SiCf / siC composite-heterogeneous blade of high-temperature alloy low stress connecting structure and preparation method

By constructing a three-dimensional topological structure and coating a surface functional layer on the inner surface of SiCf/SiC composite blades, and combining femtosecond laser and directional solidification processes, the problem of insufficient interfacial bonding strength in the connection between SiCf/SiC composite materials and high-temperature alloy heterostructure blades was solved, achieving low-stress connection and high reliability.

CN123064529APending Publication Date: 2026-11-10AVIC BEIJING INST OF AERONAUTICAL MATERIALS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611331303.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-31
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing technologies for joining SiCf/SiC composite materials with high-temperature alloy heterostructures suffer from problems such as insufficient interfacial bonding strength, difficulty in controlling local thermal stress, and limited metal melt filling. In particular, it is difficult to achieve low-stress connections on blades with complex curved surfaces.

Method used

A three-dimensional topological structure was constructed on the inner surface of the SiCf/SiC composite blade shell, and a surface functional layer was coated. Combined with femtosecond laser processing and directional solidification, a locking connection was formed between the three-dimensional topological structure and the high-temperature alloy load-bearing skeleton.

Benefits of technology

It effectively controls interfacial thermal damage and stress concentration, improves interfacial bonding reliability, reduces the risk of chemical reactions, adapts to the complex stress state of heterogeneous blades, and is suitable for high-temperature alloy casting with different microstructures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123064529A_ABST
    Figure CN123064529A_ABST
Patent Text Reader

Abstract

This invention discloses a SiC f A low-stress connection structure and fabrication method for SiC composite material-high-temperature alloy heterostructure blades are disclosed. This connection structure is formed by a three-dimensional topological structure, a surface functional layer, and a high-temperature alloy cast into the topological unit. The three-dimensional topological structure is arranged on SiC... f The inner surface of the SiC composite blade shell has a three-dimensional topological structure coated with a surface functional layer. The preparation method includes the following steps: preparing SiC... f / SiC composite material blade shell; using femtosecond laser on SiC f / SiC composite blade shell inner surface is machined with topological units; in SiC f A surface functional layer is coated onto the inner surface of the SiC composite blade shell and the inner surface of the topological unit; a surface functional layer is applied to SiC... f A high-temperature alloy melt is cast into the inner side of the SiC composite blade shell, and directionally solidifies to form a high-temperature alloy load-bearing skeleton. This high-temperature alloy load-bearing skeleton forms a locking connection with the three-dimensional topological structure. This invention can improve the compatibility of heterogeneous interfaces, reduce processing damage and local stress concentration, and improve the reliability of interface interlocking.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of aero-engine composite turbine blade manufacturing technology, specifically relating to a SiC... f Low-stress connection structure and preparation method of SiC composite material-high temperature alloy heterostructure blade. Background Technology

[0002] SiC f SiC composites possess low density and high-temperature resistance, making them ideal for manufacturing aerospace hot-end components. High-temperature alloys (such as nickel-based and cobalt-based alloys) offer excellent high-temperature load-bearing capacity and mature casting processes. Combining these two materials, with the outer SiC layer... f Using SiC composite material as the outer shell of the blade and high-temperature alloy as the load-bearing skeleton in the inner layer, the heterogeneous structure blade can simultaneously exert the dual advantages of high temperature resistance of the material and high load-bearing capacity of the structure.

[0003] However, SiC f SiC composites and high-temperature alloys differ in their thermophysical and chemical properties. On one hand, their coefficients of thermal expansion and elastic moduli differ, making the heterogeneous interface prone to residual stress and localized stress concentration during processing and service temperature changes. On the other hand, alloying elements (such as Ni, Co, and Cr) in the high-temperature alloy melt readily react with SiC at high temperatures. f / SiC composite materials undergo interfacial reactions. Existing methods for joining ceramic and metal materials (such as brazing, diffusion welding, and melt casting) still face technical challenges when dealing with complex curved blade surfaces, including insufficient interfacial bonding strength, difficulty in controlling local thermal stress, and limited metal melt filling.

