A method for preparing a self-supporting electrode with low loading of precious metals for hydrogen production from oilfield produced water and its application.

By depositing Pt on the surface of a non-precious metal alloy, the problem of high precious metal content in hydrogen production from produced water in oil fields has been solved, achieving efficient and low-cost hydrogen production through water electrolysis, improving catalytic performance and mechanical strength, and promoting the recycling of resources.

CN123063804APending Publication Date: 2026-11-10LIAOHE GASOLINEEUM EXPLORATION BUREAU CO LTD +2
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202510594137.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-09
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

In existing oilfield produced water hydrogen production technologies, traditional electrodes have a high content of precious metals, resulting in high investment costs and insufficient catalytic performance, making it difficult to effectively utilize oilfield produced water resources.

Method used

Atomic layer deposition (ALD) is used to deposit a layer of Pt on the surface of a non-precious metal alloy to form a self-supporting electrode with low loading capacity for hydrogen production from produced water in oilfields. The catalytic performance is optimized by controlling the deposition time and thickness.

Benefits of technology

It reduces the amount of precious metals used, improves catalytic performance and mechanical strength, lowers production costs, and enables a highly efficient water electrolysis process for hydrogen production, thereby enhancing energy efficiency and environmental friendliness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123063804A_ABST
    Figure CN123063804A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of hydrogen production technology from produced water in oilfields. It discloses a method for preparing a self-supporting electrode with low-load precious metal in produced water hydrogen production and its application. A non-precious metal alloy is smelted in a vacuum arc furnace, and the smelted alloy liquid is cooled and used as an alloy carrier. Oil contamination on the surface of the alloy carrier is removed using an organic solvent. In an atomic layer deposition system, a Pt compound is used as a precursor material and heated to its vaporization temperature. The atomic layer deposition system temperature is between 200-300℃, and the Pt precursor material is purged for 5-60 seconds. This invention not only solves wastewater treatment problems but also converts the oil and gas components in wastewater into high-value hydrogen resources, improving energy utilization efficiency. Using a non-precious metal alloy as a substrate enhances mechanical strength, increases the durability of the electrode material in the extreme environment of produced water, and reduces production costs. The atomic layer deposition of precious metal Pt on the surface achieves high-efficiency hydrogen evolution at the cathode of the produced water electrolysis process, reducing energy consumption during electrolysis.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of hydrogen production technology from produced water in oilfields, and relates to a method for preparing a self-supporting electrode with low loading of precious metals for hydrogen production from produced water in oilfields and its application. Background Technology

[0002] Produced water hydrogen production technology can be integrated with the oil extraction process to utilize oil and gas components in wastewater, achieving resource recycling. This not only reduces the environmental impact of oil extraction but also improves its economic efficiency. Produced water hydrogen production technology converts oil and gas components into clean energy hydrogen. Compared to traditional petroleum fuels, hydrogen combustion produces exhaust gases that contain almost no harmful substances, resulting in less environmental pollution and effectively reducing greenhouse gas emissions.

[0003] Hydrogen (H2) has a high energy density (between 120 and 142 MJ / kg) and releases water as a clean combustion product, making it a promising energy carrier. H2 is also an indispensable feedstock for some important modern chemical industries, including petroleum refining (e.g., hydrocracking and desulfurization) and ammonia production.

[0004] Hydrogen production by water electrolysis, as the reverse reaction of hydrogen combustion, uses water as the sole raw material to achieve a closed hydrogen cycle with zero carbon emissions, and is therefore considered the greenest and most sustainable method.

[0005] Currently, research on catalytic materials for water electrolysis in neutral saline environments is relatively limited. While phosphorus (Pt) is an excellent catalytic material, its limited reserves on Earth severely restrict its practical application as a cathode material. Atomic layer deposition (ALD) can deposit a single layer of atoms on a metal surface, reducing the amount of Pt required while achieving excellent catalytic performance.

[0006] CN103638925A discloses a core-shell structured catalyst for fuel cells and its pulse electrodeposition preparation method. The catalyst uses a non-platinum noble metal or transition metal as the core and one or more of Pt, Ir, or Au as the shell. The preparation method involves: preparing nanoparticles as the core, fabricating a pulse electrodeposition working electrode, and obtaining the catalyst through pulse electrodeposition. This catalyst can be used as an anode or cathode catalyst in low-temperature fuel cells. However, the method of preparing the working electrode by pulse electrodeposition has shortcomings in terms of film uniformity and process controllability, and is also costly. Summary of the Invention

[0007] The water quality in the process of producing hydrogen from produced water in oil fields is complex, which places high demands on the electrodes. Traditional electrodes have a high content of precious metals, resulting in high investment costs. This invention mainly addresses the problem of reducing the amount of precious metals used in electrode preparation.

[0008] This invention utilizes atomic layer deposition (ALD) to deposit a layer of Pt on the surface of a non-precious metal alloy. Using a Pt compound as a precursor to deposit a Pt layer on the non-precious metal alloy substrate significantly enhances catalytic performance.

