A composite refinement method for nickel-based alloy castings

By combining rare earth element pretreatment with core-shell structure refiners, the problems of internal purity and grain refinement in nickel-based alloy castings were solved, achieving a synergistic improvement in high purity and fine grains, thus enhancing the overall performance of nickel-based alloy castings.

CN123063640APending Publication Date: 2026-11-10TYCON ALLOY IND (ZHONGSHAN) CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611342474.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-01
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing grain refinement technologies for nickel-based alloy castings suffer from limitations such as the limited effectiveness of single grain refiners, the tendency for overall refinement to introduce inclusions, and the inability of surface refinement to improve internal purity.

Method used

Rare earth element pretreatment combined with a core-shell structure refiner is employed. Rare earth oxides in the melt generate nucleation cores and cobalt aluminate and lanthanum hexaboride in the shell surface layer to generate Co particles and [B] atoms, achieving synergistic refinement both internally and externally. This is combined with low-temperature annealing.

Benefits of technology

It achieves high purity and fine grain refinement of nickel-based alloy castings, improves tensile strength, yield strength and elongation, and significantly enhances overall performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This invention relates to a composite grain refinement method for nickel-based alloy castings, belonging to the technical field of nickel-based alloy castings. In this invention, rare earth elements yttrium and cerium are added to the melt during the later stages of vacuum melting of the nickel-based alloy, while argon gas is blown in for refining. Cobalt aluminate is added to the shell coating to coat lanthanum hexaboride; during shell firing, the cobalt aluminate shell protects the lanthanum hexaboride from oxidation; during casting, Co particles are generated as heterogeneous nucleation cores, releasing [B] atoms to pin grain boundaries. The rare earth treatment and the core-shell particles work synergistically to provide nucleation cores both inside the melt and at the mold wall interface, achieving both high purity and grain refinement. The overall performance of nickel-based alloy castings prepared using this method is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of nickel-based alloy casting technology, and relates to a composite refinement method for nickel-based alloy castings. Background Technology

[0002] Nickel-based alloys, due to their excellent high-temperature strength, corrosion resistance, and oxidation resistance, are widely used in key pump and valve components in aero-engines, ships, chemical industries, and nuclear industries. As industrial equipment develops towards higher performance and longer service life, the requirements for the mechanical properties and reliability of nickel-based alloy castings are increasing. Refining the grain structure is an effective way to improve the mechanical properties of castings; grain refinement can increase strength, enhance toughness, improve thermal fatigue performance, and reduce susceptibility to hot cracking.

[0003] Currently, grain refinement technologies for precision casting of nickel-based superalloys mainly include mechanical methods, thermal control methods, and chemical methods. Among these, chemical methods refine grains by adding heterogeneous nucleating agents to increase the crystallization nuclei during solidification of the liquid metal. This can be divided into surface refinement and overall refinement. Overall refinement involves adding a refiner to the melt after the superalloy has melted. However, the added nucleating agent easily forms oxide inclusions in the melt, becoming fatigue sources, making process control difficult. Surface refinement, on the other hand, involves coating the mold surface with a refiner to refine the surface grains of the casting. This process is simple and less prone to introducing inclusions.

[0004] In the field of shell surface layer refinement technology, various refining agents have been reported in studies. For example, the research and application of cobalt aluminate grain refiner for K418 high-temperature alloy showed that the grain size grade could be improved by more than 100% after using the cobalt aluminate refiner. Patent CN110976773A discloses that adding cobalt chlorate refiner (3-8%) to the shell surface layer slurry can make the grain size of the casting five to six times finer than that of normal casting. CN115069979A uses a mixture of cobalt aluminate refiner and silica sol to form a slurry and coat it on the core surface to inhibit the growth of columnar crystals on the inner surface of equiaxed hollow turbine blades.