[0004] Laser surface texturing technology is often used to control the morphology and mechanical interlocking state of material interfaces. Femtosecond lasers, due to their short pulse duration, can achieve micro / nano structure fabrication within a relatively small heat-affected zone. However, in complex curved surfaces like SiC… f In the application of SiC heterostructured blades, if only conventional groove processing is used, the strength of the composite material shell is easily weakened due to the notch effect. At the same time, the matching problem of interfacial reaction isolation and effective filling still needs to be solved during melt casting.

[0005] Therefore, it is necessary to develop a SiC f The low-stress connection structure and preparation method of SiC composite material-high temperature alloy heterostructure blades aim to effectively control interfacial thermal damage, stress concentration and harmful chemical reactions while achieving geometric locking effect. Summary of the Invention

[0006] To address the problems existing in the prior art, the present invention provides a SiC fA low-stress connection structure for SiC composite material-high temperature alloy heterogeneous blades, wherein the blade body region of the heterogeneous blades comprises SiC from the outside to the inside. f / SiC composite material blade shell, heterogeneous connection interface, and high-temperature alloy load-bearing frame; the SiC f The inner surface of the SiC composite blade shell is provided with a three-dimensional topological structure, which is composed of a number of regularly distributed topological units. The surface of the three-dimensional topological structure is coated with a surface functional layer. The heterogeneous connection interface includes the surface functional layer. The low-stress connection structure is formed by the three-dimensional topological structure, the surface functional layer and a high-temperature alloy cast inside the topological units.

[0007] Preferably, the type of the topological unit includes any one of the following: microgroove locking unit, helical tooth locking unit, stepped locking unit, partially tapered locking unit, and dovetail locking unit, and the topological unit has a filling opening for casting high-temperature alloy on the side facing the high-temperature alloy load-bearing skeleton.

[0008] In any of the above embodiments, it is preferred that the topological unit is composed of a bottom region, a sidewall region, and a central cavity region, with the bottom region and the sidewall region smoothly transitioning through rounded corners. The sidewall region includes any one of a straight transition structure, a helical tooth transition structure, a stepped transition structure, an arc transition structure, and a ramp transition structure, with the sharp corners of the helical tooth transition structure and the stepped transition structure smoothly transitioning through rounded corners.

[0009] Preferably, in any of the above embodiments, the flat sidewalls of the microgroove locking unit are perpendicular to the SiC. f The blade casing is made of SiC composite material, and the straight sidewalls of the helical toothed locking unit are perpendicular to the SiC composite material. f / SiC composite material blade shell configuration, oblique tooth sidewalls inclined to the SiC f The blade shell is made of SiC composite material, and the straight sidewall of the stepped locking unit is perpendicular to the SiC. f / SiC composite material blade shell configuration, stepped sidewalls parallel to the SiC f The blade shell is made of SiC composite material, and the flat sidewall of the partially tapered locking unit is perpendicular to the SiC. f / SiC composite material blade shell configuration, with arc-shaped sidewalls inclined to the SiC f The blade shell is made of SiC composite material, and the sloped sidewall of the dovetail locking unit is inclined to the SiC. f / SiC composite blade casing.

[0010] With SiC fThe inner surface of the / SiC composite blade shell is a reference surface. The angle between the helical tooth sidewall and the reference surface is 30-45°, and the angle between the slope sidewall and the reference surface is 45-60°.

[0011] In any of the above embodiments, preferably, the width of the topology unit is the maximum opening width of the topology unit projected onto the heterogeneous connection interface surface, and the depth of the topology unit is the depth of the topology unit centered on SiC. f The inner surface of the / SiC composite blade shell is the maximum depth extending inward from the reference surface. The spacing of the topological units is the distance between the center lines of two adjacent topological units, and the net spacing of the topological units is the shortest distance between the sidewalls of two adjacent topological units.

[0012] In any of the above schemes, it is preferred that the width of the topology unit is defined as W, W=20-500μm; the depth of the topology unit is defined as D, D=(0.1-0.5)W; the spacing of the topology units is defined as P, P=(1.2-1.5)W; and the net spacing of the topology units is defined as S, S=PW.

[0013] In any of the above schemes, it is preferred that the three-dimensional topology is arranged in a gradient along the leaf height direction and / or the leaf circumference in the leaf region.

[0014] For guide vanes: along the blade height direction, the spacing and depth of the topological units gradually increase from the two side edge plates toward the middle of the blade within their control range; along the circumferential direction of the blade, the spacing and depth of the topological units gradually increase from the leading edge to the trailing edge within their control range.