[0009] The above-mentioned objective of this invention is achieved through the following technical solutions:

[0010] A method for preparing a self-supporting electrode with low loading of precious metals for hydrogen production from oilfield produced water includes the following steps:

[0011] (1) Alloy preparation: Weigh the non-precious metals and put them into a vacuum arc furnace for melting. Pour the melted alloy liquid into a mold to cool, and use it as an alloy carrier.

[0012] (2) Use organic solvents to wash away the oil stains on the surface of the alloy carrier;

[0013] (3) In the atomic layer deposition system, Pt compounds are used as precursor materials and heated to the vaporization temperature. The temperature of the atomic layer deposition system is between 200-300℃, and the Pt precursor material is purged for 5-60s.

[0014] The working process of the atomic layer deposition system is as follows: a non-precious metal alloy carrier is placed in the reaction chamber and a vacuum is drawn. The Pt precursor material is placed into the purge chamber. The Pt precursor material is deposited on the surface of the non-metallic alloy carrier in the deuterium reaction chamber with the gas flow and deposited into a film under high temperature.

[0015] The thickness of Pt deposition can be controlled by changing the deposition time and the number of depositions, depending on the required thickness.

[0016] Furthermore, step (1) includes non-precious metals such as Ni and Fe, and any mixture of 0 to 4 of the following metals: Cu, Mn, Co, and Zn.

[0017] Furthermore, the mass ratio of Ni to Fe is 1:0.5-2.

[0018] Furthermore, if Cu is included, the mass ratio of Cu to Ni is 0.5-2:1; if Mn is included, the mass ratio of Mn to Ni is 0.5-2:1; if Co is included, the mass ratio of Co to Ni is 0.5-2:1; if Zn is included, the mass ratio of Zn to Ni is 0.5-2:1.

[0019] Furthermore, in step (1), the melting temperature is 1200-1800℃ and the melting time is 15-30min.

[0020] Furthermore, the number of melting operations in step (1) is 2-5 times.

[0021] Furthermore, the organic solvent in step (2) includes alcohol or acetone.

[0022] Furthermore, the compound of Pt in step (3) is trimethylplatinum, hexafluoroacetylacetonate platinum, etc., preferably cyclopentadiene trimethylplatinum.

[0023] Furthermore, before purging the Pt precursor material in step (3), nitrogen gas is used for purging for 5-60 seconds.

[0024] Furthermore, in step (3), the thickness of the Pt precursor material deposition is 5-100 nm.

[0025] Furthermore, the vaporization temperature in step (3) is 60-120℃.

[0026] The application of a self-supporting electrode with low loading of precious metals for hydrogen production from oilfield produced water can be applied to wastewater treatment.

[0027] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0028] Produced water from oil fields, as wastewater generated during oil extraction, is produced in enormous quantities. Utilizing produced water to produce hydrogen not only solves the wastewater treatment problem but also converts the oil and gas components in the wastewater into high-value hydrogen resources, improving energy efficiency. This achieves both pollution reduction and carbon sequestration of produced water, as well as its resource utilization, and also enables the efficient absorption of wind and solar power waste.

[0029] Using a non-precious metal substrate, a high-efficiency hydrogen evolution efficiency was achieved by depositing the precious metal Pt in an atomic layer on the surface of the cathode for electrolytic produced water. Its performance is comparable to that of precious metals, reducing the production cost of cathode materials for water electrolysis. Compared with traditional cathode catalysts, the precious metal loading is reduced by more than 20%, making a 20% cost reduction feasible.

[0030] Atomic layer deposition of Pt will improve catalytic activity and reduce energy consumption during electrolysis. Using a non-precious metal alloy as a substrate will also enhance the mechanical strength of traditional C substrates and increase the durability of electrode materials in the extreme environments of produced water. Attached Figure Description

[0031] Figure 1 These are morphological images of the NiFeCo-200Pt surface before and after deposition. a is the morphological image before deposition, and b is the morphological image after deposition.

[0032] Figure 2 These are the elemental distribution diagrams for NiFeCo-200Pt: a is the elemental distribution diagram for Fe, b is the elemental distribution diagram for Co, c is the elemental distribution diagram for Ni, and d is the elemental distribution diagram for Pt.

[0033] Figure 3 This is the hydrogen evolution polarization curve of NiFeCo-200Pt. Detailed Implementation

[0034] The present invention is described in detail below through specific embodiments, but this does not limit the scope of protection of the present invention. Unless otherwise specified, the experimental methods used in the present invention are all conventional methods, and the experimental equipment, materials, reagents, etc. used can all be obtained commercially.

[0035] Example 1

[0036] (1) Alloy preparation: Weigh 0.25g Ni, 0.25g Fe, 0.25g Co and 0.25g Zn, put them into a vacuum electric arc furnace, melt them at 1300 degrees Celsius for 20 minutes, repeat the melting three times, and pour the melted metal solution into a 30*10*2 copper mold to cool.

