A method for treating lily stems and leaves with a deep eutectic solvent and preparing cellulose
By treating lily stems and leaves with a deep eutectic solvent, the problem of low cellulose extraction efficiency was solved, enabling the preparation of high-purity cellulose and the high-value utilization of resources, while reducing environmental pollution.
Patent Information
- Application Number
- CN202611177935.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-05
- Publication Date
- 2026-11-10
AI Technical Summary
In existing technologies, the extraction efficiency of cellulose from lily stem and leaf waste is low. Traditional methods result in resource waste and environmental pollution, and cellulose is easily damaged under strong acid and alkali conditions.
High-purity cellulose was prepared by treating lily stems and leaves with a deep eutectic solvent, and by extracting the eutectic mixture formed by hydrogen bond acceptors and hydrogen bond donors through heating and stirring, followed by centrifugation.
This method achieves efficient extraction and purification of cellulose from lily stems and leaves, with a cellulose purity of over 90%, reducing energy consumption and wastewater generation, and realizing the high-value utilization of resources.
Smart Images

Figure CN123064037A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of cellulose extraction technology from lily stems and leaves, specifically relating to a method for treating lily stems and leaves with a deep eutectic solvent to prepare cellulose. Background Technology
[0002] Lily production generates significant waste products, such as bulb outer skin and substandard rhizomes, in the medicinal, edible, and floricultural industries. Currently, most of this waste is landfilled or incinerated, resulting in resource waste and environmental pollution. Most research focuses on extracting medicinal active ingredients, while the waste residue after extraction receives little attention. Even after extracting active ingredients, lily stem and leaf waste remains rich in cellulose, hemicellulose, and lignin, representing a potential biomass resource. Cellulose, in particular, can be further used to prepare high-value-added products such as nanocellulose, bioethanol, and biodegradable membranes.
[0003] Traditional cellulose extraction methods include alkaline treatment (such as boiling with sodium hydroxide), acid hydrolysis, and bleaching. These methods have problems such as large wastewater generation, severe equipment corrosion, and the degree of polymerization of cellulose being easily damaged under strong acid and alkali conditions.
[0004] Deep eutectic solvents are eutectic mixtures formed by hydrogen bond acceptors (such as choline chloride) and hydrogen bond donors (such as lactic acid, oxalic acid, malic acid, etc.) through hydrogen bonding. Deep eutectic solvents possess green chemical properties such as biodegradability, low cost, low vapor pressure, non-flammability, and recyclability. Previous studies have used deep eutectic solvents for the pretreatment of lignocellulose, but their application on the specific matrix of lily waste, particularly a systematic method for the high-value extraction of cellulose, has not yet been reported. Summary of the Invention
[0005] Purpose of the invention: In order to solve the above-mentioned technical problems, the present invention provides a method for treating lily stems and leaves with a deep eutectic solvent to prepare cellulose, which can achieve efficient extraction and purification of cellulose.
[0006] Technical Solution: To achieve the above-mentioned objectives, the technical solution adopted by this invention is as follows:
[0007] A method for treating lily stems and leaves with a deep eutectic solvent and preparing cellulose includes the following steps:
[0008] (1) The lily stem and leaf waste residue is dried, crushed and sieved to obtain lily stem and leaf waste residue powder;
[0009] (2) Using hydrogen bond acceptors and hydrogen bond donors as the main raw materials, a deep eutectic solvent was prepared;
[0010] (3) Mix the powder obtained in step (1) with the deep eutectic solvent obtained in step (2), and heat and stir to extract;
[0011] (4) Separate the solid residue, wash and dry it to obtain lily stem and leaf cellulose.
[0012] As a specific implementation plan, in step (1), the lily stem and leaf waste residue is the lily stem and leaf residue that has undergone supercritical or subcritical extraction to extract active substances such as polyphenols.
[0013] As a specific implementation plan, in step (2), the hydrogen bond acceptor is choline chloride; the hydrogen bond donor is selected from one or more of lactic acid, citric acid, glycerol, propylene glycol, ethylene glycol, urea, and ascorbic acid.
[0014] The water content of the deep eutectic solvent is controlled at 10% to 40% (mass fraction, w / w).
[0015] As a further implementation, in step (2), the deep eutectic solvent is a binary deep eutectic solvent formed by pairing choline chloride as a hydrogen bond acceptor with lactic acid, citric acid, glycerol, propylene glycol, ethylene glycol, urea, or ascorbic acid, respectively, wherein the molar ratio of hydrogen bond acceptor to hydrogen bond donor is 1:(1-3); or, the deep eutectic solvent is a ternary deep eutectic solvent of choline chloride / lactic acid / glycerol, choline chloride / malic acid / propylene glycol, or choline chloride / citric acid / glycerol, wherein the molar ratio of hydrogen bond acceptor, hydrogen bond donor, and hydrogen bond donor is 1:(1-3):(1-3);
[0016] Preferably, the deep eutectic solvent is mainly a binary deep eutectic solvent made of choline chloride and malic acid, with a molar ratio of choline chloride to malic acid of 1:2 and a water content of 10% (w / w).
[0017] As a specific implementation plan, in step (3), the extraction temperature is 90~150℃, the time is 1~3 hours, the stirring speed is 300-900 rpm, and the solid-liquid ratio is 1:(15-25) (g / mL); preferably, the temperature is 150℃, the time is 2-3 hours, the stirring speed is 600 rpm, and the solid-liquid ratio is 1:20 (g / mL).
