A high-power, high-vacuum suspension melting and purification equipment and melting method
By using high-power high-vacuum suspension melting equipment and methods, the problems of discharge under high vacuum and removal of gaseous impurities have been solved, enabling the preparation of high-purity alloys. This method is applicable to the melting of various high-purity metals and alloys.
Patent Information
- Application Number
- CN202611449837.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-17
- Publication Date
- 2026-11-10
AI Technical Summary
Existing metal smelting technologies are difficult to achieve high-power smelting in a high-vacuum environment, pose a risk of discharge, have limited ability to remove gas impurities, produce uneven molten pool temperatures, and have secondary pollution problems, making it difficult to prepare high-purity alloys.
The equipment employs a high-power, high-vacuum suspension melting system, including a vacuum system, a heating system, a melting system, and a cooling system. It utilizes induction coils and segmented water-cooled copper crucibles to achieve suspension melting. Impurities are removed through a combination of electromagnetic stirring and multi-stage vacuum pumps. Dual-frequency coils control the temperature of the molten pool, and a condensation pump group is configured to thoroughly remove residual gases.
It achieves deep coupling of high vacuum and high power, significantly reduces the content of gas impurities, avoids crucible contamination and temperature unevenness, and improves material purity and composition uniformity, making it suitable for smelting a variety of high-purity metals and alloys.
Smart Images

Figure CN123065231A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of metal material smelting and purification technology, and in particular to a suspension smelting and purification equipment and smelting method. Background Technology
[0002] High-purity and ultra-pure metals and alloys are key basic materials for strategic industries such as aerospace, semiconductors, and high-end sputtering targets. With the increasing demands for material purity in these fields, metal smelting and purification technologies face ever-growing challenges. Currently, metal smelting and purification mainly employs technologies such as vacuum induction melting, cold crucible levitation melting, and vacuum arc melting. Vacuum induction melting is a widely used advanced melting technology that heats the molten material through electromagnetic induction. The vacuum environment eliminates atmospheric contamination of the molten material, enabling the production of high-purity alloy products. However, traditional vacuum induction melting still requires the use of oxide crucibles (such as zirconium oxide, alumina, and magnesium oxide ceramics). During the high-temperature melting process, the crucible material can contaminate the molten metal, making it difficult to avoid the introduction of impurities such as C, O, Fe, and Si. This is particularly unsuitable for melting reactive metals such as titanium alloys and zirconium alloys, as well as high-melting-point refractory alloys such as tungsten, molybdenum, niobium, and tantalum. To overcome the crucible contamination problem, electromagnetic levitation melting technology (also known as cold crucible vacuum induction melting) has emerged. This technology utilizes a segmented water-cooled copper crucible, which uses an electromagnetic field to keep the molten raw materials in a suspended or quasi-suspended state during the melting process. This avoids contamination of the melt by the crucible material and has technical advantages such as no crucible material contamination, high melting temperature, and strong electromagnetic stirring ability.
[0003] However, the existing technology still has the following technical problems that urgently need to be solved: (i) It is difficult to achieve both high vacuum and high power simultaneously. High vacuum environment (vacuum degree not exceeding 6.67 × 10⁻⁶) -3 At pressures below a certain level (Pa), electromagnetic fields are highly susceptible to discharge, posing a significant industry-wide challenge in vacuum induction melting. To address this discharge issue, existing equipment typically requires either reducing input power or relaxing vacuum requirements, making it impossible to simultaneously achieve high vacuum and high-power melting. Currently, conventional vacuum induction melting equipment typically operates at 300-500kW power levels, making it difficult to stably operate at higher power levels under higher vacuum conditions. This inherent contradiction severely restricts the simultaneous improvement of melting and purification efficiency and quality.
[0004] (ii) Limited ability to remove gaseous impurities. In the smelting process of high-purity metals and alloys, gaseous impurities such as hydrogen, oxygen, and nitrogen are key factors affecting the plasticity, toughness, and fatigue life of materials. For materials that are sensitive to gases, such as titanium alloys and high-temperature alloys, traditional smelting methods are unable to effectively reduce the oxygen content to a low level, and controlling the hydrogen content is even more difficult.