[0015] For the working blade: along the blade height direction, the spacing and depth of the topological units gradually increase from the cusp to the blade tip within their control range; along the blade circumference, the spacing and depth of the topological units gradually increase from the leading edge to the trailing edge within their control range.

[0016] In any of the above embodiments, it is preferred that the high-temperature alloy load-bearing skeleton is made of a nickel-based high-temperature alloy or a cobalt-based high-temperature alloy; the surface functional layer extends along the SiC... f The inner surface of the / SiC composite blade shell and the inner surface of the topological unit are conformally coated, and the thickness of the surface functional layer is 10-50nm.

[0017] The present invention also provides a SiC f A method for preparing a low-stress connection structure for SiC composite material-high temperature alloy heterostructure blades, the method comprising the following steps in sequence: Step 1: Preparation of SiC f / SiC composite material blade shell, and its inner surface is cleaned and dried; Step 2: Following the layout of the three-dimensional topology, femtosecond lasers are used on SiC... f The inner surface of the SiC composite blade shell is machined with topological units, and the inner surface of the topological units is cleaned to remove the debris and slag generated during processing. Step 3: In SiC f A surface functional layer is conformally coated on the inner surface of the blade shell and the inner surface of the topological unit of the SiC composite material. Step 4: Apply SiC with three-dimensional topology and surface functional layers f / SiC composite material blade shell is placed in a heterogeneous blade forming mold; Step 5: Add SiC f High-temperature alloy melt is poured into the inner side of the SiC composite blade shell, and the high-temperature alloy melt is directionally solidified to form a high-temperature alloy load-bearing skeleton. At the same time, the high-temperature alloy load-bearing skeleton forms a locking connection with the three-dimensional topological structure, thus obtaining a low-stress connection structure composed of a three-dimensional topological structure, a surface functional layer, and a high-temperature alloy poured into the topological unit.

[0018] Preferably, in step two, the main process parameters of the femtosecond laser include: pulse width 100-900 fs, single pulse energy 20-100 μJ, repetition frequency 100-500 kHz, scanning speed 100-1000 mm / s, and number of scans 10-100 times. The femtosecond laser processes the topological unit according to a parallel scanning path, a cross scanning path, or an array point scanning path. By controlling the main process parameters of the femtosecond laser, the thickness of the heat-affected zone around the processed three-dimensional topological structure is not greater than 5 μm, the inner surface of the processed SiCf / SiC composite material blade shell does not have continuous processing microcracks with a length greater than 10 μm, and the edge chipping width of the processed three-dimensional topological structure is not greater than 10 μm.

[0019] In any of the above schemes, it is preferred that, in step five, the temperature gradient for directional solidification is 30-100 K / cm and the pulling rate is 1-6 mm / min.

[0020] In this invention, existing technologies can be used to prepare the SiCf / SiC composite blade shell (such as chemical vapor infiltration, precursor impregnation / pyrolysis, melt infiltration, etc.). No special requirements are placed on the specific preparation process and process parameters. Conventional methods can be used for cleaning and drying the inner surface of the SiCf / SiC composite blade shell. Femtosecond laser processing of the topological units is also an existing technology; as long as the main process parameters such as pulse width, single pulse energy, repetition frequency, scanning speed, and number of scans meet the requirements of this invention, it is acceptable.

[0021] The surface functional layer is formed using physical vapor deposition, chemical vapor deposition, atomic layer deposition, slurry coating-sintering, or a combination thereof. During the formation of the surface functional layer, it is applied by rotation, oscillation, impregnation, or multi-directional supply to cover the inner surface of the topological unit. The surface functional layer is used to improve the physicochemical compatibility between the inner surface of the SiCf / SiC composite blade shell and the high-temperature alloy load-bearing skeleton.

[0022] The molding die includes any one of directional solidification molds, ceramic shells, and casting molds. Directional solidification is an existing technology; it is only necessary to ensure that the temperature gradient and pulling rate of directional solidification meet the requirements of this invention.