[0018] As a specific implementation plan, in step (4), the separation of solid residue is carried out by centrifugation, including: adding a small amount of deionized water to balance the mixture, and centrifuging at 10,000-12,000 rpm for 10-15 minutes; preferably, centrifuging at 10,000 rpm for 15 minutes.
[0019] The washing process involves first washing with deionized water until neutral, and then washing with anhydrous ethanol.
[0020] The drying conditions are: temperature 50-60℃, drying time 12-24 hours.
[0021] As a specific implementation plan, the method further includes: taking the lily stem and leaf cellulose obtained in step (4), adding sodium hypochlorite solution, heating and reacting, filtering, drying, repeating 2 to 3 times to obtain purified lily stem and leaf cellulose.
[0022] As a further embodiment, the sodium hypochlorite solution has a concentration of 0.5-1.5 wt%, a solid-liquid ratio of 1:(25-35) (g / mL), and the heating reaction is carried out at a temperature of 90-100℃ for 0.1-1 hours.
[0023] The present invention also provides lily stem and leaf cellulose prepared by the above method.
[0024] This invention systematically investigated the effects of extraction temperature, processing time, and solvent moisture content on the extraction of cellulose from lily stem and leaf residues using eutectic solvents. Furthermore, this invention combined the National Renewable Energy Laboratory (NREL) method and the 1-phenyl-3-methyl-5-pyrazolone derivatization method for cellulose content determination. The results showed that eutectic solvents can promote the removal of non-cellulose components from lily stem and leaf residues, significantly improving the purity of the obtained solid cellulose. In particular, the choline chloride / malic acid eutectic solvent showed significantly better extraction performance, achieving unexpected results.
[0025] This invention has the following innovative features:
[0026] (1) Raw material innovation: For the first time, cellulose was extracted from lily stem and leaf waste, realizing the resource utilization of agricultural waste and turning waste into treasure.
[0027] (2) Green solvent: Deep eutectic solvent is used, and the raw materials are all biodegradable natural products that are non-toxic, non-corrosive, and recyclable, which is in line with the concept of green chemistry.
[0028] (3) Mild process: The extraction temperature is 90-150℃, rather than high temperature and high pressure conditions, resulting in low energy consumption, less cellulose degradation, and high crystallinity.
[0029] (4) High extraction efficiency: selectively removes lignin and hemicellulose. In the preferred scheme, the purity of cellulose after bleaching and purification can reach more than 90%.
[0030] Beneficial effects: Compared with the prior art, the present invention has the following advantages:
[0031] (1) High purity: The purity of the cellulose obtained by this invention after bleaching is ≥90%;
[0032] (2) Environmental protection: No strong acids or alkalis are used, no corrosive wastewater is generated, and the deep eutectic solvent can be recycled and reused;
[0033] (3) Wide range of raw material sources: Lily stems and leaves are a large amount of agricultural waste, and the cost is low. Attached Figure Description
[0034] Figure 1 The effects of choline chloride / malic acid eutectic solvent on the solid recovery rate and cellulose purity of lily stem and leaf residue under different temperatures, times, and moisture contents. (A) represents the solid recovery rate at different temperatures under a moisture content of 10% for 1 hour; (B) represents the solid recovery rate at different moisture contents under a moisture content of 150℃ for 1 hour; (C) represents the solid recovery rate at different treatment times under a moisture content of 10% for 150℃; (D), (E), and (F) represent the cellulose purity of the product under the treatment conditions (A), (B), and (C).
[0035] Figure 2 X-ray diffraction patterns: black represents the raw material, and red represents the sample obtained in Example 8.
[0036] Figure 3 Fourier transform infrared spectra; black represents the raw material, and red represents the sample obtained in Example 8. Detailed Implementation
[0037] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0038] The preparation method of the lily stem and leaf residue powder used in the following examples is as follows: The lily stem and leaf residue (cellulose content of 42.9%), which has been extracted with polyphenols and other active substances by supercritical or subcritical methods, is dried at 60°C for 24 hours, pulverized and passed through an 80-mesh sieve, and the lily stem and leaf residue powder is obtained after sieving.
[0039] The preparation method of the choline chloride / malic acid deep eutectic solvent used in Examples 1-18 is as follows: Choline chloride and malic acid are mixed in a molar ratio of 1:2 and reacted at 80°C with stirring until a homogeneous and transparent liquid is formed. The stirring speed is 300 rpm. After cooling, deionized water is added to adjust the water content of the solvent. The mixture is heated at 80°C with stirring for 0.5-1 hour until a transparent and homogeneous solution is formed.
[0040] Example 1
[0041] Step (1): Weigh 1g of lily stem and leaf residue powder, add 20mL of choline chloride / malic acid with 10% water content, and stir in an oil bath at 90℃ for 1 hour at a stirring speed of 600 rpm.
[0042] Step (2): After the reaction is complete, transfer the mixture to a centrifuge tube, centrifuge at 10,000 rpm for 15 minutes, remove the filtrate, and collect the residue.
[0043] Step (3): Wash the residue repeatedly with deionized water until the filtrate is neutral (pH≈7), then wash once with about 50 mL of anhydrous ethanol, and dry at 60°C overnight to obtain crude cellulose product.
[0044] The solid mass recovery rate was 92.7% based on weighing. The cellulose content in the product was determined to be 46.7% using the method of the National Renewable Energy Laboratory (NREL).