[0005] Although the above technologies have achieved certain results in refining the grain size of nickel-based alloys, they still have the following shortcomings: (1) Existing technologies mostly use a single refining agent (such as cobalt aluminate, cobalt chlorate or nano NiAlTi), which only relies on increasing the nucleation core to achieve grain refinement, and lacks the synergistic effect of multiple mechanisms. (2) In the overall refining technology, the refining agent is prone to forming oxide inclusions, while the surface refining technology cannot improve the purity inside the melt, making it difficult to achieve high purity and fine grain size at the same time. Summary of the Invention

[0006] The purpose of this invention is to provide a composite grain refinement method for nickel-based alloy castings, which aims to achieve a synergistic improvement in the internal purity and surface grain refinement of nickel-based alloy castings through the synergistic effect of melt rare earth pretreatment and shell surface refiner.

[0007] The objective of this invention can be achieved through the following technical solutions: This invention provides a composite refining method for nickel-based alloy castings, comprising the following steps: (1) Rare earth pretreatment of melt: Nickel-based alloy raw materials are added to a vacuum induction furnace for melting. In the later stage of melting, rare earth elements yttrium (Y) and cerium (Ce) are added to the melt, and inert gas argon is blown in for refining. The temperature of the resulting melt is reduced to 1450-1490℃ to obtain the casting melt.

[0008] On the one hand, the microbubbles generated by bottom-blown argon can adsorb and carry non-metallic inclusions in the melt to the surface for removal during the upward movement. On the other hand, the addition of rare earth elements to the melt causes them to react with residual oxygen, generating high-melting-point rare earth oxides (such as Ce₂O₃ and Y₂O₃) in situ. These oxides can adhere to and encapsulate sharp inclusions such as Al₂O₃, forming composite nucleation cores with good lattice matching, thereby promoting heterogeneous nucleation and refining grains during alloy solidification. The study "The Influence of Ce on the Solidification Microstructure of Fe-Ni Expansion Alloys" indicates that rare earth oxides have low mismatch with the nickel-based alloy matrix on certain low-index planes, making them effective substrates for heterogeneous nucleation.

[0009] Preferably, the nickel-based alloy comprises, by mass percentage: Cr 21.0-22.5%, Mo 12.5-13.5%, Fe 3.0-5.0%, W 2.5-3.5%, with the balance being Ni.

[0010] Preferably, the rare earth elements are yttrium (Y) and cerium (Ce), and the amount of rare earth elements added is 0.05-0.15% of the melt mass.

[0011] Preferably, the argon flow rate is 1.0-2.0 L / min, and the argon blowing time is 20-30 minutes.

[0012] (2) Shell preparation and refining agent addition: The specific operation process for shell preparation is as follows: the prepared surface coating is applied to the surface of the wax model, sand (zircon sand) is sprinkled, and dried for 12-24 hours; the transition layer (3 layers) and the reinforcing layer (5 layers) are applied repeatedly. The slurry used is a mixture of back layer silica sol and mullite powder in a ratio of 1:1.5; after dewaxing, it is calcined at 950-1000℃ for 4-6 hours.

[0013] Preparation of the topcoat: The topcoat silica sol and zirconium powder are mixed at a weight ratio of 1:3, and a wetting agent and defoamer are added to adjust the coating performance. A refining agent, which is a core-shell structured particle of cobalt aluminate coated with lanthanum hexaboride, is added to the topcoat, and the amount added is 25-30% of the mass of the topcoat powder.

[0014] The core-shell structured particles are prepared by: generating a cobalt aluminate precursor in situ on the surface of lanthanum hexaboride powder using a sol-gel method, followed by heat treatment at 950-1000℃ in an inert atmosphere. The advantage of the sol-gel method is that it can achieve uniform coating of cobalt aluminate on the surface of lanthanum hexaboride, forming a dense shell structure.

[0015] Lanthanum hexaboride is prone to oxidation and deactivation during high-temperature calcination of the mold shell (approximately 1000°C in air atmosphere), which limits its application in precision casting. The core-shell structure is designed so that during mold shell calcination, the dense cobalt aluminate shell physically protects the lanthanum hexaboride core from premature oxidation and failure. This is the key to enabling the application of lanthanum hexaboride in precision casting.

