A method for manufacturing ultra-supercritical rotor forgings

By leveraging the synergistic effect of isothermal transformation and high-temperature recrystallization, the microstructure inheritance problem of ultra-supercritical rotor forgings was solved, resulting in grain refinement and a shorter heat treatment cycle, thereby improving production efficiency and product quality.

CN123063583APending Publication Date: 2026-11-10CHINA FIRST HEAVY IND +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610977448.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-02
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing technologies struggle to completely eliminate microstructure inheritance when manufacturing ultra-supercritical rotor forgings, resulting in poor grain refinement and long heat treatment cycles, leading to low production efficiency and high costs.

Method used

The method employs isothermal transformation combined with high-temperature recrystallization, which involves directly using the residual heat from forging for isothermal transformation to generate a balanced ferrite and pearlite microstructure, followed by undercooling, medium-temperature holding and high-temperature austenitization recrystallization, and finally refining the grains by furnace cooling.

Benefits of technology

It significantly improves grain refinement, shortens heat treatment cycle, reduces energy consumption and production costs, while ensuring the microstructure quality of forgings and meeting ultrasonic testing requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123063583A_ABST
    Figure CN123063583A_ABST
Patent Text Reader

Abstract

This invention discloses a manufacturing method for ultra-supercritical rotor forgings, belonging to the field of large forging manufacturing technology. It addresses the technical problem in existing technologies where C630R heat-resistant steel is used to manufacture ultra-supercritical rotor forgings, where it is difficult to completely eliminate microstructure inheritance and the grain refinement effect is poor. The manufacturing method includes: Step 1, preparing a rotor forging blank; Step 2, using residual heat from forging to complete an isothermal transformation treatment to obtain the rotor forging; Step 3, supercooling and heat preservation treatment; Step 4, medium-temperature heat preservation treatment; Step 5, high-temperature austenitization recrystallization process; the rotor forging after medium-temperature heat preservation treatment is heated to 950℃-1050℃, and then heat-preserved at this temperature to ensure that the entire cross-section of the rotor forging completes austenitization recrystallization; Step 6, annealing treatment to obtain an ultra-supercritical high-temperature rotor. This invention can effectively cut off the microstructure inheritance effect and obtain a better grain refinement effect, with a grain size of 1.5-2 grades.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of large forging manufacturing technology, and particularly relates to a method for manufacturing ultra-supercritical rotor forgings. Background Technology

[0002] Ultra-supercritical thermal power units represent a mature and advanced power generation technology worldwide. Currently, increasingly stringent requirements for improving energy efficiency and controlling environmental pollution are driving the secondary reheat temperature of ultra-supercritical units to rise continuously, placing increasingly demanding requirements on material performance. To adapt to this trend, C630R material has emerged. It is a new type of heat-resistant steel specifically developed for 630℃ secondary reheat ultra-supercritical thermal power units, capable of meeting the stable operation requirements of high-parameter units in high-temperature environments, providing key material support for further performance improvements and compliance with environmental protection and energy efficiency requirements.

[0003] C630R heat-resistant steel is a martensitic heat-resistant steel. Rotor forgings made from this steel have significant drawbacks, including strong stability of supercooled austenite and severe microstructure inheritance. Therefore, to meet subsequent testing standards and practical application requirements, the forged rotor forgings must undergo grain refinement heat treatment.

[0004] The current mainstream heat treatment processes for refining the grain size of this type of rotor mainly include two categories: one is multiple high-temperature austenitizing recrystallization normalizing or annealing treatments, and the other is rapid heating in the critical zone to increase the superheat during high-temperature phase transformation. However, these two processes face significant compatibility challenges when applied to advanced ultra-supercritical rotor forgings made of C630R steel. Due to the extremely high hardenability of this forging and its unusually significant microstructure inheritance effect, traditional processes require long-term, multi-round repeated heating and cooling heat treatments to control the grain size. Not only does the heating and holding time need to be significantly extended to overcome the microstructure inheritance barrier, but the cooling rate also needs to be precisely controlled, resulting in an overall heat treatment cycle that is far longer than that of conventional steel forgings, seriously affecting production efficiency and manufacturing costs. More importantly, even after complex multiple heat treatments, the grain refinement effect is still very limited: the microstructure inheritance phenomenon is difficult to completely eliminate, the grain size uniformity is poor, and grass-like defects frequently appear in subsequent ultrasonic flaw detection. These types of defects can interfere with the interpretation of flaw detection signals, potentially masking dangerous defects such as internal cracks, or leading to misjudgment of qualified forgings, thus posing a hidden danger to the safe operation of the unit. They also restrict the efficient application of C630R steel in high-parameter ultra-supercritical units. Summary of the Invention

[0005] Based on the above analysis, the present invention aims to provide a method for manufacturing ultra-supercritical rotor forgings, in order to solve the technical problem in the prior art that it is difficult to completely eliminate microstructure inheritance and the grain refinement effect is poor when manufacturing ultra-supercritical rotor forgings using C630R heat-resistant steel.

[0006] The objective of this invention is mainly achieved through the following technical solutions: This invention provides a method for manufacturing an ultra-supercritical rotor forging, comprising the following steps: Step 1: Prepare the rotor forging blank; Step 2: Utilize the residual heat from forging to complete the isothermal transformation treatment; Rotor forging blanks with a temperature greater than 850℃ are directly loaded into a waiting furnace with a temperature of 650-750℃ and held for ≥250 hours to obtain rotor forgings. After isothermal transformation treatment, a balanced microstructure of more than 90% ferrite + pearlite is generated. Step 3: Cooling and heat preservation treatment; The rotor forgings, which were subjected to isothermal transformation treatment at 650-750℃, were cooled to 250℃-350℃ and then subjected to supercooling and heat preservation at 250℃-350℃. Step 4: Medium-temperature insulation treatment; The rotor forgings that have undergone supercooling and heat preservation treatment are heated to 600℃-650℃ for medium-temperature heat preservation treatment. Step 5: High-temperature austenitizing recrystallization process; The rotor forgings, after medium-temperature heat treatment, are heated to 950℃-1050℃ and then heat-treated at this temperature to ensure that the entire cross-section of the rotor forgings is austenitized and recrystallized.

[0007] Step 6: Annealing treatment; After high-temperature austenitization recrystallization, the rotor is directly furnace cooled to 150°C or below, and then air-cooled to room temperature. This completes the entire grain refinement heat treatment process and yields an ultra-supercritical high-temperature rotor.

[0008] Furthermore, in step 3, the cooling rate of the rotor forging is 5-20℃ / h.

[0009] Furthermore, in step 3, the cooling rate of the rotor forging is 10-20℃ / h.

[0010] Furthermore, in step 3, the supercooling holding time is designed according to the shaft diameter of the rotor forging, and the holding time is 1-2 hours / 100mm.