[0045] Example 2
[0046] Step (1): Weigh 1g of lily stem and leaf residue powder, add 20mL of choline chloride / malic acid with 10% water content, and stir in an oil bath at 90℃ for 2 hours at a stirring speed of 600 rpm.
[0047] Step (2): After the reaction is complete, transfer the mixture to a centrifuge tube, centrifuge at 10,000 rpm for 15 minutes, remove the filtrate, and collect the residue.
[0048] Step (3): Wash the residue repeatedly with deionized water until the filtrate is neutral (pH≈7), then wash once with about 50 mL of anhydrous ethanol, and dry at 60°C overnight to obtain crude cellulose product.
[0049] Results: The solid mass recovery rate was 94.3%, and the cellulose content in the product was 49.3%.
[0050] Example 3
[0051] Step (1): Weigh 1g of lily stem and leaf residue powder, add 20mL of choline chloride / malic acid with 10% water content, and stir in an oil bath at 90℃ for 3 hours at a stirring speed of 600 rpm.
[0052] Step (2): After the reaction is complete, transfer the mixture to a centrifuge tube, centrifuge at 10,000 rpm for 15 minutes, remove the filtrate, and collect the residue.
[0053] Step (3): Wash the residue repeatedly with deionized water until the filtrate is neutral (pH≈7), then wash once with about 50 mL of anhydrous ethanol, and dry at 60°C overnight to obtain crude cellulose product.
[0054] Results: The solid mass recovery rate was 93.9%, and the cellulose content in the product was 44.0%.
[0055] Example 4
[0056] Step (1): Weigh 1g of lily stem and leaf residue powder, add 20mL of choline chloride / malic acid with 10% water content, and stir in an oil bath at 120℃ for 1 hour at a stirring speed of 600 rpm.
[0057] Step (2): After the reaction is complete, transfer the mixture to a centrifuge tube, centrifuge at 10,000 rpm for 15 minutes, remove the filtrate, and collect the residue.
[0058] Step (3): Wash the residue repeatedly with deionized water until the filtrate is neutral (pH≈7), then wash once with about 50 mL of anhydrous ethanol, and dry at 60°C overnight to obtain crude cellulose product.
[0059] Results: The solid mass recovery rate was 83.1%, and the cellulose content in the product was 44.6%.
[0060] Example 5
[0061] Step (1): Weigh 1g of lily stem and leaf residue powder, add 20mL of choline chloride / malic acid with 10% water content, and stir in an oil bath at 120℃ for 3 hours at a stirring speed of 600 rpm.
[0062] Step (2): After the reaction is complete, transfer the mixture to a centrifuge tube, centrifuge at 10,000 rpm for 15 minutes, remove the filtrate, and collect the residue.
[0063] Step (3): Wash the residue repeatedly with deionized water until the filtrate is neutral (pH≈7), then wash once with about 50 mL of anhydrous ethanol, and dry at 60°C overnight to obtain crude cellulose product.
[0064] Results: The solid mass recovery rate was 68.5%, and the cellulose content in the product was 43.7%.
[0065] Example 6
[0066] Step (1): Weigh 1g of lily stem and leaf residue powder, add 20mL of choline chloride / malic acid with 10% water content, and stir in an oil bath at 150℃ for 1 hour at a stirring speed of 600 rpm.
[0067] Step (2): After the reaction is complete, transfer the mixture to a centrifuge tube, centrifuge at 10,000 rpm for 15 minutes, remove the filtrate, and collect the residue.
[0068] Step (3): Wash the residue repeatedly with deionized water until the filtrate is neutral (pH≈7), then wash once with about 50 mL of anhydrous ethanol, and dry at 60°C overnight to obtain crude cellulose product.
[0069] Results: The solid mass recovery rate was 68.8%, and the cellulose content in the product was 73.9%.
[0070] Example 7
[0071] Step (1): Weigh 1g of lily stem and leaf residue powder, add 20mL of choline chloride / malic acid with 10% water content, and stir in an oil bath at 150℃ for 2 hours at a stirring speed of 600 rpm.
[0072] Step (2): After the reaction is complete, transfer the mixture to a centrifuge tube, centrifuge at 10,000 rpm for 15 minutes, remove the filtrate, and collect the residue.
[0073] Step (3): Wash the residue repeatedly with deionized water until the filtrate is neutral (pH≈7), then wash once with about 50 mL of anhydrous ethanol, and dry at 60°C overnight to obtain crude cellulose product.
[0074] Results: The solid mass recovery rate was 54.2%, and the cellulose content in the product was 80.2%.
[0075] Example 8
[0076] Step (1): Weigh 1g of lily stem and leaf residue powder, add 20mL of choline chloride / malic acid with 10% water content, and stir in an oil bath at 150℃ for 3 hours at a stirring speed of 600 rpm.
[0077] Step (2): After the reaction is complete, transfer the mixture to a centrifuge tube, centrifuge at 10,000 rpm for 15 minutes, remove the filtrate, and collect the residue.
[0078] Step (3): Wash the residue repeatedly with deionized water until the filtrate is neutral (pH≈7), then wash once with about 50 mL of anhydrous ethanol, and dry at 60°C overnight to obtain crude cellulose product.
[0079] Results: The solid mass recovery rate was 52.4%, and the cellulose content in the product was 83.7%.
[0080] Example 9
[0081] Step (1): Weigh 1g of lily stem and leaf residue powder, add 20mL of choline chloride / malic acid with 25% water content, and stir in an oil bath at 90℃ for 1 hour at a stirring speed of 600 rpm.