[0023] The design concept of this invention is to construct a micro-topological structure at the connection interface of the SiCf / SiC composite blade shell, and attach a functional coating to its surface. The metal melt is then used to fill the topological space through casting or directional solidification, and a locking is formed after solidification. The specific implementation logic is as follows: (1) The topological unit is processed by femtosecond laser. The small heat input of ultrafast laser processing is used to control the heat-affected zone and the scale of the microcracks. (2) The topological unit introduces rounded corners for smooth transition, which alleviates stress concentration at sharp corners. At the same time, it is combined with limiting structures such as inclined sidewalls to provide shear and peel resistance. (3) A gradient distribution design is adopted to reduce the topological depth and area ratio in the transition area of ​​the blade with high load to retain the matrix wall thickness. The topological depth is appropriately increased in the middle of the blade to provide sufficient interlocking area. (4) A surface functional layer is introduced to isolate the ceramic matrix and the high-temperature alloy melt, and to assist in controlling the interface reaction and filling and wetting process during solidification, ultimately forming a physical and geometric synergistic connection between heterogeneous materials.

[0024] This invention SiC f The low-stress connection structure and preparation method of SiC composite material-high temperature alloy heterostructure blades have the following beneficial effects: (1) The present invention uses femtosecond laser to construct a three-dimensional topological structure and limits the range of its geometric parameters such as width, depth and spacing. While providing space for melt filling, it helps to control processing thermal damage and microcracks, and reduces the weakening of the bulk strength of SiCf / SiC composite material.

[0025] (2) The topological unit designed in this invention provides mechanical locking in a geometric interlocking manner, which can effectively share the shear and peel loads borne by the interface. Combined with the introduction of rounded corners and gentle slopes, it helps to reduce local stress concentration caused by abrupt changes in geometric shape.

[0026] (3) The topological parameters of the present invention are designed with gradient distribution along the leaf height direction and / or the leaf circumference, which can adapt to the complex stress state of different regions of heterogeneous blades and achieve a reasonable match between the local connection area and the matrix wall thickness retention rate.

[0027] (4) The surface functional layer set on the topological surface in this invention can play a blocking or wetting role, reduce the risk of direct chemical corrosion of the ceramic matrix by high temperature metal melt, and improve the melt filling state.

[0028] (5) The preparation process of the low-stress connection structure of the present invention has good system compatibility, can be adapted to various surface deposition technologies, and is applicable to the casting and forming of high-temperature alloys with different microstructures such as single crystal, columnar crystal and equiaxed crystal.

[0029] (6) The technical solution of the present invention can improve the compatibility of heterogeneous interfaces, reduce processing damage and local stress concentration, and improve the reliability of interface fitting. Attached Figure Description

[0030] Figure 1 According to the present invention, SiC f A comparison diagram of the types of topological units in a preferred embodiment of the low-stress connection structure and preparation method of / SiC composite material-high temperature alloy heterostructure blade, wherein: (a) microgroove locking unit, (b) helical tooth locking unit, (c) stepped locking unit, (d) partially constricted locking unit, (e) dovetail locking unit. Figure 2 for Figure 1 A schematic diagram illustrating the definition of geometric parameters of the topological unit in the illustrated embodiment. Detailed Implementation

[0031] To further understand the invention, the following detailed description of the invention will be provided in conjunction with specific embodiments.

[0032] Example 1: According to the present invention, SiC f A preferred embodiment of the low-stress connection structure of the SiC composite material-high temperature alloy heterogeneous blade, wherein the blade body region of the heterogeneous blade comprises SiC from the outside to the inside. f / SiC composite material blade shell, heterogeneous connection interface, and high-temperature alloy load-bearing frame; the SiC f The inner surface of the SiC composite blade shell is provided with a three-dimensional topological structure, which is composed of a number of regularly distributed topological units. The surface of the three-dimensional topological structure is coated with a surface functional layer. The heterogeneous connection interface includes the surface functional layer. The low-stress connection structure is formed by the three-dimensional topological structure, the surface functional layer and a high-temperature alloy cast inside the topological units.

[0033] like Figure 1As shown, the type of the topological unit includes any one of the following: microgroove locking unit, helical tooth locking unit, stepped locking unit, partially tapered locking unit, and dovetail locking unit. The topological unit has a filling opening for casting high-temperature alloy on the side facing the high-temperature alloy load-bearing skeleton.

[0034] In this embodiment, the type of topological unit is a microgroove locking unit. The topological unit consists of a bottom region, a sidewall region, and a central cavity region. The bottom region and the sidewall region are smoothly transitioned by rounded corners. The sidewall region has a straight transition structure, and its straight sidewalls are perpendicular to the SiC. f / SiC composite blade casing.