[0016] During casting, the cobalt aluminate shell preferentially reacts with the molten alloy and is consumed, exposing and releasing [B] atoms of lanthanum hexaboride. The compositional supercooling effect produced by these released [B] atoms effectively interrupts dendrite growth, inducing a large number of new nuclei and thus achieving final grain refinement. The Co particles released from cobalt aluminate have a crystal structure highly compatible with the nickel-based alloy matrix, serving as efficient heterogeneous nucleation nuclei and significantly increasing the nucleation rate, thereby achieving grain refinement. Meanwhile, the [B] atoms released from lanthanum hexaboride are repelled by the solid-liquid interface during solidification, accumulating at the interface front and generating a compositional supercooling effect, further promoting the formation of fine equiaxed crystals. Simultaneously, some [B] atoms segregate at grain boundaries, inhibiting grain growth through a pinning effect, forming a synergistic nucleation-pinning refinement process.

[0017] (3) Casting: The molten material obtained in step (1) is cast into the mold shell obtained in step (2), and the mold shell is preheated to 500-650℃. The following synergistic refining effect occurs during the casting process: The cobalt aluminate shell undergoes a displacement reaction with active elements such as Ti, Al, and Cr in the alloy melt, generating in-situ face-centered cubic metallic Co particles. The lattice constant of Co (3.55 Å) is highly matched with the γ phase of the nickel-based alloy (approximately 3.54 Å), serving as a highly efficient heterogeneous nucleation core, significantly increasing the nucleation rate at the mold wall, forming a fine-grained layer that propagates towards the center of the casting.

[0018] Lanthanum hexaboride releases [B]: After the cobalt aluminate shell is consumed, the internal lanthanum hexaboride is exposed and comes into contact with the molten metal, releasing [B] atoms. B atoms accumulate at the solid-liquid interface front and segregate at grain boundaries, acting as grain boundary pinning agents and inhibiting grain growth. Studies have shown that adding B-containing compounds to the alloy melt can cause B to segregate at grain boundaries, improving grain boundary bonding and inhibiting grain coarsening.

[0019] Internal rare earth synergy: The rare earth elements pre-stored in the melt provide supplementary nucleation cores inside the melt, forming an internal-external synergy with the nucleation of Co particles at the mold wall, achieving fine grains across the entire cross-section from the mold wall to the center of the casting.

[0020] (4) Low-temperature annealing: After casting, the mold shell is cooled and removed to obtain the alloy casting. Then, a low-temperature annealing treatment is performed at 500-600℃ for 4-8 hours. The purpose of low-temperature annealing is to eliminate casting internal stress, stabilize the microstructure, and avoid grain coarsening and dissolution of dispersed particles caused by high-temperature treatment. This invention adopts a low-temperature annealing path, deliberately avoiding high-temperature solution treatment to protect the fine-grained microstructure obtained during the casting stage from damage.

[0021] The beneficial effects of this invention are as follows: This invention involves adding rare earth elements Ce and Y to the melt during the later stages of vacuum melting. These rare earth elements react with residual oxygen in the melt to generate high-melting-point rare earth oxides in situ. These oxides act as nucleation sites, promoting nucleation and transforming columnar crystals into equiaxed crystals, thus refining the grain size. Furthermore, the rare earth oxides can adhere to and coat the surface of inclusions such as Al₂O₃, purifying impurities.

[0022] This invention uses lanthanum hexaboride as the core and cobalt aluminate as the outer shell to form core-shell composite particles. During shell calcination, the lanthanum hexaboride is protected from oxidation and decomposition; during casting, the cobalt aluminate shell reacts with the alloy liquid, generating Co particles in situ as nucleation cores, while lanthanum hexaboride releases [B] atoms to pin grain boundaries, achieving a sequential release of Co particle nucleation and B grain boundary pinning at the mold wall interface.

[0023] Rare earth treatment purifies the melt and provides nucleation sites, while the reaction products of the core-shell particles are confined to the surface of the casting. This approach balances high purity with fine grain refinement, overcoming the contradiction that overall refinement easily introduces inclusions while surface refinement cannot improve the internal structure. The nickel-based alloy castings prepared by this method exhibit better tensile strength, yield strength, and elongation, demonstrating improved overall performance compared to castings produced using conventional processes. Detailed Implementation

[0024] To further illustrate the technical means and effects of the present invention in achieving the intended purpose, the following detailed description of the specific implementation methods, structures, features and effects of the present invention, in conjunction with preferred embodiments, is provided below.