[0082] Step (2): After the reaction is complete, transfer the mixture to a centrifuge tube, centrifuge at 10,000 rpm for 15 minutes, remove the filtrate, and collect the residue.
[0083] Step (3): Wash the residue repeatedly with deionized water until the filtrate is neutral (pH≈7), then wash once with about 50 mL of anhydrous ethanol, and dry at 60°C overnight to obtain crude cellulose product.
[0084] Results: The solid mass recovery rate was 91.6%. The cellulose content in the product was 46.1%.
[0085] Example 10
[0086] Step (1): Weigh 1g of lily stem and leaf residue powder, add 20mL of choline chloride / malic acid with 25% water content, and stir in an oil bath at 90℃ for 3 hours at a stirring speed of 600 rpm.
[0087] Step (2): After the reaction is complete, transfer the mixture to a centrifuge tube, centrifuge at 10,000 rpm for 15 minutes, remove the filtrate, and collect the residue.
[0088] Step (3): Wash the residue repeatedly with deionized water until the filtrate is neutral (pH≈7), then wash once with about 50 mL of anhydrous ethanol, and dry at 60°C overnight to obtain crude cellulose product.
[0089] Results: The solid mass recovery rate was 93.2%, and the cellulose content in the product was 43.3%.
[0090] Example 11
[0091] Step (1): Weigh 1g of lily stem and leaf residue powder, add 20mL of choline chloride / malic acid with 25% water content, and stir in an oil bath at 120℃ for 1 hour at a stirring speed of 600 rpm.
[0092] Step (2): After the reaction is complete, transfer the mixture to a centrifuge tube, centrifuge at 10,000 rpm for 15 minutes, remove the filtrate, and collect the residue.
[0093] Step (3): Wash the residue repeatedly with deionized water until the filtrate is neutral (pH≈7), then wash once with about 50 mL of anhydrous ethanol, and dry at 60°C overnight to obtain crude cellulose product.
[0094] Results: The solid mass recovery rate was 73.8%, and the cellulose content in the product was 63.6%.
[0095] Example 12
[0096] Step (1): Weigh 1g of lily stem and leaf residue powder, add 20mL of choline chloride / malic acid with 25% water content, and stir in an oil bath at 150℃ for 1 hour at a stirring speed of 600 rpm.
[0097] Step (2): After the reaction is complete, transfer the mixture to a centrifuge tube, centrifuge at 10,000 rpm for 15 minutes, remove the filtrate, and collect the residue.
[0098] Step (3): Wash the residue repeatedly with deionized water until the filtrate is neutral (pH≈7), then wash once with about 50 mL of anhydrous ethanol, and dry at 60°C overnight to obtain crude cellulose product.
[0099] Results: The solid mass recovery rate was 66.5%, and the cellulose content in the product was 53.1%.
[0100] Example 13
[0101] Step (1): Weigh 1g of lily stem and leaf residue powder, add 20mL of choline chloride / malic acid with 25% water content, and stir in an oil bath at 150℃ for 2 hours at a stirring speed of 600 rpm.
[0102] Step (2): After the reaction is complete, transfer the mixture to a centrifuge tube, centrifuge at 10,000 rpm for 15 minutes, remove the filtrate, and collect the residue.
[0103] Step (3): Wash the residue repeatedly with deionized water until the filtrate is neutral (pH≈7), then wash once with about 50 mL of anhydrous ethanol, and dry at 60°C overnight to obtain crude cellulose product.
[0104] Results: The solid mass recovery rate was 54.3%, and the cellulose content in the product was 70.9%.
[0105] Example 14
[0106] Step (1): Weigh 1g of lily stem and leaf residue powder, add 20mL of choline chloride / malic acid with 40% water content, and stir in an oil bath at 90℃ for 1 hour at a stirring speed of 600 rpm.
[0107] Step (2): After the reaction is complete, transfer the mixture to a centrifuge tube, centrifuge at 10,000 rpm for 15 minutes, remove the filtrate, and collect the residue.
[0108] Step (3): Wash the residue repeatedly with deionized water until the filtrate is neutral (pH≈7), then wash once with about 50 mL of anhydrous ethanol, and dry at 60°C overnight to obtain crude cellulose product.
[0109] Results: The solid mass recovery rate was 92.9%, and the cellulose content in the product was 44.9%.
[0110] Example 15
[0111] Step (1): Weigh 1g of lily stem and leaf residue powder, add 20mL of choline chloride / malic acid with 40% water content, and stir in an oil bath at 120℃ for 2 hours at a stirring speed of 600 rpm.
[0112] Step (2): After the reaction is complete, transfer the mixture to a centrifuge tube, centrifuge at 10,000 rpm for 15 minutes, remove the filtrate, and collect the residue.
[0113] Step (3): Wash the residue repeatedly with deionized water until the filtrate is neutral (pH≈7), then wash once with about 50 mL of anhydrous ethanol, and dry at 60°C overnight to obtain crude cellulose product.
[0114] Results: The solid mass recovery rate was 66.1%, and the cellulose content in the product was 48.4%.
[0115] Example 16
[0116] Step (1): Weigh 1g of lily stem and leaf residue powder, add 20mL of choline chloride / malic acid with 40% water content, and stir in an oil bath at 120℃ for 3 hours at a stirring speed of 600 rpm.