[0005] (iii) Insufficient removal efficiency of harmful impurities. The removal of low-melting-point metallic impurities and non-metallic inclusions depends on the convection and mass transfer of the molten pool. The electromagnetic stirring intensity of existing equipment is limited, making it difficult to form sufficiently strong convection inside the molten pool. This results in low efficiency of volatilization, decomposition, and flotation of harmful impurities, which restricts further improvement of material purity.
[0006] (iv) Secondary pollution and temperature unevenness exist in the smelting process. In traditional vacuum induction melting, the crucible material releases impurities into the melt at high temperatures. At the same time, existing single-frequency induction heating, when melting large scales, results in a large longitudinal temperature gradient in the molten pool, with the surface layer prone to overheating and the bottom temperature too low, affecting the compositional uniformity of refractory alloys. In addition, traditional methods typically use oil diffusion pumps to obtain the vacuum environment required for melting, which may backflow trace amounts of hydrocarbon gases into the furnace at high temperatures, causing secondary carbon and hydrogen pollution to the active metal melt.
[0007] In summary, there is currently no integrated technical solution that can simultaneously achieve high power input, high vacuum environment, non-contact levitation melting, ultra-high vacuum deep degassing, and precise temperature field control. Summary of the Invention
[0008] The purpose of this invention is to provide a high-power, high-vacuum suspension melting and purification equipment and melting method, which can at least solve the technical problem of the difficulty in achieving both high vacuum and high power.
[0009] According to a first aspect of the present invention, a high-power high-vacuum suspension melting and purification device is provided, which includes a vacuum system, a heating system, a melting system and a cooling system; The vacuum system includes a vacuum furnace chamber and a vacuum pumping unit, wherein the vacuum furnace chamber is connected to the vacuum pumping unit. The heating system includes an induction power supply, a coaxial water-cooled electrode, and an induction coil, which are connected in sequence, and the induction coil is located inside the vacuum furnace chamber. The smelting system includes a segmented water-cooled copper crucible and a crucible tilting mechanism. The segmented water-cooled copper crucible is located in a vacuum furnace chamber, and the segments of the segmented water-cooled copper crucible are insulated from each other. The crucible tilting mechanism is used to drive the segmented water-cooled copper crucible to tilt and pour out the melt. The cooling system is used to supply cooling water to the coaxial water-cooled electrode and the segmented water-cooled copper crucible; An insulator is provided on the outside of the induction coil. One end of the induction coil is connected to a fixing member, and the other end of the fixing member is recessed into the insulator. The outer side of the conductor of the induction coil is sequentially covered with an insulating varnish layer, a polyimide film layer, a mica tape layer, and a glass fiber tape layer.
[0010] According to the high-power high-vacuum suspension melting and purification equipment, the induction coil has an upper heat preservation coil and a lower main heating coil that can be controlled separately, and the upper heat preservation coil and the lower main heating coil are isolated by a high-voltage resistant insulating partition.
[0011] According to the high-power high-vacuum suspension melting and purification equipment, the vacuum pumping unit includes a rotary vane pump, a Roots pump, a first fore-stage valve, a magnetic levitation molecular pump, a first vacuum valve, and a roughing valve. The rotary vane pump, Roots pump, first fore-stage valve, magnetic levitation molecular pump, first vacuum valve, and vacuum furnace are connected in series. The roughing valve is connected in parallel between the inlet of the first vacuum valve and the outlet of the first fore-stage valve.
[0012] According to the high-power high-vacuum suspension melting and purification equipment, the vacuum system further includes a condenser pump group connected in parallel with the vacuum pumping unit. The condenser pump group includes a dry mechanical pump, a second fore-stage valve, a cryogenic condenser pump, and a second vacuum valve. The dry mechanical pump, the second fore-stage valve, the cryogenic condenser pump, the second vacuum valve, and the vacuum furnace chamber are connected in series. A water-cooled metal vapor condenser plate is installed on one side of the vacuum chamber of the second vacuum valve.