[0035] The width of the topological unit is the maximum opening width of the topological unit projected onto the heterogeneous connection interface surface, and the depth of the topological unit is the depth of the topological unit centered on SiC. f The inner surface of the / SiC composite blade shell is the maximum depth extending inward from the reference surface. The spacing of the topological units is the distance between the center lines of two adjacent topological units, and the net spacing of the topological units is the shortest distance between the sidewalls of two adjacent topological units.

[0036] like Figure 2 As shown, in this embodiment, the width of the topology unit is defined as W, W=260μm; the depth of the topology unit is defined as D, D=(0.1-0.5)W=26-130μm; the spacing of the topology units is defined as P, P=(1.2-1.5)W=312-390μm; and the net spacing of the topology units is defined as S, S=PW=52-130μm.

[0037] The three-dimensional topology is arranged in a gradient along the leaf height direction and / or the leaf circumference in the leaf region.

[0038] For guide vanes: along the blade height direction, the spacing and depth of the topological units gradually increase from the two side edge plates toward the middle of the blade within their control range; along the circumferential direction of the blade, the spacing and depth of the topological units gradually increase from the leading edge to the trailing edge within their control range.

[0039] For the working blade: along the blade height direction, the spacing and depth of the topological units gradually increase from the cusp to the blade tip within their control range; along the blade circumference, the spacing and depth of the topological units gradually increase from the leading edge to the trailing edge within their control range.

[0040] The high-temperature alloy load-bearing frame is made of a nickel-based high-temperature alloy; the surface functional layer runs along the SiC... fThe inner surface of the / SiC composite blade shell and the inner surface of the topological unit are conformally coated, and the thickness of the surface functional layer is 30nm.

[0041] This embodiment also provides a SiC f A method for preparing a low-stress connection structure for SiC composite material-high temperature alloy heterostructure blades, the method comprising the following steps in sequence: Step 1: Preparation of SiC f / SiC composite material blade shell, and its inner surface is cleaned and dried; Step 2: Following the layout of the three-dimensional topology, femtosecond lasers are used on SiC... f The inner surface of the SiC composite blade shell is machined with topological units, and the inner surface of the topological units is cleaned to remove the debris and slag generated during processing. Step 3: In SiC f A surface functional layer is conformally coated on the inner surface of the blade shell and the inner surface of the topological unit of the SiC composite material. Step 4: Apply SiC with three-dimensional topology and surface functional layers f / SiC composite material blade shell is placed in a heterogeneous blade forming mold; Step 5: Add SiC f High-temperature alloy melt is poured into the inner side of the SiC composite blade shell, and the high-temperature alloy melt is directionally solidified to form a high-temperature alloy load-bearing skeleton. At the same time, the high-temperature alloy load-bearing skeleton forms a locking connection with the three-dimensional topological structure, thus obtaining a low-stress connection structure composed of a three-dimensional topological structure, a surface functional layer, and a high-temperature alloy poured into the topological unit.

[0042] In step two, the main process parameters of the femtosecond laser include: pulse width 500 fs, single pulse energy 60 μJ, repetition frequency 300 kHz, scanning speed 550 mm / s, and 55 scans. The femtosecond laser processes the topological unit according to the parallel scanning path, cross scanning path, or array point scanning path. By controlling the main process parameters of the femtosecond laser, the thickness of the heat-affected zone around the processed three-dimensional topological structure is not greater than 5 μm, the inner surface of the processed SiCf / SiC composite material blade shell is free of continuous microcracks with a length greater than 10 μm, and the edge chipping width of the processed three-dimensional topological structure is not greater than 10 μm.

[0043] In step five, the temperature gradient for directional solidification is 65 K / cm and the pulling rate is 3.5 mm / min.

[0044] In this embodiment, the preparation of the SiCf / SiC composite blade shell (such as chemical vapor infiltration, precursor impregnation / pyrolysis, melt infiltration, etc.) can be carried out using existing technologies. No special requirements are placed on the specific preparation process and parameters. The cleaning and drying of the inner surface of the SiCf / SiC composite blade shell can be performed using conventional methods. The surface functional layer is formed using physical vapor deposition, chemical vapor deposition, atomic layer deposition, slurry coating-sintering, or a combination thereof. During the formation of the surface functional layer, the surface functional layer covers the inner surface of the topological unit through rotation, oscillation, impregnation, or multi-directional supply. The molding die includes any one of directional solidification molds, ceramic shell molds, and casting molds.