[0117] Step (2): After the reaction is complete, transfer the mixture to a centrifuge tube, centrifuge at 10,000 rpm for 15 minutes, remove the filtrate, and collect the residue.
[0118] Step (3): Wash the residue repeatedly with deionized water until the filtrate is neutral (pH≈7), then wash once with about 50 mL of anhydrous ethanol, and dry at 60°C overnight to obtain crude cellulose product.
[0119] Results: The solid mass recovery rate was 62.7%, and the cellulose content in the product was 58.4%.
[0120] Example 17
[0121] Step (1): Weigh 1g of lily stem and leaf residue powder, add 20mL of choline chloride / malic acid with 40% water content, and stir in an oil bath at 150℃ for 1 hour at a stirring speed of 600 rpm.
[0122] Step (2): After the reaction is complete, transfer the mixture to a centrifuge tube, centrifuge at 10,000 rpm for 15 minutes, remove the filtrate, and collect the residue.
[0123] Step (3): Wash the residue repeatedly with deionized water until the filtrate is neutral (pH≈7), then wash once with about 50 mL of anhydrous ethanol, and dry at 60°C overnight to obtain crude cellulose product.
[0124] Results: The solid mass recovery rate was 83.6%, and the cellulose content in the product was 50.2%.
[0125] Example 18
[0126] Step (1): Weigh 1g of lily stem and leaf residue powder, add 20mL of choline chloride / malic acid with 40% water content, and stir in an oil bath at 150℃ for 3 hours at a stirring speed of 600 rpm.
[0127] Step (2): After the reaction is complete, transfer the mixture to a centrifuge tube, centrifuge at 10,000 rpm for 15 minutes, remove the filtrate, and collect the residue.
[0128] Step (3): Wash the residue repeatedly with deionized water until the filtrate is neutral (pH≈7), then wash once with about 50 mL of anhydrous ethanol, and dry at 60°C overnight to obtain crude cellulose product.
[0129] Results: The solid mass recovery rate was 64.3%, and the cellulose content in the product was 65.2%.
[0130] Bleaching Examples
[0131] Step (1): Weigh 0.3g of the extract from Example 8, add 9mL of 1wt% sodium hypochlorite solution, and stir in a 95°C oil bath for 0.5 hours.
[0132] Step (2): After the reaction is complete, cool to room temperature, vacuum filter the mixture, rinse the flask wall with about 50 mL of deionized water to remove any remaining extract and wash the extract, and dry at 60°C overnight.
[0133] Step (3): Repeat steps (1) and (2) above twice to remove residual lignin more thoroughly and obtain the final cellulose product.
[0134] Results: The solid mass recovery rate was 72.8%, and the cellulose content in the product was 97.6%.
[0135] Examples 19-28 below illustrate the application of other eutectic solvent systems using choline chloride as a hydrogen bond acceptor in the extraction of cellulose from lily stem and leaf residues. Each new eutectic solvent was first paired with a single hydrogen bond donor to form a binary system, with only a small number of ternary systems included for comparison. The extraction conditions for each new example were uniformly set as follows: 10% water content, 150°C, and 1 hour. The reference results are listed in Table 1.
[0136] Example 19
[0137] Step (1): Mix choline chloride and lactic acid in a molar ratio of 1:2 and stir at 70°C for 1 hour to form a homogeneous and transparent choline chloride / lactic acid eutectic solvent. Add deionized water to adjust the water content to 10%. Weigh 1g of lily stem and leaf residue powder, add 20mL of the above choline chloride / lactic acid eutectic solvent, and stir in an oil bath at 150°C for 1 hour at a stirring speed of 600 rpm.
[0138] Step (2): After the reaction is complete, transfer the mixture to a centrifuge tube, centrifuge at 10,000 rpm for 15 minutes, remove the filtrate, and collect the residue.
[0139] Step (3): Wash the residue repeatedly with deionized water until the filtrate is neutral (pH≈7), then wash once with about 50 mL of anhydrous ethanol, and dry overnight at 60°C to obtain the crude cellulose product treated with the choline chloride / lactic acid system.
[0140] Results: The solid mass recovery rate was 65.7%, and the cellulose content was 50.1%.
[0141] Example 20
[0142] Step (1): Mix choline chloride and citric acid in a molar ratio of 1:1 and stir at 80°C for 1 hour to form a homogeneous and transparent choline chloride / citric acid eutectic solvent. Add deionized water to adjust the water content to 10%. Weigh 1g of lily stem and leaf residue powder, add 20mL of the above choline chloride / citric acid eutectic solvent, and stir in an oil bath at 150°C for 1 hour at a stirring speed of 600 rpm.
[0143] Step (2): After the reaction is complete, transfer the mixture to a centrifuge tube, centrifuge at 10,000 rpm for 15 minutes, remove the filtrate, and collect the residue.
[0144] Step (3): Wash the residue repeatedly with deionized water until the filtrate is neutral (pH≈7), then wash once with about 50 mL of anhydrous ethanol, and dry at 60 °C overnight to obtain the crude cellulose product treated with the choline chloride / citric acid system.
[0145] Results: The solid mass recovery rate was 62.4%, and the cellulose content was 62.8%.
[0146] Example 21
[0147] Step (1): Mix choline chloride and glycerol at a molar ratio of 1:2 and stir at 70°C for 1 hour to form a homogeneous and transparent choline chloride / glycerol eutectic solvent. Add deionized water to adjust the water content to 10%. Weigh 1g of lily stem and leaf residue powder, add 20mL of the above choline chloride / glycerol eutectic solvent, and stir in an oil bath at 150°C for 1 hour at a stirring speed of 600 rpm.