[0025] Examples 1-5 Examples 1-5 provide composite refinement methods for nickel-based alloys and nickel-based alloy castings, respectively. The chemical composition of the nickel-based alloys is shown in Table 2.

[0026] Composite refinement methods for nickel-based alloy castings include: (1) Raw materials were prepared according to the target composition of the nickel-based alloy and added to a vacuum induction melting furnace. Melting was carried out under vacuum conditions ≤5 Pa and temperature 1550-1600℃. In the later stage of melting, a mixture of rare earth elements yttrium (Y) and cerium (Ce) (mass ratio 4:6) was added to the melt at a rate of 0.10% of the melt mass. At the same time, argon gas was blown into the furnace bottom for refining at a flow rate of 1.0-2.0 L / min for 20-30 minutes. The temperature of the resulting melt was lowered to 1450-1490℃ to obtain the casting melt.

[0027] (2) Shell preparation: Apply the prepared surface coating to the surface of the wax model, sprinkle zircon sand, and dry for 12-24 hours; repeat the application of the transition layer (3 layers) and the reinforcing layer (5 layers). The slurry used for the transition layer and the reinforcing layer is a mixture of backing silica sol and mullite powder in a ratio of 1:1.5; after dewaxing, calcine at 950-1000℃ for 4-6 hours.

[0028] (3) The molten material obtained in step (1) is poured into the mold shell obtained in step (2), and the mold shell is preheated to 500-650℃.

[0029] (4) After casting, cool the mold shell and remove the mold shell to obtain the alloy casting. Place the casting in a heat treatment furnace, heat it to 500-600℃, keep it at that temperature for 4-8 hours, then cool it in the furnace to below 300℃, and take it out to air cool to room temperature.

[0030] The topcoat is prepared by mixing the topcoat silica sol and zirconium powder at a weight ratio of 1:3, adding a core-shell structure refiner (25-30% of the zirconium powder mass), and adding 0.1% sodium dodecyl sulfonate and 0.1% n-octanol to adjust the coating performance.

[0031] The preparation of the core-shell structure refiner involved dissolving 23 parts of cobalt nitrate hexahydrate and 60 parts of aluminum nitrate nonahydrate in 65 parts of water, adding 2.0 parts of lanthanum hexaboride powder, and ultrasonically dispersing for 30 minutes. 56 parts of hexamethylenetetramine were dissolved in 100 parts of water to prepare an alkaline solution. The salt solution was kept at 5°C, and the alkaline solution was slowly added dropwise to the salt solution suspension while stirring. After the addition was complete, stirring continued for 2 hours. The gel was then aged at 80°C for 24 hours and dried at 150°C for 24 hours to obtain a dry gel. The dry gel was calcined at 950-1000°C for 1 hour under an inert atmosphere (argon), and then ground through a 325-mesh sieve to obtain the final product.

[0032] Table 1 Examples of process parameters in Examples 1-5

[0033] Table 2 Chemical composition of nickel-based alloys in Examples 1-5:

[0034] Table 3 Mechanical property data of Examples 1-5

[0035] Metallographic observation of the cross-sections of the castings in Examples 1-5 revealed a fine-grained microstructure. Grain refinement is a means to improve the overall performance of nickel-based alloys, enhancing both strength and toughness. Studies have shown that grain refinement significantly increases the number of grain boundaries, more strongly hinders dislocation movement, and consequently improves the yield strength and tensile strength of the material.

[0036] Comparative example: Comparative Examples 1-5 Comparative Examples 1-5 correspond to the alloy composition of Examples 1-5, respectively, and are cast using conventional processes. That is, the difference between them and Examples 1-5 of the present invention is that: no rare earth yttrium and cerium melt pretreatment is performed, and no cobalt aluminate-coated lanthanum hexaboride core-shell structure refiner is added to the shell surface coating.

