high-pressure crack sealing performance of plugging particles in Example 1

[0082] Crack width / mm Test temperature / °C Test pressure / MPa Cumulative leakage / mL Blocking results 0.5 230 5 8 Form a stable blockade 1.5 230 5 8 Form a stable blockade 3.5 230 5 11 Form a stable blockade 5.0 230 5 12 Form a stable blockade Table 4. High-temperature and high-pressure crack sealing performance of plugging particles in Example 2

[0083] Crack width / mm Test temperature / °C Test pressure / MPa Cumulative leakage / mL Blocking results 0.5 230 5 6 Form a stable blockade 1.5 230 5 7 Form a stable blockade 3.5 230 5 10 Form a stable blockade 5.0 230 5 13 Form a stable blockade Table 5. High-temperature and high-pressure crack sealing performance of plugging particles in Example 3

[0084] Crack width / mm Test temperature / °C Test pressure / MPa Cumulative leakage / mL Blocking results 0.5 230 5 9 Form a stable blockade 1.5 230 5 9 Form a stable blockade 3.5 230 5 13 Form a stable blockade 5.0 230 5 12 Form a stable blockade Table 6. High-temperature and high-pressure crack sealing performance of plugging particles in Example 4

[0085] Crack width / mm Test temperature / °C Test pressure / MPa Cumulative leakage / mL Blocking results 0.5 230 5 5 Form a stable blockade 1.5 230 5 7 Form a stable blockade 3.5 230 5 11 Form a stable blockade 5.0 230 5 11 Form a stable blockade As shown in Tables 3-6, under the conditions of 230 ℃ and 5 MPa, the composite plugging particles prepared in this invention can effectively seal cracks of different widths in the range of 0.5 to 5.0 mm. The cumulative leakage under each working condition is controlled below 20 mL, indicating that the material has good high temperature and high pressure resistance and multi-scale crack adaptability.

[0086] Evaluation of oil phase wetting properties:

[0087] Take particles of the same size before and after spraying in Example 1, fix the particles, and prepare a relatively flat test surface. Under the same temperature and droplet volume conditions, drop oil-based drilling fluid base oil is applied. After the droplet profile stabilizes, the static contact angle is measured. Parallel tests are performed at no fewer than 5 different locations for each group, and the average value is taken. The oil phase contact angle of the uncoated particles is recorded as θ1, and the oil phase contact angle of the resin-coated modified particles is recorded as θ2. Figure 4 As shown, the spread of oil droplets on the particle surface increases after spraying, and θ2 < θ1, indicating that the silicone-modified phenolic resin thin layer reduces the wetting resistance of the oil phase on the particle surface, which is beneficial to the rapid wetting and uniform dispersion of particles in the continuous oil phase of oil-based drilling fluid.

[0088] In summary, this invention constructs a high-strength pressure-bearing skeleton using aluminate cement and utilizes high-temperature latex, basalt fiber, elastic graphite, and nano-polytetrafluoroethylene to achieve synergistic reinforcement of toughening, crack resistance, pore filling, and corrosion resistance. The resulting plugging particles exhibit good structural stability, compressive strength, and crack sealing ability under high temperature and high pressure conditions, making them suitable for plugging operations in deep, ultra-deep, and deep-water high-temperature fractured formations.

[0089] Comparative Example: Silicate Cement Replacing Aluminate Cement

[0090] Except for replacing the refractory cement (aluminate cement) in the examples with ordinary silicate cement, the types, amounts and preparation processes of the other raw materials are the same as in Example 1.

[0091] First, weigh 160 g of water and 60 g of high-temperature latex, and add them to the slurry cup in sequence. Place the slurry cup on a stirrer and stir at a speed of 300-500 r / min to evenly disperse the high-temperature latex in the water.

[0092] The second step involves adding 400 g of ordinary silicate cement, 4 g of basalt fiber with a length of 1–2 mm, 2.2 g of elastic graphite, and 0.6 g of polytetrafluoroethylene with an average particle size of 200 nm in sequence while maintaining a stirring speed of 300–500 r / min. The mixture is then stirred until all components are evenly dispersed.

[0093] The third step is to increase the speed of the mixer to 800-1000 r / min after all the raw materials have been added, and continue mixing for 5-8 minutes to obtain a uniform composite cement paste.

[0094] The fourth step is to pour the obtained slurry into the concrete mold, use a vibrator to fully vibrate it to remove air bubbles inside the slurry, and then scrape the surface of the mold smooth.

[0095] The fifth step is to place the mold in a 90 ℃ constant temperature hydration curing device for 48 h. After curing is completed and cooled to room temperature, the mold is removed to obtain ordinary silicate cement-based test blocks.

[0096] The sixth step is to test the compressive strength of the specimen using a universal testing machine and compare it with the specimen prepared using aluminate cement in the example.