[0148] Step (2): After the reaction is complete, transfer the mixture to a centrifuge tube, centrifuge at 10,000 rpm for 15 minutes, remove the filtrate, and collect the residue.
[0149] Step (3): Wash the residue repeatedly with deionized water until the filtrate is neutral (pH≈7), then wash once with about 50 mL of anhydrous ethanol, and dry at 60 °C overnight to obtain the crude cellulose product treated with the choline chloride / glycerol system.
[0150] Results: The solid mass recovery rate was 76.8%, and the cellulose content was 55.6%.
[0151] Example 22
[0152] Step (1): Mix choline chloride and propylene glycol at a molar ratio of 1:2 and stir at 70°C for 1 hour to form a homogeneous and transparent choline chloride / propylene glycol eutectic solvent. Add deionized water to adjust the water content to 10%. Weigh 1g of lily stem and leaf residue powder, add 20mL of the above choline chloride / propylene glycol eutectic solvent, and stir in an oil bath at 150°C for 1 hour at a stirring speed of 600 rpm.
[0153] Step (2): After the reaction is complete, transfer the mixture to a centrifuge tube, centrifuge at 10,000 rpm for 15 minutes, remove the filtrate, and collect the residue.
[0154] Step (3): Wash the residue repeatedly with deionized water until the filtrate is neutral (pH≈7), then wash once with about 50 mL of anhydrous ethanol, and dry at 60 °C overnight to obtain the crude cellulose product treated with the choline chloride / propylene glycol system.
[0155] Results: The solid mass recovery rate was 73.5%, and the cellulose content was 58.9%.
[0156] Example 23
[0157] Step (1): Mix choline chloride and ethylene glycol at a molar ratio of 1:2 and stir at 70°C for 1 hour to form a homogeneous and transparent choline chloride / ethylene glycol eutectic solvent. Add deionized water to adjust the water content to 10%. Weigh 1g of lily stem and leaf residue powder, add 20mL of the above choline chloride / ethylene glycol eutectic solvent, and stir in an oil bath at 150°C for 1 hour at a stirring speed of 600 rpm.
[0158] Step (2): After the reaction is complete, transfer the mixture to a centrifuge tube, centrifuge at 10,000 rpm for 15 minutes, remove the filtrate, and collect the residue.
[0159] Step (3): Wash the residue repeatedly with deionized water until the filtrate is neutral (pH≈7), then wash once with about 50 mL of anhydrous ethanol, and dry at 60 °C overnight to obtain the crude cellulose product treated with the choline chloride / ethylene glycol system.
[0160] Results: The solid mass recovery rate was 74.2%, and the cellulose content was 57.4%.
[0161] Example 24
[0162] Step (1): Mix choline chloride and urea at a molar ratio of 1:2 and stir at 80°C for 1 hour to form a homogeneous and transparent choline chloride / urea eutectic solvent. Add deionized water to adjust the water content to 10%. Weigh 1g of lily stem and leaf residue powder, add 20mL of the above choline chloride / urea eutectic solvent, and stir in an oil bath at 150°C for 1 hour at a stirring speed of 600 rpm.
[0163] Step (2): After the reaction is complete, transfer the mixture to a centrifuge tube, centrifuge at 10,000 rpm for 15 minutes, remove the filtrate, and collect the residue.
[0164] Step (3): Wash the residue repeatedly with deionized water until the filtrate is neutral (pH≈7), then wash once with about 50 mL of anhydrous ethanol, and dry overnight at 60°C to obtain the crude cellulose product treated with the choline chloride / urea system.
[0165] Results: The solid mass recovery rate was 78.6%, and the cellulose content was 54.8%.
[0166] Example 25
[0167] Step (1): Mix choline chloride and ascorbic acid at a molar ratio of 1:1 and stir at 70°C for 1 hour to form a homogeneous and transparent choline chloride / ascorbic acid eutectic solvent. Add deionized water to adjust the water content to 10%. Weigh 1g of lily stem and leaf residue powder, add 20mL of the above choline chloride / ascorbic acid eutectic solvent, and stir in an oil bath at 150°C for 1 hour at a stirring speed of 600 rpm.
[0168] Step (2): After the reaction is complete, transfer the mixture to a centrifuge tube, centrifuge at 10,000 rpm for 15 minutes, remove the filtrate, and collect the residue.
[0169] Step (3): Wash the residue repeatedly with deionized water until the filtrate is neutral (pH≈7), then wash once with about 50 mL of anhydrous ethanol, and dry at 60 °C overnight to obtain the crude cellulose product treated with the choline chloride / ascorbic acid system.
[0170] Results: The solid mass recovery rate was 69.4%, and the cellulose content was 61.7%.
[0171] Example 26
[0172] Step (1): Mix choline chloride, lactic acid, and glycerol in a molar ratio of 1:2:1 and stir at 70°C for 1 hour to form a homogeneous and transparent ternary eutectic solvent of choline chloride / lactic acid / glycerol. Add deionized water to adjust the water content to 10%. Weigh 1g of lily stem and leaf residue powder and add 20mL of the above choline chloride / lactic acid / glycerol eutectic solvent. Stir the mixture in an oil bath at 150°C for 1 hour at a stirring speed of 600 rpm.