[0011] Furthermore, in step 4, when the rotor forging is heated, the heating rate of the rotor forging is 20-50℃ / h.

[0012] Furthermore, in step 4, when the rotor forging is heated, the heating rate of the rotor forging is 30-50℃ / h.

[0013] Furthermore, in step 4, the medium-temperature holding time is designed according to the shaft diameter of the rotor forging, and the medium-temperature holding time is 0.5-1 hour / 100mm.

[0014] Furthermore, in step 5, when the rotor forging is heated, the heating rate is controlled within the range of 30-80℃ / h.

[0015] Furthermore, in step 5, when the rotor forging is heated, the heating rate is controlled within the range of 45-80℃ / h.

[0016] Furthermore, in step 5, the holding time during the high-temperature austenitization recrystallization process is designed according to the shaft diameter of the rotor forging, and the holding time is 1.0-1.5h / 100mm.

[0017] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects: This invention effectively cuts off the hereditary effect of microstructure through the synergistic effect of "isothermal transformation + high-temperature recrystallization", achieving a better grain refinement effect (grain size 1.5-2 grade) and ensuring that the microstructure of the forging meets the strict requirements of ultrasonic testing for microstructure (Φ1.6-Φ2.0 detectable (2MHz)). On the other hand, it makes full use of the residual heat of forging, significantly shortening the heat treatment process (the general heat treatment process cycle is more than 30 days, which can be shortened to about 20 days, saving about 10 days), significantly reducing energy consumption and total production cost; thus achieving a dual improvement in economy and product quality.

[0018] In this invention, the above-described technical solutions can be combined with each other to achieve more preferred combinations. Other features and advantages of this invention will be set forth in the following description, and some advantages may become apparent from the description or be learned by practicing the invention. The objects and other advantages of this invention can be realized and obtained from what is particularly pointed out in the description and drawings. Attached Figure Description

[0019] The accompanying drawings are for illustrative purposes only and are not intended to limit the invention. Throughout the drawings, the same reference numerals denote the same parts.

[0020] Figure 1 This is a schematic diagram of the manufacturing process of the ultra-supercritical high-temperature rotor blank of the present invention; Figure 2 This is a schematic diagram of the rotor forging specifications provided in Embodiment 1 of the present invention; Figure 3 This is a schematic diagram of the microstructure of the rotor forging provided in Embodiment 1 of the present invention; Figure 4 This is a schematic diagram of the rotor forging specifications provided in Embodiment 2 of the present invention; Figure 5 This is a schematic diagram of the microstructure of the rotor forging provided in Embodiment 2 of the present invention; Figure 6 This is a schematic diagram of the rotor forging specifications provided in Embodiment 3 of the present invention; Figure 7 This is a schematic diagram of the microstructure of the rotor forging provided in Embodiment 3 of the present invention. Detailed Implementation

[0021] The preferred embodiments of the present invention will now be described in detail with reference to the accompanying drawings, which constitute a part of the present invention and are used together with the embodiments of the present invention to illustrate the principles of the present invention, but are not intended to limit the scope of the present invention.

[0022] This invention provides a method for manufacturing ultra-supercritical rotor forgings, such as... Figure 1 As shown, it includes the following steps: Step 1: Prepare the rotor forging blank; Step 2: Utilize the residual heat from forging to complete the isothermal transformation treatment; Forging blanks with a temperature greater than 850℃ (e.g., 860℃, 870℃, 900℃) after forging and drawing are directly loaded into a waiting furnace with a temperature of 650-750℃ (e.g., 650℃, 670℃, 700℃, 740℃, 750℃) and held for ≥250h (e.g., 250h, 260h, 370h, 280h, 300h) to obtain rotor forgings.

[0023] Compared with existing technologies, this invention, through precise control of the material temperature and holding time, ensures sufficient holding time to complete the isothermal transformation, thereby obtaining a balanced microstructure composed of ferrite and pearlite. Furthermore, this process directly utilizes the residual heat from forging for the isothermal transformation, eliminating the need for additional heating, significantly shortening the heat treatment cycle and reducing production costs.

[0024] It is important to emphasize that the grain refinement effect of this invention is significantly superior to that of traditional processes. Existing technologies typically involve first cooling the forging blank to a supercooling temperature (150-200°C) to induce a non-equilibrium phase transformation (producing martensite), and then reheating it for austenitic re-crystallization. In contrast, this invention directly transfers the high-temperature forging into the furnace for isothermal transformation, forming a stable equilibrium structure, effectively cutting off the material's microstructure inheritance. In comparison, the continuous cooling in traditional processes produces a non-equilibrium structure (martensite), resulting in severe microstructure inheritance. When reheated to high temperatures, the material easily reverts to its original coarse grain size, leading to a significant reduction in grain refinement.

[0025] Step 3: Insulate against cold; The rotor forgings, after isothermal transformation treatment at temperatures of (e.g., 650℃, 670℃, 700℃, 740℃, 750℃), are cooled to 250℃-350℃ (e.g., 250℃, 270℃, 300℃, 340℃, 350℃) at a cooling rate of 5-20℃ / h (e.g., 5℃ / h, 10℃ / h, 15℃ / h, 18℃ / h, 20℃ / h). They are then subjected to supercooling at 250℃-350℃ (e.g., 250℃, 270℃, 300℃, 340℃, 350℃). The supercooling holding time is designed based on the shaft diameter of the rotor forgings, and is 1-2h / 100mm (e.g., 1h / 100mm, 1.2h / 100mm, 1.5h / 100mm, 1.8h / 100mm, 2h / 100mm).

[0026] For example, if the shaft diameter of the rotor forging is 1000mm, then the holding time is 1000 / 100. (1-2)h, that is, 10-20h.

[0027] In step 3, controlling the supercooling holding temperature and time can accelerate the microstructure transformation process in the core or positive segregation zone of the forging, thereby further improving the grain refinement effect. The mechanism is as follows: after isothermal transformation, a small amount of untransformed retained austenite remains in the core of the forging. During the subsequent supercooling holding process, as the temperature decreases, this retained austenite will further transform into pearlite or martensite, making the microstructure transformation more complete and uniform, thus effectively enhancing the grain refinement effect.

[0028] Compared with the prior art, the present invention controls the cooling rate within the range of 5-20℃ / h. Its main objectives include: on the one hand, the lower cooling rate can effectively reduce the temperature difference between the core and the surface of the rotor forging, thereby significantly reducing the thermal stress level; on the other hand, the reduction of thermal stress helps to reduce the structural stress and cracking tendency of the rotor forging in the low temperature stage, and improve the integrity and pass rate of the forging.

[0029] Preferably, the cooling rate of the rotor forging is 10-20℃ / h (e.g., 10℃ / h, 15℃ / h, 18℃ / h, 20℃ / h).