[0045] This embodiment has the following beneficial effects: (1) A three-dimensional topological structure is constructed using a femtosecond laser, and its geometric parameters such as width, depth, and spacing are limited within a certain range. While providing space for melt filling, it helps to control processing heat damage and microcracks, and reduces the weakening of the bulk strength of SiCf / SiC composite material. (2) The topological unit provides mechanical locking in a geometric interlocking manner, which can effectively share the shear and peel loads borne by the interface. Combined with the introduction of rounded corners and gentle slopes, it helps to reduce local stress concentration caused by abrupt changes in geometric morphology. (3) The topological parameters are distributed in a gradient along the blade height direction and / or the blade circumferential direction, which can adapt to the complex stress state of different regions of heterogeneous blades and achieve a reasonable match between the local connection area and the matrix wall thickness retention rate. (4) The surface functional layer set on the topological surface can play a barrier or wetting role, reduce the risk of direct chemical erosion of the ceramic matrix by high-temperature metal melt, and improve the melt filling state. (5) The connection structure preparation process has good system compatibility, can be adapted to various surface deposition technologies, and is suitable for high-temperature alloy casting with different microstructures. (6) It can improve the compatibility of heterogeneous interfaces, reduce processing damage and local stress concentration, and improve the reliability of interface mating.

[0046] Example 2: According to the present invention, SiC f Another preferred embodiment of the low-stress connection structure and preparation method of SiC composite material-high temperature alloy heterostructure blades is basically the same as that of Embodiment 1 in terms of structural composition, preparation method and beneficial effects, except that: In this embodiment, the topological unit is a helical tooth locking unit. The topological unit consists of a bottom region, a sidewall region, and a central cavity region. The bottom region and the sidewall region are smoothly transitioned by rounded corners. The straight sidewalls of the helical tooth locking unit are perpendicular to the SiCf / SiC composite blade shell, while the helical tooth sidewalls are inclined to the SiCf / SiC composite blade shell. Using the inner surface of the SiCf / SiC composite blade shell as a reference plane, the angle between the helical tooth sidewalls and this reference plane is 45°.

[0047] In this embodiment, the width of the topological unit is defined as W, where W = 100 μm; the depth of the topological unit is defined as D, where D = (0.1-0.5)W = 10-50 μm; the spacing between the topological units is defined as P, where P = (1.2-1.5)W = 120-150 μm; and the net spacing between the topological units is defined as S, where S = PW = 20-50 μm. The high-temperature alloy load-bearing skeleton is made of cobalt-based high-temperature alloy; and the thickness of the surface functional layer is 10 nm.

[0048] In step two, the main process parameters for the femtosecond laser include: pulse width 100 fs, single pulse energy 20 μJ, repetition rate 100 kHz, scanning speed 100 mm / s, and 10 scans. In step five, the temperature gradient for directional solidification is 30 K / cm, and the pulling rate is 1 mm / min.

[0049] Example 3: According to the present invention, SiC f Another preferred embodiment of the low-stress connection structure and preparation method of SiC composite material-high temperature alloy heterostructure blades is basically the same as that of Embodiment 1 in terms of structural composition, preparation method and beneficial effects, except that: In this embodiment, the topological unit is a dovetail locking unit. The topological unit consists of a bottom region, a sidewall region, and a central cavity region. The bottom region and the sidewall region are smoothly transitioned by rounded corners. The sloping sidewall of the dovetail locking unit is inclined to the outer shell of the SiCf / SiC composite blade. Using the inner surface of the SiCf / SiC composite blade outer shell as a reference plane, the angle between the sloping sidewall and this reference plane is 60°.

[0050] In this embodiment, the width of the topological unit is defined as W, where W = 500 μm; the depth of the topological unit is defined as D, where D = (0.1-0.5)W = 50-250 μm; the spacing of the topological units is defined as P, where P = (1.2-1.5)W = 600-750 μm; and the net spacing of the topological units is defined as S, where S = PW = 100-250 μm. The high-temperature alloy load-bearing skeleton is made of cobalt-based high-temperature alloy; and the thickness of the surface functional layer is 50 nm.