[0173] Step (2): After the reaction is complete, transfer the mixture to a centrifuge tube, centrifuge at 10,000 rpm for 15 minutes, remove the filtrate, and collect the residue.
[0174] Step (3): Wash the residue repeatedly with deionized water until the filtrate is neutral (pH≈7), then wash once with about 50 mL of anhydrous ethanol, and dry at 60 °C overnight to obtain the crude cellulose product treated with the choline chloride / lactic acid / glycerol system.
[0175] Results: The solid mass recovery rate was 60.8%, and the cellulose content was 68.5%.
[0176] Example 27
[0177] Step (1): Mix choline chloride, malic acid, and propylene glycol in a molar ratio of 1:2:1 and stir at 80°C for 1 hour to form a homogeneous and transparent ternary eutectic solvent of choline chloride / malic acid / propylene glycol. Add deionized water to adjust the water content to 10%. Weigh 1g of lily stem and leaf residue powder, add 20mL of the above choline chloride / malic acid / propylene glycol eutectic solvent, and stir in an oil bath at 150°C for 1 hour at a stirring speed of 600 rpm.
[0178] Step (2): After the reaction is complete, transfer the mixture to a centrifuge tube, centrifuge at 10,000 rpm for 15 minutes, remove the filtrate, and collect the residue.
[0179] Step (3): Wash the residue repeatedly with deionized water until the filtrate is neutral (pH≈7), then wash once with about 50 mL of anhydrous ethanol, and dry at 60 °C overnight to obtain the crude cellulose product treated with the choline chloride / malic acid / propylene glycol system.
[0180] Results: The solid mass recovery rate was 55.6%, and the cellulose content was 78.4%.
[0181] Example 28
[0182] Step (1): Mix choline chloride, citric acid, and glycerol in a molar ratio of 1:1:2 and stir at 80°C for 1 hour to form a homogeneous and transparent ternary eutectic solvent of choline chloride / citric acid / glycerol. Add deionized water to adjust the water content to 10%. Weigh 1g of lily stem and leaf residue powder and add 20mL of the above choline chloride / citric acid / glycerol eutectic solvent. Stir the mixture in an oil bath at 150°C for 1 hour at a stirring speed of 600 rpm.
[0183] Step (2): After the reaction is complete, transfer the mixture to a centrifuge tube, centrifuge at 10,000 rpm for 15 minutes, remove the filtrate, and collect the residue.
[0184] Step (3): Wash the residue repeatedly with deionized water until the filtrate is neutral (pH≈7), then wash once with about 50 mL of anhydrous ethanol, and dry overnight at 60 °C to obtain the crude cellulose product treated with the choline chloride / citric acid / glycerol system.
[0185] Results: The solid mass recovery rate was 59.8%, and the cellulose content was 67.3%.
[0186] The comparative experiment used traditional sodium hydroxide solution for extraction.
[0187] Step (1): Weigh 1g of lily stem and leaf residue powder, add 20mL of 10% sodium hydroxide solution, and stir in an oil bath at 90℃ for 1 hour.
[0188] Step (2): After the reaction is complete, transfer the mixture to a centrifuge tube, centrifuge at 10,000 rpm for 15 minutes, remove the filtrate, and collect the residue.
[0189] Step (3): Wash the residue repeatedly with deionized water until the filtrate is neutral (pH≈7), then wash once with 50 mL of anhydrous ethanol, and dry overnight at 60 °C to obtain crude cellulose product.
[0190] Results: The solid mass recovery rate was 59.3%, and the cellulose content in the product was 59.1%.
[0191] Test case
[0192] I. Testing Methods
[0193] 1) Cellulose solids recovery rate: The solids recovery rate is used to characterize the mass retention of the solid product obtained after deep eutectic solvent (DES) treatment, washing, and drying relative to the original lily stem and leaf residue, and is calculated using the following formula:
[0194] Solid mass recovery rate (%) = m1 / m0 × 100%
[0195] In the formula, m0 is the dry weight of the lily stem and leaf residue powder before treatment, and m1 is the dry weight of the solid product obtained after treatment with deep eutectic solvent (DES) or sodium hypochlorite, centrifugation, filtration, washing and drying.
[0196] 2) Cellulose content: The content of glucose was determined by derivatization with 1-phenyl-3-methyl-5-pyrazolone according to the method of the National Renewable Energy Laboratory of the United States.
[0197] Weigh 0.300 g of the extracted substance. First, decompose it using 72% sulfuric acid at a solid-liquid ratio of 1:10 (g / mL) at 30℃, stirring the solution every five minutes to prevent clumping. Dilute the solution to 4% and autoclave at 121℃ for 1 hour. After vacuum filtration to obtain the supernatant, adjust the pH to 5-6 using calcium carbonate. After precipitation, take 50 μL of the sample solution and add 50 μL of 0.6M sodium hydroxide solution and 100 μL of 0.5M 1-phenyl-3-methyl-5-pyrazolone methanol solution. Seal and heat at 70℃ for 100 minutes, with gentle shaking during the reaction. After the reaction, add 80 μL of 0.3M hydrochloric acid and dilute to 1 mL with deionized water. Add 1 mL of chloroform to the diluted solution and shake vigorously for 1 minute to remove excess 1-phenyl-3-methyl-5-pyrazolone. Repeat this process three times. Measure the cellulose content of the resulting sample solution. The cellulose content of the raw material was determined to be 42.9% using the method of the U.S. National Renewable Energy Laboratory.