[0030] Step 4: Medium-temperature insulation treatment; After being cooled and held at room temperature, the rotor forgings are heated to 600℃-650℃ (e.g., 600℃, 620℃, 640℃, 650℃) at a heating rate of 20-50℃ / h (e.g., 20℃, 25℃, 35℃, 45℃, 50℃), and then held at room temperature for 0.5-1h / 100mm (e.g., 0.5h / 100mm, 0.7h / 100mm, 0.9h / 100mm, 1h / 100mm).

[0031] In step 4 above, the purpose of medium-temperature heat preservation is to effectively reduce the temperature difference between the core and surface of the rotor forging by controlling the heating rate and the medium-temperature heat preservation time, thereby reducing thermal stress and reducing the tendency of the rotor forging to crack in subsequent processing.

[0032] In step 4 above, the heating rate of the rotor forging is 35-45℃ / h.

[0033] Step 5: High-temperature austenitizing recrystallization process; The rotor forgings, after medium-temperature heat treatment, are heated to 950℃-1050℃ (e.g., 950℃, 960℃, 1000℃, 1040℃, 1050℃) at a heating rate of 30-80℃ / h (e.g., 30℃ / h, 35℃ / h, 50℃ / h, 75℃ / h, 80℃ / h). At this temperature, the holding time is determined according to 1.0-1.5h / 100mm (e.g., 1.0h / 100mm, 1.2h / 100mm, 1.4h / 100mm, 1.5h / 100mm) to ensure that the entire cross-section of the rotor forgings completes austenitization recrystallization.

[0034] In step 5 above, controlling the heating rate within the range of 30-80℃ / h can improve the heating efficiency of the rotor forging during the high-temperature austenitization transformation and promote the grain refinement effect of the recrystallization process.

[0035] In step 5 above, the holding temperature is controlled within the range of 950℃-1050℃. On the one hand, this ensures that the austenitization transformation is fully completed across the entire cross section of the forging. On the other hand, the grains will not grow rapidly within this temperature range, which is conducive to obtaining fine and uniform austenite grains and laying the microstructure foundation for subsequent cooling transformation.

[0036] Preferably, in step 5 above, the temperature after heating is 960℃-1040℃ (e.g., 960℃, 980℃, 1000℃, 1040℃).

[0037] Step 6: Annealing treatment; After high-temperature austenitization recrystallization, the rotor is directly furnace cooled to 150°C or below, and then air-cooled to room temperature. This completes the entire grain refinement heat treatment process and yields an ultra-supercritical high-temperature rotor.

[0038] It should be noted that the rotor forging of the present invention weighs 10-50t, the shaft diameter (i.e., the maximum diameter) is 500-1400mm, and the forging length is 4000-10000mm.

[0039] In existing technologies, the grain refinement heat treatment for rotor forgings typically involves first cooling the forging blank to a supercooled temperature (150-200℃) to induce a non-equilibrium phase transformation (producing martensite), followed by reheating for austenitic re-crystallization. This process route, due to the continuous cooling that produces a non-equilibrium structure, results in severe microstructure inheritance. When reheated to a high temperature, the material easily reverts to its original coarse grain size, significantly reducing the grain refinement effect. Furthermore, it requires prolonged and repeated heating and cooling cycles, with a heat treatment cycle exceeding 30 days.

[0040] To address the aforementioned issues, this invention employs a "residual heat isothermal transformation + single-stage heating and annealing" method: First, the residual heat from forging (temperature above 850℃ after forging and drawing) is directly utilized to place the forged billet into a waiting furnace at 650-750℃ for holding, completing the isothermal transformation and obtaining an equilibrium microstructure dominated by ferrite and pearlite; Second, the equilibrium microstructure after isothermal transformation is reheated to 950-1050℃ for high-temperature austenitization recrystallization, followed by furnace cooling to complete the annealing process.

[0041] The synergistic mechanism of the above two steps is as follows: After the isothermal transformation, more than 90% of the generated microstructure is a ferrite + pearlite equilibrium microstructure, while the remaining microstructure is completely transformed into martensite in the low-temperature range of 200-250℃. The mixed microstructure composed of the equilibrium microstructure and this martensite microstructure is then heated to a high temperature of 950℃-1050℃, and completely recrystallized into high-temperature austenite. Subsequently, after furnace cooling, it is completely transformed back into martensite. During the recrystallization process, the equilibrium microstructure (ferrite + pearlite), when heated to the austenite region, can effectively sever the hereditary effect of the microstructure and eliminate the inheritance of the original coarse grains, thereby significantly refining the austenite grains after recrystallization, and ultimately refining the martensite microstructure after furnace cooling (e.g., ...). Figure 3 , 5 7).

[0042] If a sufficient equilibrium microstructure (i.e., a ferrite + pearlite ratio below 90%) is not obtained after isothermal transformation, the residual martensite or bainite, or other non-equilibrium microstructures, tend to retain the orientation of the original austenite grains when subsequently heated to the austenite region. This leads to microstructure inheritance, resulting in coarse austenite grains after recrystallization, and consequently, deteriorating the toughness and fatigue resistance of the final material. Therefore, controlling the isothermal transformation process to achieve an equilibrium microstructure ratio of over 90% is a crucial prerequisite for effectively preventing microstructure inheritance and refining grain size.

[0043] This invention achieves two key objectives: firstly, through the synergistic effect of "isothermal transformation + high-temperature recrystallization," it effectively severs the hereditary effect of tissue structure, achieving a superior grain refinement effect in a short time (e.g., Figure 3 , 57) Ensure that the microstructure of the forging meets the strict requirements of ultrasonic flaw detection for microstructure; on the other hand, make full use of the residual heat of forging to significantly shorten the heat treatment process (the general heat treatment process cycle is more than 30 days, but this invention can shorten it to about 20 days, saving about 10 days), significantly reducing energy consumption and total production cost; and taking into account both economic efficiency and product quality improvement.

[0044] It should be noted that in step 1 above, the process of preparing the rotor forging blank includes: Step 11: Prepare the consumable electrode; Prepare raw materials according to the component ratio, melt the raw materials using a vacuum induction melting equipment, and cast the molten steel obtained under inert gas protection to obtain consumable electrodes for electroslag remelting. In step 11 above, vacuum melting is carried out in a ladle refining furnace. The vacuum induction melting temperature is 1600-1700℃ (e.g., 1600℃, 1625℃, 1650℃, 1685℃, 1700℃). The molten steel obtained by melting is protected by an argon atmosphere to avoid secondary oxidation of the molten steel.

[0045] In step 11 above, during casting, a bottom-pouring gating system is used to inject molten steel into a metal mold for casting, thereby obtaining a consumable electrode for electroslag remelting.