[0051] In step two, the main process parameters for the femtosecond laser include: pulse width 900 fs, single pulse energy 100 μJ, repetition rate 500 kHz, scanning speed 1000 mm / s, and 100 scans. In step five, the temperature gradient for directional solidification is 100 K / cm, and the pulling rate is 6 mm / min.

[0052] The above three embodiments were tested, and the test results are shown in Table 1.

[0053]

[0054] The test results above show that, through the synergistic effect of three-dimensional topological gradient distribution design, topological unit geometric parameter limitation, surface functional layer and high-temperature alloy load-bearing skeleton geometric integration, the three embodiments can improve the reliability of interface integration while reducing local stress concentration at the heterogeneous connection interface.

[0055] Special Note: The technical solution of this invention involves numerous parameters, and the synergistic effects between these parameters must be comprehensively considered to achieve the beneficial effects and significant progress of this invention. Furthermore, the value ranges of each parameter in the technical solution were obtained through extensive experimentation. For each parameter and the combinations thereof, the inventors have recorded a large amount of experimental data; however, due to space limitations, the specific experimental data is not disclosed here.

[0056] It will be readily understood by those skilled in the art that this invention includes any combination of the inventive description and specific embodiments outlined in the foregoing specification, as well as the various parts shown in the accompanying drawings. Due to space limitations and for the sake of brevity, not all of these combinations have been described in detail. Any modifications, equivalent substitutions, or improvements made within the spirit and principles of this invention should be included within the scope of protection of this invention.

Claims

1. A SiC f The low-stress connection structure of SiC composite material-high temperature alloy heterostructure blades is characterized by... The blade region of the heterogeneous blade, from the outside in, includes SiC... f / SiC composite material blade shell, heterogeneous connection interface, and high-temperature alloy load-bearing frame; the SiC f The inner surface of the SiC composite blade shell is provided with a three-dimensional topological structure, which is composed of a number of regularly distributed topological units. The surface of the three-dimensional topological structure is coated with a surface functional layer. The heterogeneous connection interface includes the surface functional layer. The low-stress connection structure is formed by the three-dimensional topological structure, the surface functional layer and a high-temperature alloy cast inside the topological units.

2. The SiC according to claim 1 f The low-stress connection structure of SiC composite material-high temperature alloy heterostructure blades is characterized by... The type of the topological unit includes any one of the following: microgroove locking unit, helical tooth locking unit, stepped locking unit, partially tapered locking unit, and dovetail locking unit. The topological unit has a filling opening for casting high-temperature alloy on the side facing the high-temperature alloy load-bearing skeleton.

3. The SiC according to claim 2 f The low-stress connection structure of SiC composite material-high temperature alloy heterostructure blades is characterized by... The topological unit consists of a bottom region, a sidewall region, and a central cavity region. The bottom region and the sidewall region are smoothly transitioned by rounded corners. The sidewall region includes any one of a straight transition structure, a helical tooth transition structure, a stepped transition structure, an arc transition structure, and a ramp transition structure. The sharp corners of the helical tooth transition structure and the stepped transition structure are smoothly transitioned by rounded corners.

4. The SiC according to claim 3 f The low-stress connection structure of SiC composite material-high temperature alloy heterostructure blades is characterized by... The flat sidewalls of the microgroove locking unit are perpendicular to the SiC. f The blade casing is made of SiC composite material, and the straight sidewalls of the helical toothed locking unit are perpendicular to the SiC. f / SiC composite material blade shell configuration, oblique tooth sidewalls inclined to the SiC f The blade shell is made of SiC composite material, and the straight sidewall of the stepped locking unit is perpendicular to the SiC. f / SiC composite material blade shell configuration, stepped sidewalls parallel to the SiC f The blade shell is made of SiC composite material, and the flat sidewall of the partially tapered locking unit is perpendicular to the SiC. f / SiC composite material blade shell configuration, with arc-shaped sidewalls inclined to the SiC f The blade shell is made of SiC composite material, and the sloped sidewall of the dovetail locking unit is inclined to the SiC. f / SiC composite material blade casing; With SiC f The inner surface of the / SiC composite blade shell is a reference surface. The angle between the helical tooth sidewall and the reference surface is 30-45°, and the angle between the slope sidewall and the reference surface is 45-60°.