[0037] (2) Surface cleaning: Clean the alloy surface with alcohol;

[0038] (3) The precursor was heated to 80 degrees Celsius to vaporize it. The temperature of the atomic layer deposition system was controlled at 270 degrees Celsius, and nitrogen was purged for 25 seconds, followed by purging of the Pt precursor for 25 seconds. The purging was repeated 100 times, and the resulting catalytic electrode was named NiFeCoZn-100Pt.

[0039] Example 2

[0040] (1) Alloy preparation: Weigh 0.25g Ni, 0.25g Fe, 0.25g Cu and 0.25g Mn, put them into a vacuum electric arc furnace, melt them at 1300 degrees Celsius for 20 minutes, repeat the melting three times, and pour the melted metal solution into a 30*10*2 copper mold to cool.

[0041] (2) Surface cleaning: Clean the alloy surface with acetone;

[0042] (3) The precursor was heated to 80 degrees Celsius to vaporize it. The temperature of the atomic layer deposition system was controlled at 270 degrees Celsius, and nitrogen was purged for 25 seconds, followed by purging of the Pt precursor for 25 seconds. The purging was repeated 200 times, and the resulting catalytic electrode was named NiFeCo-200Pt.

[0043] from Figure 1 It can be seen that the alloy surface was smooth before Pt deposition. After depositing 200 layers of Pt, the surface became rough.

[0044] from Figure 2 It can be seen that the alloy substrate has a uniform element distribution, and the Pt deposited on the surface is also uniformly loaded.

[0045] from Figure 3 It can be seen that the overpotential of the original alloy substrate was 194mV, and after atomic layer deposition of Pt, the overpotential decreased to 46mV.

[0046] The embodiments described above are merely preferred embodiments of the present invention, and not all feasible embodiments of the present invention. Any obvious modifications made by those skilled in the art without departing from the principles and spirit of the present invention should be considered to be included within the scope of protection of the claims of the present invention.

Claims

1. A method for preparing a self-supporting electrode with low loading of precious metals for hydrogen production from oilfield produced water, characterized in that, Includes the following steps: (1) Alloy preparation: Weigh the non-precious metals and put them into a vacuum arc furnace for melting. Pour the melted alloy liquid into a mold to cool, and use it as an alloy carrier. (2) Use organic solvents to wash away the oil stains on the surface of the alloy carrier; (3) In the atomic layer deposition system, Pt compounds are used as precursor materials and heated to the vaporization temperature. The temperature of the atomic layer deposition system is between 200-300℃, and the Pt precursor material is purged for 5-60s.

2. The method for preparing a self-supporting electrode with low loading of precious metals for hydrogen production from oilfield produced water according to claim 1, characterized in that, Step (1) Non-precious metals include two metals, Ni and Fe, and any mixture of 0 to 4 of the four metals, Cu, Mn, Co and Zn.

3. The method for preparing a self-supporting electrode with low noble loading metal for hydrogen production from oilfield produced water according to claim 2, characterized in that, The mass ratio of Ni to Fe is 1:0.5-2.

4. The method for preparing a self-supporting electrode with low loading of precious metals for hydrogen production from oilfield produced water according to claim 2, characterized in that, If Cu is included, the mass ratio of Cu to Ni is 0.5-2:1; if Mn is included, the mass ratio of Mn to Ni is 0.5-2:1; if Co is included, the mass ratio of Co to Ni is 0.5-2:1; if Zn is included, the mass ratio of Zn to Ni is 0.5-2:

1.

5. The method for preparing a self-supporting electrode with low loading of precious metals for hydrogen production from oilfield produced water according to claim 1, characterized in that, Step (1) The melting temperature is 1200-1800℃ and the melting time is 15-30min.

6. The method for preparing a self-supporting electrode with low loading of precious metals for hydrogen production from oilfield produced water according to claim 1, characterized in that, Step (1) involves smelting 2-5 times.

7. The method for preparing a self-supporting electrode with low loading of precious metals for hydrogen production from oilfield produced water according to claim 1, characterized in that, Step (2) Organic solvents include alcohol or acetone.

8. The method for preparing a self-supporting electrode with low loading of precious metals for hydrogen production from oilfield produced water according to claim 1, characterized in that, In step (3), the compound of Pt is trimethylplatinum or platinum hexafluoroacetylacetonate.

9. The method for preparing a self-supporting electrode with low loading of precious metals for hydrogen production from oilfield produced water according to claim 1, characterized in that, Before purging the Pt precursor material in step (3), purge with nitrogen for 5-60 seconds.

10. The method for preparing a self-supporting electrode with low loading of precious metals for hydrogen production from oilfield produced water according to claim 1, characterized in that, Step (3) The deposition thickness of the Pt precursor material is 5-100 nm.

11. The method for preparing a self-supporting electrode with low loading of precious metals for hydrogen production from oilfield produced water according to claim 1, characterized in that, The vaporization temperature in step (3) is 60-120℃.

12. An application of a self-supporting electrode with low loading of precious metals in hydrogen production from oilfield produced water, characterized in that, It is used in wastewater treatment.

Citation Information

Patent Citations

  • Core-shell structure catalyst for fuel cells and its pulse electrodeposition preparation method

    CN103638925A