[0046] Step 12, electroslag remelting process; The consumable electrode obtained in step 11 is inserted into the slag pool of the electroslag remelting equipment. The slag pool uses a mixed slag system as the molten slag. During the electroslag remelting process, the cooling water volume of the water-cooled crystallizer is dynamically adjusted according to the solidification state of the steel ingot. After the smelting is completed, an electroslag steel ingot is obtained.

[0047] In step 12 above, an electroslag steel ingot obtained by electroslag remelting is used, with a density of 96% to 99.5% (e.g., 96%, 97%, 98.3%, 99%).

[0048] In step 12 above, the aforementioned mixed slag system is a multi-component mixed slag system containing multiple oxides. Compared to binary slag systems or even single-component slag systems, the multi-component mixed slag system, by introducing multiple oxide components, can effectively overcome the contradiction between stability and control precision in the electroslag remelting process of single or binary slag systems, thereby improving the process stability, composition control precision, and surface quality of electroslag steel ingots in the electroslag remelting process.

[0049] Specifically, this invention controls the content of unstable oxides (e.g., SiO2) in the multi-component mixed slag system to a low level (1-5%) to ensure that the slag composition does not change significantly during electroslag remelting, thus guaranteeing the stability of the electroslag remelting process. Furthermore, by regulating the components of the multi-component slag system, easily oxidizable elements in the steel are stabilized, achieving precise control over the electroslag remelting composition. Moreover, the multi-component mixed slag system reduces the melting point and viscosity of the slag: the low melting point and low viscosity of the slag system result in good fluidity, enabling the formation of a uniform thin slag layer, effectively reducing slag groove defects on the ingot surface, thereby improving the surface quality of the final product.

[0050] In step 12 above, the multi-component mixed slag system contains CaF2: 40%-60%, Al2O3: 15%-25%, CaO: 10%-20%, MgO: 1-10%, and SiO2: 1-5%.

[0051] For example, the above-mentioned multi-component mixed slag system contains CaF2: 50%-60%, Al2O3: 18%-22%, CaO: 15%-20%, MgO: 4-9%, and SiO2: 2-4%.

[0052] For example, the above-mentioned multi-element mixed slag system contains CaF2: 55%-60%, Al2O3: 18%-20%, CaO: 15%-18%, MgO: 6-9%, and SiO2: 2-3%.

[0053] For example, the above-mentioned multi-component mixed slag system contains CaF2: 42%, Al2O3: 16%, CaO: 13%, MgO: 4%, and SiO2: 1%.

[0054] For example, the above-mentioned multi-component mixed slag system contains CaF2: 50%, Al2O3: 18%, CaO: 15%, MgO: 8%, and SiO2: 2%.

[0055] For example, the above-mentioned multi-component mixed slag system contains CaF2: 55%, Al2O3: 23%, CaO: 17%, MgO: 9%, and SiO2: 4%.

[0056] In the above-mentioned multi-component mixed slag system, CaF2 can reduce the melting point and viscosity of the slag and adjust its electrical conductivity.

[0057] In the aforementioned multi-component mixed slag system, Al2O3 reduces energy consumption by regulating the efficiency of the electroslag remelting process through adjusting its electrical conductivity.

[0058] In the above-mentioned multi-element mixed slag system, CaO can increase the ability of slag to remove harmful elements P and S, and controlling its content within the above range can improve the purity of the ingot metal.

[0059] In the above-mentioned multi-component mixed slag system, MgO can form a semi-solidified film on the surface of the slag pool; controlling its content within the above range can prevent hydrogen absorption by the ingot and reduce heat loss from the slag surface.

[0060] In the aforementioned multi-element mixed slag system, SiO2 is used to lower the melting point of the slag and improve its high-temperature plasticity. By controlling the SiO2 content at a low level, the effects of lowering the melting point of the slag and improving its high-temperature plasticity can be achieved without increasing the oxygen activity of the slag system due to excessive content. This avoids the oxidation and burning of easily oxidized elements in the molten steel, thus ensuring the compositional stability of the electroslag ingot.

[0061] In step 12 above, the oxygen content in the atmosphere inside the electroslag remelting equipment is ≤0.005% (e.g., oxygen content of 0.001%, 0.002%, or 0.005%). Controlling the oxygen content within this range can effectively reduce the risk of steel molten metal oxidation during the melting of consumable electrodes, prevent the loss of alloying elements, especially easily oxidized elements such as B and Al, ensure the accuracy of the composition of the finished steel ingot, and also reduce the formation of oxide inclusions, thereby improving the internal purity of the electroslag steel ingot.

[0062] In step 12 above, the voltage during the electroslag remelting process is controlled to be 60-110V (e.g., 60V, 62V, 75V, 85V, 93V, 105V, 110V).

[0063] By controlling the electroslag remelting voltage within the aforementioned range, the voltage is primarily used to adjust the depth of the consumable electrode insertion into the slag pool and maintain stable slag pool resistance. Maintaining a constant voltage ensures that the electrode spacing (i.e., the distance from the end of the consumable electrode to the surface of the molten metal pool) remains unchanged, thereby achieving stable slag resistance and molten pool shape, thus guaranteeing the solidification quality of the electroslag steel ingot. If the voltage is below 60V, the slag pool resistance is too high, the consumable electrode is inserted too deeply, easily leading to uneven overheating of the molten pool and affecting the surface quality of the steel ingot. If the voltage is above 110V, the slag pool resistance is too low, the consumable electrode is inserted too shallowly, and the molten pool temperature is too low, which is detrimental to the thorough refining and sequential solidification of the molten steel. Controlling the voltage within the aforementioned range balances smelting efficiency and steel ingot quality, ensuring the stability and controllability of the electroslag remelting process.

[0064] In step 12 above, the current during the electroslag remelting process is controlled to be 30kA to 60kA (e.g., 30kA, 32kA, 44kA, 50kA, 58kA, 60kA).

[0065] Compared with existing technologies, this invention controls the current within the aforementioned range, which not only improves the melting rate of the consumable electrode, but also, the strong electromagnetic force generated by the larger current creates a vigorous stirring effect on the slag pool, which is beneficial to improving the metallurgical reaction kinetics at the slag-metal interface, promoting the removal of inclusions and the homogenization of composition. If the current is below 30kA, Joule heating is insufficient, the melting rate of the consumable electrode is low, the melting cycle is prolonged, and the electromagnetic stirring force is weakened, which is not conducive to the full progress of the metallurgical reaction. If the current is above 60kA, the molten pool is overheated and the slag temperature is too high, which can easily lead to increased component segregation and deterioration of surface quality in the electroslag remelting ingot. Controlling the current within this range can balance melting efficiency and electroslag ingot quality, ensuring the stability and controllability of the electroslag remelting process.

[0066] In step 12 above, the melting rate of the consumable electrode is 5 to 30 kg / min (e.g., 5 kg / min, 8 kg / min, 12 kg / min, 18 kg / min, 24 kg / min, 30 kg / min).