[0013] According to the high-power high-vacuum suspension melting and purification equipment, the rated power of the induction power supply is greater than 800KW and the rated voltage is less than 500V; the inner diameter of the segmented water-cooled copper crucible is greater than 108mm.
[0014] According to the high-power high-vacuum suspension melting and purification equipment, the segments of the segmented water-cooled copper crucible are arranged at intervals, and corundum sheets are filled between the segments of the segmented water-cooled copper crucible.
[0015] According to a second aspect of the present invention, a suspension melting and purification method based on the above-mentioned high-power high-vacuum suspension melting and purification equipment is provided, comprising: S1. Charging: Load the raw materials to be smelted into the segmented water-cooled copper crucible and close the vacuum furnace chamber; S2. Vacuuming: Start the vacuum pumping unit to evacuate the vacuum furnace chamber, so that the vacuum degree of the vacuum furnace chamber does not exceed 6.67×10-3 Pa; S3. Electro-melting: Start the induction power supply. The electromagnetic field generated by the induction coil penetrates the segmented water-cooled copper crucible and heats the raw materials. Under the action of electromagnetic force, the raw materials melt to form a melt and the melt is in a suspended state. S4. High-vacuum refining: The melt is refined by electromagnetic stirring for 10-120 minutes to remove impurities; and the vacuum degree in the vacuum furnace is controlled to be no higher than 0.01 Pa. S5. Casting: The molten material is poured into the mold. S6. Cooling and Removal: The melt is cooled into a casting under vacuum or protective atmosphere, and the casting is removed from the vacuum furnace chamber.
[0016] According to the suspension melting and purification method described above, in step S3, the electromagnetic field generated by energizing the induction coil penetrates the segmented water-cooled copper crucible to heat the raw material, and the raw material melts under the action of electromagnetic force to form a melt, including: The induction coil is energized with a preset initial power to preheat the raw materials; The induction coil gradually increases its power until all the raw material is melted; and when all the raw material is melted, it increases its power to the first level. In step S4, the induction coil is energized with a second power, and the second power is not less than the first power.
[0017] According to the suspension melting and purification method, in step S4, the lower main heating coil uses a preset constant power, the upper heat preservation coil uses a variable power, and the longitudinal temperature difference of the molten pool is not greater than 50°C; and the frequency of the upper heat preservation coil is less than the frequency of the lower main heating coil.
[0018] According to the suspension melting and purification method, the vacuum system further includes a condenser pump group, which includes a dry mechanical pump, a second fore-stage valve, a cryogenic condenser pump, and a second vacuum valve. The dry mechanical pump, the second fore-stage valve, the cryogenic condenser pump, the second vacuum valve, and the vacuum furnace chamber are connected in series. In step S2, after starting the vacuum pumping unit to evacuate the vacuum furnace chamber, the process also includes: closing the second vacuum valve, starting the dry mechanical pump, opening the second fore-stage valve to evacuate the cryogenic condenser pump, closing the second fore-stage valve when the vacuum level inside the cryogenic condenser pump is lower than 40 Pa, starting the cryogenic condenser pump, and cooling the pump to 20 K. In step S4, 3-30 minutes before the end of high vacuum refining, the second vacuum valve is opened to purge residual gas from the vacuum furnace chamber until the high vacuum refining is completed.