[0198] Cellulose content is calculated using the following formula:
[0199] Cellulose content (%) = C_Glu × V × DF × 0.90 / (m × 1000) × 100%
[0200] In the formula, C_Glu is the glucose concentration obtained by derivatization with 1-phenyl-3-methyl-5-pyrazolone and calculated from the standard curve, in mg / mL; V is the total volume of the hydrolysate, in mL; DF is the dilution factor of the sample before detection; 0.90 is the correction factor for converting glucose to anhydrous dextran, i.e., 162 / 180; m is the dry weight of the sample used for hydrolysis determination, in g; and 1000 is the conversion factor between mg and g.
[0201] II. Summary of Results
[0202] Table 1. Solid mass recovery rate and cellulose content of lily stem and leaf cellulose under different extraction conditions (n=3)
[0203]
[0204]
[0205] As shown in Table 1, temperature has the greatest impact on cellulose purity: under the same conditions, as the temperature increases from 90℃ to 150℃, the purity increases from 46.7% to 73.8%, while the recovery rate decreases accordingly; extending the treatment time to 3 hours at high temperature achieves a purity of 83.7% (Example 8); low moisture content (10%) yields the best results. The optimal conditions are 150℃, 3 hours, and 10% moisture content, achieving a purity of 83.7%, which reaches 97.63% after bleaching. Comparative examples show that while the traditional sodium hydroxide method has some extraction effect at 90℃, under conditions of 10% moisture content, 150℃, and 3 hours, the cellulose purity (83.7%) of the choline chloride / malic acid deep eutectic solvent system of this invention is significantly better than that of the sodium hydroxide method (59.1%), and avoids strong alkali corrosion and wastewater problems. The reference results for the newly added eutectic solvents were all uniformly set at 10% water content, 150℃, and 1 hour. The binary system was first formed by pairing choline chloride with a single hydrogen bond donor. The results showed that choline chloride / citric acid, choline chloride / ascorbic acid, and a small number of ternary systems, such as choline chloride / malic acid / propylene glycol and choline chloride / lactic acid / glycerol, have high value for subsequent verification.
[0206] The embodiments of the present invention have been described in detail above with reference to specific examples. However, the present invention is not limited to the above embodiments. Within the scope of knowledge possessed by those skilled in the art, various changes can be made without departing from the spirit of the present invention.
Claims
1. A method for treating lily stems and leaves with a deep eutectic solvent and preparing cellulose, characterized in that, Includes the following steps: (1) The lily stem and leaf waste residue is dried, crushed and sieved to obtain lily stem and leaf waste residue powder; (2) Using hydrogen bond acceptors and hydrogen bond donors as the main raw materials, a deep eutectic solvent was prepared; (3) Mix the powder obtained in step (1) with the deep eutectic solvent obtained in step (2), and heat and stir to extract; (4) Separate the solid residue, wash and dry it to obtain lily stem and leaf cellulose.
2. The method according to claim 1, characterized in that, In step (1), the lily stem and leaf waste residue is the lily stem and leaf residue that has undergone supercritical or subcritical extraction to extract active substances such as polyphenols.
3. The method according to claim 1, characterized in that, In step (2), the hydrogen bond acceptor is choline chloride; the hydrogen bond donor is selected from one or more of lactic acid, citric acid, glycerol, propylene glycol, ethylene glycol, urea, and ascorbic acid. The water content of the deep eutectic solvent is controlled at 10% to 40% (mass fraction, w / w).
4. The method according to claim 1, characterized in that, In step (2), the deep eutectic solvent is a binary deep eutectic solvent formed by pairing choline chloride as a hydrogen bond acceptor with lactic acid, citric acid, glycerol, propylene glycol, ethylene glycol, urea, or ascorbic acid, respectively, wherein the molar ratio of hydrogen bond acceptor to hydrogen bond donor is 1:(1-3); or, the deep eutectic solvent is a ternary deep eutectic solvent of choline chloride / lactic acid / glycerol, choline chloride / malic acid / propylene glycol, or choline chloride / citric acid / glycerol, wherein the molar ratio of hydrogen bond acceptor, hydrogen bond donor, and hydrogen bond donor is 1:(1-3):(1-3).
5. The method according to claim 1, characterized in that, In step (3), the extraction temperature is 90~150℃, the time is 1~3 hours, the stirring speed is 300-900 rpm, and the solid-liquid ratio is 1:(15-25) (g / mL).
6. The method according to claim 1, characterized in that, In step (4), the separation of solid residue is carried out by centrifugation, including: adding a small amount of deionized water to balance the mixture, and centrifuging at 10,000-12,000 rpm for 10-15 minutes. The washing process involves first washing with deionized water until neutral, and then washing with anhydrous ethanol. The drying conditions are: temperature 50-60℃, drying time 12-24 hours.
7. The method according to claim 1, characterized in that, Also includes: Take the lily stem and leaf cellulose obtained in step (4), add sodium hypochlorite solution, heat to react, filter, dry, repeat 2 to 3 times to obtain purified lily stem and leaf cellulose.
8. The method according to claim 7, characterized in that, The sodium hypochlorite solution has a concentration of 0.5-1.5 wt%, a solid-liquid ratio of 1:(25-35) (g / mL), and the heating reaction is carried out at a temperature of 90-100℃ for 0.1-1 hours.
9. A lily stem and leaf cellulose prepared by the method according to any one of claims 1 to 8.