[0067] Compared with existing technologies, this invention, by precisely controlling the melting rate within a certain range, enables the molten pool shape to remain stable, thereby obtaining a uniform solidification structure. A stable molten pool shape helps reduce component segregation, improves the internal density of the steel ingot, and enhances surface quality.

[0068] In step 12 above, the insertion depth of the consumable electrode is 7 to 15 mm (e.g., 7 mm, 9 mm, 12 mm, 14 mm, 15 mm).

[0069] It should be noted that controlling the insertion depth of the consumable electrode within the range of 7–15 mm ensures a good match between the slag pool resistance and the power supply parameters, maintains a stable slag temperature and smelting process, and is beneficial to ensuring the solidification quality of the steel ingot. If the consumable electrode is inserted too shallowly (less than 7 mm), the slag pool resistance will be too high, which can easily generate an open arc between the consumable electrode and the slag surface, leading to current fluctuations and instability in the smelting process. If the consumable electrode is inserted too deeply (more than 15 mm), the slag pool resistance will be too low, the current will easily become uncontrollable, the slag temperature will rise abnormally, and it may cause component segregation in the steel ingot.

[0070] In step 12 above, the slag pool temperature is 1580-1680℃ (e.g., 1580℃, 1590℃, 1620℃, 1650℃, 1680℃). Controlling the slag pool temperature within this range can ensure the fluidity of the molten slag and remove inclusions.

[0071] Step 13: Forging and shaping; Electroslag steel ingots are heated to 1150-1200℃ (e.g., 1150℃, 1165℃, 1185℃, 1200℃) at a heating rate of 50-80℃ / h (e.g., 50℃ / h, 60℃ / h, 70℃ / h, 80℃ / h), and held at that temperature for 30-50h (e.g., 30h, 35h, 45h, 50h). Then, the finished product is drawn out according to the step dimensions of the forging blank drawing using an upper flat and lower V-shaped anvil on a hydraulic press of 8000 tons or more (e.g., 8000 tons, 9000 tons, 10000 tons). The forging ratio is 1.4-2 (e.g., 1.4, 1.6, 1.7, 1.9, 2.0), resulting in an ultra-supercritical high-temperature rotor blank.

[0072] In step 13 above, the present invention controls the heating rate of the electroslag steel ingot within the range of 50-80℃ / h, which can reduce the internal and external temperature difference of the electroslag steel ingot and prevent the electroslag steel ingot from cracking or expanding internal defects during the heating process.

[0073] In step 13 above, the present invention controls the temperature of the electroslag steel ingot within the range of 1150-1200℃. The purpose is to reduce the material's resistance to deformation, reduce the load requirements on the equipment during forging deformation, and facilitate deformation during the forging process.

[0074] Furthermore, by strictly controlling the forging ratio within the range of 1.4-2, this invention can ensure that the rotor forgings have a regular shape and uniform machining allowance, while also minimizing forging defects such as folds and cracks.

[0075] It should be emphasized that the purpose of the forging process described above in this invention is to forge the dimensions of each step of the ultra-supercritical rotor, which is different from the function of traditional forging center compaction and defect elimination.

[0076] When using heat-resistant steel to manufacture ultra-supercritical rotor forgings, it is difficult to completely eliminate the inherited microstructure and the grain refinement effect is poor.

[0077] The ultra-supercritical high-temperature rotor of the present invention comprises the following components by weight percentage: C: 0.09-0.15%, Mn: 0.38-0.62%, P: ≤0.015%, S: ≤0.007%, Si: ≤0.08%, Ni: ≤0.05%, Cr: 8.75-9.35%, Mo: 0.32-0.52%, V: 0.18-0.22%, W: 1.92-2%. 48%, Co: 2.75-3.25%, Nb: 0.04-0.075%, N: 0.006-0.010%, B: 0.012-0.018%, Zr: 0.01-0.02%, Al: ≤0.010%, Cu: ≤0.10%, Sb: ≤0.0015%, Sn: ≤0.010%, As: ≤0.015%, balance being Fe and unavoidable impurities.

[0078] The functions of each component in the above-mentioned ultra-supercritical high-temperature rotor blank are as follows: C: The C element mainly plays a precipitation strengthening role by forming carbides. The C element content is strictly controlled within the above range in order to avoid problems such as insufficient material strength or embrittlement.

[0079] Cr: Cr is used to form a reinforcing phase and improve the high-temperature oxidation resistance of materials. Controlling its content within the above range can prevent the decline in corrosion resistance or the formation of brittle phases.

[0080] Fe: As a matrix component, Fe can provide basic structural strength for materials.

[0081] Mo, W, and Co are all high-temperature strengthening elements. Mo and W can both dissolve into the iron matrix, thereby achieving composite solid solution strengthening and improving creep resistance. Controlling the content of both within the above range can prevent insufficient material strength or precipitation of brittle phases.

[0082] Co: Co can suppress brittle phases and improve tissue stability.

[0083] V, Nb, and N and B are all grain and grain boundary strengthening elements. Among them, V, Nb and N form fine MX phases, which pin grain boundaries and refine grains.

[0084] B: B element segregates at grain boundaries, which can improve the long-term plasticity of materials. Controlling its content within the above range can prevent insufficient grain boundary strengthening or hot brittleness of materials.

[0085] Si and Mn are used for deoxidation and quality improvement, while Ni is used to improve low-temperature toughness. P and S are harmful impurities, and their contents are strictly controlled within the above range to prevent grain boundary embrittlement and thermal cracking of materials.

[0086] The synergistic effects among the above components include: (1) Synergistic effect of C-Cr-Mo-W elements: C, Cr, Mo, and W form a composite system of intragranular solid solution strengthening and grain boundary precipitation strengthening through a synergistic effect to ensure the high-temperature strength of the material. Among them, C is the core element, which combines with Cr, Mo, and W to form M x C-composite carbides. Within the crystal, the solid-dissolved Cr, Mo, W, and interstitial C atoms induce multiple lattice distortions, hindering dislocation movement and providing matrix strength; simultaneously, the dispersed precipitated nanoscale M... x C particles play a precipitation strengthening role, further enhancing resistance to deformation. At grain boundaries, M... xC carbides are distributed in granular or chain-like forms, producing a pinning effect that effectively inhibits grain boundary slip and migration, hindering crack propagation. Furthermore, Cr ensures corrosion resistance, while Mo and W work synergistically to guarantee the long-term stability of the microstructure at high temperatures.

[0087] (2) Synergistic effect of V-Nb-N elements: V, Nb and N form a triple composite strengthening mechanism of solid solution strengthening, fine grain strengthening and MX phase precipitation strengthening through synergistic effect, which comprehensively improves the strength, toughness and high temperature structure stability of the material (at room temperature, the tensile strength of the material is ≥800MPa, the impact toughness is ≥8.1J, and the fracture time is ≥100h at 650℃ and 171MPa).