[0097] Table 7 Compressive properties of specimens with different cementitious matrices

[0098] Sample Cement type Maintenance conditions compressive strength Example 1 aluminate cement 90℃、48h 15.8MPa Comparative Example 1 Silicate cement 90℃、48h 6.3MPa Test results show that, under the same raw material ratios and preparation conditions, the compressive strength of the composite cement block is significantly reduced when ordinary Portland cement is used instead of aluminate cement. Ordinary Portland cement exhibits weaker structural stability under high-temperature curing conditions than aluminate cement, leading to a decrease in the density and load-bearing capacity of the cement matrix. Therefore, plugging particles prepared with ordinary Portland cement are more prone to breakage under high-pressure extrusion, hindering the formation of a stable particle skeleton and load-bearing chain within cracks. In contrast, aluminate cement significantly improves the high-temperature resistance and compressive strength of composite plugging particles, making it more suitable as the main load-bearing material for high-temperature, high-pressure plugging particles.

Claims

1. A high-temperature, high-pressure resin-modified fiber-reinforced composite plugging particle for oil-based drilling fluids, characterized in that... The composite plugging particles comprise a fiber-reinforced cement-based pressure-bearing core and an organosilicon-modified phenolic resin layer formed on the surface of the fiber-reinforced cement-based pressure-bearing core and impregnated into its surface pores. The fiber-reinforced cement-based pressure-bearing core is prepared by mixing, molding, hydration curing, crushing, and screening raw materials including aluminate cement, water, high-temperature latex, basalt fiber, elastic graphite, and polytetrafluoroethylene. Based on 100 parts by weight of aluminate cement, the raw materials include 35-45 parts water, 10-20 parts high-temperature latex, 0.5-1.5 parts basalt fiber, 0.3-0.8 parts elastic graphite, and 0.1-0.2 parts polytetrafluoroethylene.

2. The composite plugging particles according to claim 1, characterized in that, The aluminate cement is CA-50 type aluminate cement, the basalt fiber has a length of 1-2 mm, and the polytetrafluoroethylene is polytetrafluoroethylene micro powder with an average particle size of 200 nm.

3. The composite plugging particles according to claim 1 or 2, characterized in that, Based on 100 parts by weight of aluminate cement, the water comprises 40 parts, the high-temperature latex comprises 15 parts, the basalt fiber comprises 1 part, the elastic graphite comprises 0.55 parts, and the polytetrafluoroethylene comprises 0.15 parts.

4. The composite plugging particles according to any one of claims 1 to 3, characterized in that, The cured resin weight gain R of the organosilicon-modified phenolic resin layer is 3% to 6%. The cured resin weight gain R is calculated according to R = (m1 - m0) / m0 × 100%, where m0 is the mass of the particles before spraying and m1 is the mass of the particles after the resin is cured.

5. The composite plugging particles according to any one of claims 1 to 4, characterized in that, The organosilicon-modified phenolic resin layer is formed by 2 to 5 thin-layer sprayings, with the resin covering the surface of the fiber-reinforced cement-based pressure-bearing core and at least partially penetrating the surface pores.

6. A method for preparing the composite plugging particles according to any one of claims 1 to 5, characterized in that, Includes the following steps: (1) Add high-temperature latex to water and mix at a stirring speed of 300-500 r / min to obtain a latex dispersion; (2) At a stirring speed of 300-500 r / min, aluminate cement, basalt fiber, elastic graphite and polytetrafluoroethylene are added to the latex dispersion in sequence, and then the stirring speed is increased to 800-1000 r / min and stirring is continued for 5-8 min to obtain composite cement paste. (3) The composite cement slurry is injected into the mold and vibrated to form the shape. It is then hydrated and cured at 90 °C for 48 h. After cooling and demolding, fiber-reinforced composite cement blocks are obtained. (4) The fiber-reinforced composite cement block is crushed, ground and sieved to obtain fiber-reinforced cement-based pressure-bearing particles; (5) After drying the fiber-reinforced cement-based pressure-bearing particles, place them in a roller coating equipment or a fluidized bed equipment, and spray the organosilicon-modified phenolic resin liquid onto the particle surface in a continuous rolling or fluidized state. (6) The sprayed particles are pre-cured and high-temperature cured, cooled and sieved to obtain the composite plugging particles.

7. The preparation method according to claim 6, characterized in that, In step (5), the atomizing spraying pressure is 0.2 to 0.5 MPa, and 2 to 5 thin-layer sprayings are used. After each spraying, the particles continue to roll or fluidize and are surface-dried for 5 to 15 minutes.

8. The preparation method according to claim 6 or 7, characterized in that, In step (6), the particles are first pre-cured at 60-90 ℃ for 0.5-2 h, and then cured at 140-180 ℃ for 1-4 h, while keeping the particles loose during the curing process.

9. The preparation method according to any one of claims 6 to 8, characterized in that, In step (5), the sieved particles are de-dust removed and dried at 80 ℃ for 1 h; the atomization spraying pressure is 0.3 MPa, and a total of 3 thin-layer sprayings are performed, with each spraying being surface-dry for 10 min; in step (6), the particles are first pre-cured at 80 ℃ for 1 h, and then cured at 160 ℃ for 2 h.

10. The use of the composite plugging particles according to any one of claims 1 to 5 in the preparation of fracture plugging materials for oil-based drilling fluids.

11. The application according to claim 10, characterized in that, The composite plugging particles are used in fractured formations with temperatures not exceeding 230°C and pressures not exceeding 5 MPa, and the particle size of the composite plugging particles is matched according to the target fracture width in the range of 0.5 to 5.0 mm.