5. The SiC according to claim 4 f The low-stress connection structure of SiC composite material-high temperature alloy heterostructure blades is characterized by... The width of the topological unit is the maximum opening width of the topological unit projected onto the heterogeneous connection interface surface, and the depth of the topological unit is the depth of the topological unit centered on SiC. f The inner surface of the / SiC composite blade shell is the maximum depth extending inward from the reference surface. The spacing of the topological units is the distance between the center lines of two adjacent topological units, and the net spacing of the topological units is the shortest distance between the sidewalls of two adjacent topological units.

6. The SiC according to claim 5 f The low-stress connection structure of SiC composite material-high temperature alloy heterostructure blades is characterized by... The width of the topological unit is defined as W, where W = 20-500 μm; the depth of the topological unit is defined as D, where D = (0.1-0.5) W; the spacing between the topological units is defined as P, where P = (1.2-1.5) W; and the net spacing between the topological units is defined as S, where S = PW.

7. The SiC according to claim 6 f The low-stress connection structure of SiC composite material-high temperature alloy heterostructure blades is characterized by... The three-dimensional topological structure is arranged in a gradient along the leaf height direction and / or the leaf circumference in the leaf region; For guide vanes: along the blade height direction, the spacing and depth of the topological units gradually increase from the two side edge plates toward the middle of the blade within their control range; along the circumferential direction of the blade, the spacing and depth of the topological units gradually increase from the leading edge to the trailing edge within their control range. For the working blade: along the blade height direction, the spacing and depth of the topological units gradually increase from the cusp to the blade tip within their control range; along the blade circumference, the spacing and depth of the topological units gradually increase from the leading edge to the trailing edge within their control range.

8. The SiC according to claim 7 f The low-stress connection structure of SiC composite material-high temperature alloy heterostructure blades is characterized by... The high-temperature alloy load-bearing frame is made of nickel-based or cobalt-based high-temperature alloy; the surface functional layer runs along the SiC... f The inner surface of the / SiC composite blade shell and the inner surface of the topological unit are conformally coated, and the thickness of the surface functional layer is 10-50nm.

9. A SiC according to any one of claims 1-8 f A method for preparing a low-stress connection structure for SiC composite material-high-temperature alloy heterostructure blades, characterized in that... The preparation method includes the following steps in sequence: Step 1: Preparation of SiC f / SiC composite material blade shell, and its inner surface is cleaned and dried; Step 2: Following the layout of the three-dimensional topology, femtosecond lasers are used on SiC... f The inner surface of the SiC composite blade shell is machined with topological units, and the inner surface of the topological units is cleaned to remove the debris and slag generated during processing. Step 3: In SiC f A surface functional layer is conformally coated on the inner surface of the blade shell and the inner surface of the topological unit of the SiC composite material. Step 4: Apply SiC with three-dimensional topology and surface functional layers f / SiC composite material blade shell is placed in a heterogeneous blade forming mold; Step 5: Add SiC f High-temperature alloy melt is poured into the inner side of the SiC composite blade shell, and the high-temperature alloy melt is directionally solidified to form a high-temperature alloy load-bearing skeleton. At the same time, the high-temperature alloy load-bearing skeleton forms a locking connection with the three-dimensional topological structure, thus obtaining a low-stress connection structure composed of a three-dimensional topological structure, a surface functional layer, and a high-temperature alloy poured into the topological unit.

10. The SiC according to claim 9 f A method for preparing a low-stress connection structure for SiC composite material-high-temperature alloy heterostructure blades, characterized in that... In step two, the main process parameters of the femtosecond laser include: pulse width 100-900 fs, single pulse energy 20-100 μJ, repetition frequency 100-500 kHz, scanning speed 100-1000 mm / s, and number of scans 10-100 times. The femtosecond laser processes the topological units according to parallel scanning path, cross scanning path, or array point scanning path. By controlling the main process parameters of the femtosecond laser, the thickness of the heat-affected zone around the processed three-dimensional topological structure is not greater than 5 μm, the inner surface of the processed SiCf / SiC composite material blade shell is free of continuous processing microcracks with a length greater than 10 μm, and the edge chipping width of the processed three-dimensional topological structure is not greater than 10 μm. In step five, the temperature gradient for directional solidification is 30-100 K / cm, and the pulling rate is 1-6 mm / min.