[0088] Specifically, nitrogen (N) combines with v and Nb to form stable MX-type carbonitrides, with N being the core component of this precipitated phase. At high temperatures, Nb preferentially precipitates fine MX phases, effectively pinning grain boundaries and inhibiting recrystallization and grain coarsening, achieving high-temperature fine-grain strengthening. V disperses and precipitates nanoscale MX phases in the mid-temperature range, providing strong precipitation strengthening. Simultaneously, some V, Nb, and interstitial N atoms dissolved in the matrix undergo lattice distortion, contributing significantly to solid solution strengthening. Furthermore, V and Nb mutually promote precipitation (e.g., Nb(CN) provides heterogeneous nucleation sites for V(CN)) and synergistically inhibit grain growth, thereby significantly optimizing the material's creep resistance and high-temperature service life (fracture time ≥10000h at 630℃ and 135MPa).

[0089] (3) Synergistic effect of B-Co elements: Through the synergistic effect of matrix solid solution strengthening and grain boundary cohesive strengthening, the stability of the material during long-term high-temperature service is ensured. Among them, Co stabilizes the austenitic matrix through solid solution strengthening, improving the matrix toughness and creep resistance; B segregates at grain boundaries, enhancing grain boundary bonding, inhibiting grain boundary diffusion and weakening, and delaying grain boundary void nucleation. The two work together to achieve the coupling effect of "matrix strengthening + grain boundary strengthening + microstructure stabilization", significantly improving the creep strength and thermal stability of high-temperature alloys.

[0090] (4) Synergistic effect of Cr-Si elements: By forming a double-layer composite oxide film, the material's resistance to steam oxidation is significantly improved. Among them, Cr is the main film-forming element, forming a dense Cr2O3 oxide film on the outer layer and providing solid solution reinforcement to the matrix; Si is enriched in the inner layer and forms a SiO2 isolation band, filling the microcracks and defects in the oxide film, improving the density and adhesion of the oxide film, and effectively blocking oxygen diffusion inward. The two elements synergistically optimize the composite anti-oxidation performance, significantly improving the material's high-temperature corrosion resistance and the structural stability of the surface oxide layer.

[0091] Preferably, the ultra-supercritical high-temperature rotor of the present invention comprises the following components by weight percentage: C: 0.09-0.15%, Mn: 0.38-0.62%, P: ≤0.015%, S: ≤0.007%, Si: ≤0.08%, Ni: ≤0.05%, Cr: 9-12%, Mo: 0.32-0.52%, V: 0.18-0.22%, W: 1.92-2.48%, Co: 2.75-3.25%, Nb: 0.04-0.075%, N: 0.006-0.010%, B: 0.012-0.018%, Zr: 0.01-0.02%, Al: ≤0.010%, Cu: ≤0.10%, Sb: ≤0.0015%, Sn: ≤0.010%, As: ≤0.015%, with the balance being Fe and unavoidable impurities.

[0092] For example, the chemical composition of the ultra-supercritical high-temperature rotor of the present invention, by weight percentage, includes: C: 0.11%, Mn: 0.5%, P: 0.008%, S: 0.003%, Si: 0.05%, Ni: 0.02%, Cr: 9.2%, Mo: 0.42%, V: 0.2%, W: 2.18%, Co: 2.98%, Nb: 0.058%, N: 0.008%, B: 0.015%, Zr: 0.015%, with the balance being Fe and unavoidable impurities.

[0093] For example, the chemical composition of the ultra-supercritical high-temperature rotor of the present invention, by weight percentage, includes: C: 0.12%, Mn: 0.52%, P: 0.009%, S: 0.004%, Si: 0.06%, Ni: 0.03%, Cr: 10%, Mo: 0.4%, V: 0.21%, W: 2.25%, Co: 3.05%, Nb: 0.062%, N: 0.008%, B: 0.016%, Zr: 0.016%, Al: 0.006%, Cu: 0.06%, Sb: 0.0009%, Sn: 0.006%, As: 0.009%, with the balance being Fe and unavoidable impurities.

[0094] For example, the chemical composition of the ultra-supercritical high-temperature rotor of the present invention, by weight percentage, includes: C: 0.13%, Mn: 0.55%, P: 0.01%, S: 0.004%, Si: 0.07%, Ni: 0.04%, Cr: 11.5%, Mo: 0.45%, V: 0.21%, W: 2.3%, Co: 3.10%, Nb: 0.065%, N: 0.009%, B: 0.016%, Zr: 0.017%, Al: 0.007%, Cu: 0.07%, Sb: 0.001%, Sn: 0.007%, As: 0.010%, with the balance being Fe and unavoidable impurities.

[0095] This invention achieves high strength performance at 630℃ (tensile strength ≥800MPa, impact toughness ≥8.1J, and fracture time ≥100h at 650℃ and 171MPa) by precisely controlling the content of each element, suppressing the precipitation of harmful brittle phases, ensuring the stability of rotor heat treatment and forging processes, and supporting the efficient, long-life, and safe operation of the unit.

[0096] The rotor blank manufacturing method provided in step 1 of this invention can replace the key forging and compaction process in the traditional method with the electroslag remelting process, retaining only one forging and forming process, significantly shortening the manufacturing process. Furthermore, by reducing the energy-intensive compaction step, energy input can be reduced, while the simplified process reduces labor and equipment costs, resulting in significant cost and energy savings. Moreover, by utilizing the inherent characteristics of electroslag remelted steel ingots—density, few defects, and fine grains—the ultrasonic flaw detection quality of the rotor forging core can be ensured in advance, eliminating the need for subsequent forging to compensate, achieving a breakthrough in both economy and quality, and is suitable for manufacturing large high-temperature rotor forgings weighing 10-50 tons.

[0097] Examples 1-3 Examples 1-3 are all carried out according to the following manufacturing method for ultra-supercritical high-temperature rotor blanks, specifically including the following steps: Step 1: Prepare the consumable electrode; Prepare raw materials according to the component ratio, and melt the raw materials using vacuum induction melting equipment. The vacuum induction melting temperature is 1600-1700℃. The molten steel obtained from the melting is cast under the protection of inert gas. During casting, a bottom-pouring casting system is used to inject the molten steel into the metal mold for casting, and the self-consumable electrode for electroslag remelting is obtained.

[0098] Step 2, electroslag remelting process; The consumable electrode obtained in step 1 is inserted into the slag pool of the electroslag remelting equipment. The slag pool uses a mixed slag system as the molten slag. During the electroslag remelting process, the cooling water volume of the water-cooled crystallizer is dynamically adjusted according to the solidification state of the steel ingot. After the smelting is completed, an electroslag steel ingot is obtained.