[0037] Comparative Example 6 The difference from Example 1 is that cobalt aluminate and lanthanum hexaboride are directly added to the shell surface coating in the form of a physically mixed powder.

[0038] Comparative Example 7 The difference from Example 1 is that no rare earth pretreatment is performed.

[0039] Comparative Example 8 The difference from Example 1 is that no refining agent is added to the shell surface coating, otherwise it is the same as Example 1.

[0040] Table 4 Mechanical properties of Comparative Examples 1-7

[0041] This invention provides a composite grain refinement method for nickel-based alloy castings. Through the synergistic effect of melt rare earth pretreatment and a core-shell structure refiner in the mold shell layer, the internal purity and surface grain refinement of the nickel-based alloy castings are synergistically improved. Compared with castings produced by conventional processes, nickel-based alloy castings prepared using this method exhibit an approximately 8-12% increase in tensile strength and an optimized elongation from (51.86-64.06%) to a reasonable range (≥45%), achieving a good balance between strength and plasticity.

[0042] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art can make some modifications or alterations to the above-disclosed technical content to create equivalent embodiments without departing from the scope of the present invention. Any simple modifications, equivalent changes and alterations made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the scope of the present invention.

Claims

1. A composite refining method for nickel-based alloy castings, characterized in that, Includes the following steps: (1) Add nickel-based alloy raw materials to a vacuum induction furnace for melting. In the later stage of melting, add rare earth elements to the melt and blow in inert gas for refining. Reduce the temperature of the resulting melt to 1450-1490℃ to obtain the casting melt. (2) Add a finer agent to the surface coating of the casting shell, wherein the finer agent is cobalt aluminate coated with lanthanum hexaboride; (3) Pour the melt obtained in step (1) into the mold shell described in step (2); (4) After casting is completed and cooled, the mold shell is removed to obtain the alloy casting. The obtained casting is then annealed.

2. The composite refinement method according to claim 1, characterized in that, The nickel-based alloy comprises, by mass percentage: Cr 21.0-22.5%, Mo 12.5-13.5%, Fe 3.0-5.0%, W 2.5-3.5%, with the balance being Ni.

3. The composite refinement method according to claim 1, characterized in that, The nickel-based alloy comprises, by mass percentage: C≤0.02%, Si≤0.8%, Mn≤0.8%, P≤0.01%, S≤0.005%, Cr 21.0-22.5%, Mo 12.5-13.5%, Fe 3.0-5.0%, W 2.5-3.5%, V≤0.2%, Cu≤0.02%, Nb≤0.06%, Ti≤0.03%, Co≤0.15%, Al≤0.02%, with the balance being Ni.

4. The composite refinement method according to claim 1, characterized in that, The rare earth elements mentioned in step (1) are yttrium and cerium, and the amount of rare earth elements added is 0.05-0.15% of the melt mass.

5. The composite refinement method according to claim 1, characterized in that, The inert gas mentioned in step (1) is argon, the argon flow rate is 1.0-2.0 L / min, and the argon blowing time is 20-30 minutes.

6. The composite refinement method according to claim 1, characterized in that, The amount of the refining agent added in step (2) is 25-30% of the mass of the surface powder.

7. The composite refinement method according to claim 1, characterized in that, The preparation method of cobalt aluminate coated lanthanum hexaboride in step (2) is as follows: a cobalt aluminate precursor is generated in situ on the surface of lanthanum hexaboride powder by sol-gel method, and then obtained by heat treatment in an inert atmosphere at 950-1000℃.

8. The composite refinement method according to claim 1, characterized in that, The shell in step (3) is preheated to 500-650℃.

9. The composite refinement method according to claim 1, characterized in that, The annealing temperature in step (4) is 500-600℃, and the holding time is 4-8 hours.

10. A nickel-based alloy casting, characterized in that, It is prepared by the method described in any one of claims 1-9.

Citation Information

Patent Citations

  • Method for improving performance of nickel-based alloy casting

    CN110976773A

  • Technological method for inhibiting columnar crystals on surface of inner cavity of isometric crystal hollow turbine blade

    CN115069979A