[0099] In step 2 above, the electroslag steel ingot obtained by electroslag remelting has a density of 96% to 99.5%.

[0100] In step 2 above, the multi-component mixed slag system contains CaF2: 40%-60%, Al2O3: 15%-25%, CaO: 10%-20%, MgO: 1-10%, and SiO2: 1-5%.

[0101] Preferably, the multi-component mixed slag system comprises CaF2: 50%, Al2O3: 15%, CaO: 15%, MgO: 8%, and SiO2: 2%.

[0102] In step 2 above, the oxygen content in the atmosphere inside the electroslag remelting equipment is ≤0.005%.

[0103] In step 2 above, the voltage during the electroslag remelting process is controlled at 60–110V.

[0104] In step 2 above, the current during the electroslag remelting process is controlled at 30kA to 60kA.

[0105] In step 2 above, the melting rate of the consumable electrode is 5 to 30 kg / min.

[0106] In step 2 above, the insertion depth of the consumable electrode is 7-15 mm.

[0107] In step 2 above, the slag pool temperature is 1580-1680℃. Controlling the slag pool temperature within this range can ensure the fluidity of the molten slag and remove inclusions.

[0108] Step 3: Forging and shaping; The electroslag steel ingot is heated to 1150-1200℃ at a heating rate of 50-80℃ / h and held for 30-50 hours. Then, the finished product is drawn out according to the dimensions of each step of the forging blank drawing on a hydraulic press of more than 8000 tons using an upper flat and lower V anvil. The forging ratio is 1.4-2, thus obtaining an ultra-supercritical high-temperature rotor blank.

[0109] Step 4: Post-processing of ultra-supercritical high-temperature rotor blank.

[0110] Step 41: Use the residual heat from forging to complete the isothermal transformation treatment; The forged blank, after being drawn and elongated to a temperature exceeding 850℃, is directly placed into a waiting furnace at 650-750℃ and held for ≥250 hours to obtain the rotor forging. By precisely controlling the waiting temperature and holding time, sufficient holding time can be ensured to complete the isothermal transformation, thereby obtaining a balanced microstructure composed of ferrite and pearlite. Simultaneously, utilizing the residual heat from forging for the isothermal transformation eliminates the need for additional heating, significantly shortening the heat treatment cycle and reducing production costs.

[0111] Step 42: Insulation against cold; The rotor forgings, which were subjected to isothermal transformation treatment at a temperature of 650-750℃, were cooled to 250℃-350℃ at a rate of 5-20℃ / h, and then subjected to supercooling and heat preservation at 250℃-350℃ for a time t of 1-2 hours / 100mm.

[0112] For example, if the shaft diameter of the rotor forging is 1000mm, the holding time t is 10-20h.

[0113] Step 43: Medium-temperature insulation treatment; After being cooled and held at room temperature, the rotor forgings are heated to 600℃-650℃ at a rate of 20-50℃ / h and held at medium temperature for 0.5-1 hour / 100mm.

[0114] Step 44: High-temperature austenitizing recrystallization process; The rotor forgings after medium-temperature heat treatment are heated to 950℃-1050℃ at a heating rate of 30-80℃ / h, and the heat treatment time is determined according to 1.0-1.5h / 100mm to ensure that the entire cross section of the rotor forgings completes austenitization recrystallization.

[0115] Step 45: Annealing treatment; After high-temperature austenitization recrystallization, the rotor is directly furnace-cooled to 150°C, and then air-cooled after being removed from the furnace. This completes the entire grain refinement heat treatment process, resulting in an ultra-supercritical high-temperature rotor.

[0116] It should be noted that three sets were prepared in each of Examples 1-3, that is, three rotor blanks were prepared under the same preparation conditions in each example.

[0117] The specific implementation conditions for Examples 1-3 are shown in Table 1 below: Table 1 Specific implementation conditions for Examples 1-3

[0118] It should be noted that the specifications of the rotor forging prepared in Example 1 are as follows: the forging length is 6380mm, of which the shaft body length is 3780mm and the shaft body diameter is 860mm; the shaft diameter at one end is 760mm and the length is 500mm; the shaft diameter at the other end is 660mm and the length is 2100mm, as shown below. Figure 2 As shown; the product's structure is as follows Figure 3 As shown.

[0119] Upon testing, the chemical composition of the ultra-supercritical high-temperature rotor prepared in Example 1, by weight percentage, includes the following components: C: 0.11%, Mn: 0.5%, P: 0.008%, S: 0.003%, Si: 0.05%, Ni: 0.02%, Cr: 9.2%, Mo: 0.42%, V: 0.2%, W: 2.18%, Co: 2.98%, Nb: 0.058%, N: 0.008%, B: 0.015%, Zr: 0.015%, Al: 0.005%, Cu: 0.05%, Sb: 0.0008%, Sn: 0.006%, As: 0.008%, with the balance being Fe and unavoidable impurities.

[0120] The rotor forging prepared in Example 2 has the following specifications: the forging length is 8500mm, of which the shaft body length is 4755mm and the shaft body diameter is 940mm; the shaft diameter at one end is 820mm and the length is 905mm, with a corresponding flange diameter of 960mm and a flange length of 560mm; the shaft diameter at the other end is 680mm and the length is 1780mm, with a corresponding flange diameter of 1100mm and a length of 500mm. Figure 4 As shown; the product's structure is as follows Figure 5 As shown.

[0121] Upon testing, the chemical composition of the ultra-supercritical high-temperature rotor prepared in Example 2, by weight percentage, includes: C: 0.12%, Mn: 0.52%, P: 0.009%, S: 0.004%, Si: 0.06%, Ni: 0.03%, Cr: 10.0%, Mo: 0.4%, V: 0.21%, W: 2.25%, Co: 3.05%, Nb: 0.062%, N: 0.008%, B: 0.016%, Zr: 0.016%, Al: 0.006%, Cu: 0.06%, Sb: 0.0009%, Sn: 0.006%, As: 0.009%, with the balance being Fe and unavoidable impurities.

[0122] The rotor forging prepared in Example 3 has the following specifications: the forging length is 8293 mm, of which the shaft body length is 4672 mm and the shaft body diameter is 1060 mm; the shaft diameter at one end is 573 mm and the length is 905 mm, with a corresponding flange diameter of 388 mm and a flange length of 436 mm; the shaft diameter at the other end is 680 mm and the length is 1780 mm, with a corresponding flange diameter of 1100 mm and a length of 500 mm. Figure 6 As shown; the product's structure is as follows Figure 7 As shown.

[0123] According to the test results, the chemical composition of the ultra-supercritical high-temperature rotor prepared in Example 3, by weight percentage, includes: C: 0.13%, Mn: 0.55%, P: 0.01%, S: 0.004%, Si: 0.07%, Ni: 0.04%, Cr: 11.5%, Mo: 0.45%, V: 0.21%, W: 2.3%, Co: 3.10%, Nb: 0.065%, N: 0.009%, B: 0.016%, Zr: 0.017%, Al: 0.007%, Cu: 0.07%, Sb: 0.001%, Sn: 0.007%, As: 0.010%, with the balance being Fe and unavoidable impurities.

[0124] Table 2 Mechanical and high-temperature properties of products from Examples 1-3

[0125] As can be seen from the data in Table 2 above, three rotor forgings were prepared in each of Examples 1 to 3 of the present invention. Their mechanical property data are shown in Table 2. All mechanical properties and high-temperature performance indicators meet the design and acceptance requirements. The yield strength is 665-690 MPa, the tensile strength is 805-830 MPa, the elongation is 16.5-18%, and the reduction of area is 60-65%. For fatigue resistance and room temperature impact toughness, one set of rotor forgings was selected for testing in each example. The test results are shown in Table 2 above: strain ±0.5% at 620℃, number of cycles Nf≥1800; room temperature impact toughness is 8.3-8.6 J, which proves the stability and reliability of the preparation method of the present invention.

[0126] In summary, this invention utilizes the dense, defect-free, and fine-grained characteristics of electroslag remelted steel ingots to replace the traditional multi-stage forging and compaction process, retaining only the forging and forming process. This ensures the quality of ultrasonic testing of the rotor forging core in advance, eliminating the need for subsequent forging to compensate for defects. It effectively improves the problems of high energy consumption and long process in traditional processes, shortens the manufacturing process, reduces energy consumption and costs, and ensures that the rotor forging meets the requirements for microstructure testing, achieving a breakthrough in both economy and quality.

[0127] Comparative Example 1 The forging and compaction process of existing ultra-supercritical rotor forgings, as used in the comparative example, is as follows: Step 1, First firing, press the jaws; Heat the billet to 1150-1200℃ and hold for 50 hours. Use an upper flat and lower V-shaped anvil to press out jaws on the riser end of the steel ingot.

[0128] Step 2, second firing, roughing; The billet is heated to 1150-1200℃ and held for 45 hours. Upsetting is performed using a spherical upsetting plate and an upsetting stencil. The forging ratio is 1.5-2.

[0129] Step 3, third firing, stretching; The billet is heated to 1180-1200℃ and held for 30 hours, then drawn using upper and lower V-shaped anvils. The forging ratio is 1.8-2.

[0130] Step 4, fourth firing, roughing; The forging is heated to 1150-1200℃ and held for 45 hours, then upset using a spherical upsetting plate and an upsetting stencil. The forging ratio is 1.5-2.

[0131] Step 5, fifth firing, stretching; Heat to 1150-1200℃, hold for 30 hours, and draw using upper and lower V-shaped anvils, with a forging ratio of 2-2.4.

[0132] Step 6, sixth firing, finished product; Lengthening is achieved using an anvil with a flat top and a V-shaped bottom.

[0133] A comparison of Comparative Example 1 and Example 1 of this application shows that conventional forging methods require at least six repeated heating, upsetting, and drawing processes to complete the blank forming, resulting in a long total manufacturing cycle and high overall energy consumption, significantly increasing production time and energy costs. In contrast, this invention requires only one heating and forging process, effectively reducing production costs while shortening the manufacturing process. Furthermore, the core flaw detection results of the rotor blank prepared by this invention fully meet the standard requirements, and its mechanical properties are comparable to those of products prepared by conventional multi-heat forging methods, with superior grain uniformity, fully verifying the reliability of the manufacturing method of this invention.

[0134] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention should be included within the scope of protection of the present invention.

Claims

1. A method for manufacturing an ultra-supercritical rotor forging, characterized in that, Includes the following steps: Step 1: Prepare the rotor forging blank; Step 2: Utilize the residual heat from forging to complete the isothermal transformation treatment; Rotor forging blanks with a temperature greater than 850℃ are directly loaded into a waiting furnace with a temperature of 650-750℃ and held for ≥250 hours to obtain rotor forgings. Step 3: Cooling and heat preservation treatment; The rotor forgings, which were subjected to isothermal transformation treatment at 650-750℃, were cooled to 250℃-350℃ and then subjected to supercooling and heat preservation at 250℃-350℃. Step 4: Medium-temperature insulation treatment; The rotor forgings that have undergone supercooling and heat preservation treatment are heated to 600℃-650℃ for medium-temperature heat preservation treatment. Step 5: High-temperature austenitizing recrystallization process; The rotor forgings, after medium-temperature heat treatment, are heated to 950℃-1050℃ and then heat-treated at this temperature to ensure that the entire cross-section of the rotor forgings is austenitized and recrystallized. Step 6: Annealing treatment; After high-temperature austenitization recrystallization, the rotor is directly furnace cooled to 150°C or below, and then air-cooled to room temperature. This completes the entire grain refinement heat treatment process and yields an ultra-supercritical high-temperature rotor.

2. The method for manufacturing an ultra-supercritical rotor forging according to claim 1, characterized in that, In step 3, the cooling rate of the rotor forging is 5-20℃ / h.

3. The method for manufacturing an ultra-supercritical rotor forging according to claim 2, characterized in that, In step 3, the cooling rate of the rotor forging is 10-20℃ / h.

4. The method for manufacturing an ultra-supercritical rotor forging according to claim 3, characterized in that, In step 3, the supercooling holding time is designed according to the shaft diameter of the rotor forging, and the holding time is 1-2 hours / 100mm.

5. The method for manufacturing an ultra-supercritical rotor forging according to claim 1, characterized in that, In step 4, when the rotor forging is heated, the heating rate of the rotor forging is 20-50℃ / h.

6. The method for manufacturing an ultra-supercritical rotor forging according to claim 5, characterized in that, In step 4, when the rotor forging is heated, the heating rate of the rotor forging is 30-50℃ / h.

7. The method for manufacturing an ultra-supercritical rotor forging according to claim 1, characterized in that, In step 4, the medium-temperature holding time is designed according to the shaft diameter of the rotor forging, and the medium-temperature holding time is 0.5-1 hour / 100mm.

8. The method for manufacturing an ultra-supercritical rotor forging according to claim 1, characterized in that, In step 5, the heating rate of the rotor forging is controlled within the range of 30-80℃ / h.

9. The method for manufacturing an ultra-supercritical rotor forging according to claim 8, characterized in that, In step 5, the heating rate of the rotor forging is controlled within the range of 45-80℃ / h.

10. The method for manufacturing an ultra-supercritical rotor forging according to claim 1, characterized in that, In step 5, the holding time during the high-temperature austenitization recrystallization process is designed according to the shaft diameter of the rotor forging, and the holding time is 1.0-1.5h / 100mm.