[0019] Beneficial effects: (1) Significant effect in removing gaseous impurities: Under high vacuum (not higher than 6.67×10⁻⁶), - Melting under conditions of 3Pa can significantly reduce the content of gases such as hydrogen, oxygen, and nitrogen in the molten pool; for gas-sensitive materials such as titanium alloys and high-temperature alloys, the oxygen content can be reduced to no more than 300ppm and the hydrogen content to no more than 10ppm. When using an oil-free molecular pump solution, the hydrogen content can be further stably controlled to no more than 3ppm. (2) The purity of materials is greatly improved: the strong electromagnetic stirring effect generated by the high-power oscillating current of the induction coil accelerates the volatilization, decomposition and floating of harmful impurities (such as low melting point metals and non-metallic inclusions); for rare earth metals, high-purity copper, high-purity nickel and other materials, the purity can be improved to 4N-5N level. (3) Eliminate secondary pollution: The electromagnetic field is used to make the molten pool suspended, avoiding the contamination of the melt by the crucible material; for active metals such as titanium, zirconium, and rare earth and ultrapure materials, the introduction of crucible impurities (C, O, Fe, Si, etc.) in traditional smelting methods can be avoided; it can be combined with an oil-free magnetic levitation molecular pump scheme to further eliminate C and H pollution caused by oil vapor. (4) High vacuum and high power are achieved simultaneously: Through the low voltage anti-discharge design, the industry problem of easy discharge of electromagnetic field under high vacuum conditions is solved, and the deep coupling of high vacuum and high power is realized, so that high power electromagnetic stirring purification and high vacuum degassing can be carried out simultaneously, producing a significant synergistic effect. (5) The temperature field of the molten pool is finely controlled and has strong adaptability to large sizes: When the dual-frequency control structure of the coil is adopted, the upper low-frequency coil and the lower high-frequency coil work together to control the longitudinal temperature difference of the molten pool within ≤50℃, effectively avoiding surface overheating and bottom refractory metal deposition, which is especially suitable for the preparation of large-size ingots of 150kg and above. (6) Wide range of applications greatly expanded: The basic scheme of this invention (without condenser pump set and separately controlled upper heat preservation coil and lower main heating coil) can be widely used in the smelting and purification of titanium alloys, high-temperature alloys, rare earth metals, high-purity copper, high-purity nickel, high-purity aluminum and refractory metals; the advanced scheme (with condenser pump set and separately controlled upper heat preservation coil and lower main heating coil) can be even more capable of preparing materials with extremely demanding requirements such as semiconductor-grade ultra-high purity materials (5N grade and above), low-gap element high-temperature alloys, and high-end sputtering targets.
[0020] Additional aspects and advantages of the invention will be set forth in part in the description which follows, and in part will be obvious from the description, or may be learned by practice of the invention. Attached Figure Description
[0021] The present invention will be further described below with reference to the accompanying drawings and embodiments: Figure 1 This is a schematic diagram of the overall structure of the high-power high-vacuum suspension melting and purification equipment of the present invention; Figure 2 This is a schematic diagram of the layout of a vacuum system; Figure 3 This is a schematic diagram illustrating the assembly relationship between the segmented water-cooled copper crucible and the induction coil, as well as the suspension melting state of the present invention. Figure 4 This is a schematic cross-sectional view of the induction coil of the present invention; Figure 5 This is a process flow diagram of the suspension melting and purification method of the present invention; Figure 6 This is a bar chart comparing the oxygen and hydrogen content of the titanium alloy (Ti-6Al-4V) before and after smelting and purification in Example 1 of the present invention. Figure 7 This refers to the gas content after high-purity nickel smelting and purification in Embodiment 2 of the present invention. Detailed Implementation
[0022] This section will describe in detail specific embodiments of the present invention. Preferred embodiments of the present invention are shown in the accompanying drawings. The purpose of the drawings is to supplement the textual description with graphics, so that people can intuitively and vividly understand each technical feature and overall technical solution of the present invention, but they should not be construed as limiting the scope of protection of the present invention.
[0023] Reference Figure 1-4 This invention discloses a high-power, high-vacuum suspension melting and purification device, comprising a vacuum system 10, a heating system 20, a melting system 30, a cooling system 40, and a control system 50. The vacuum system 10 includes a vacuum furnace chamber 11, a vacuum pump unit 12, and a measuring device 14. The vacuum furnace chamber 11 and the vacuum pump unit 12 are connected; the measuring device 14 is connected to the vacuum furnace chamber 11 and is used to measure the pressure inside the vacuum furnace chamber 11.
[0024] The heating system 20 includes an induction power supply 21, a coaxial water-cooled electrode 22, and an induction coil 23. The induction power supply 21, coaxial water-cooled electrode 22, and induction coil 23 are connected. The induction power supply 21 is located outside the vacuum furnace chamber 11, the coaxial water-cooled electrode 22 is movably inserted through the side wall of the vacuum furnace chamber 11, and the induction coil 23 is located inside the vacuum furnace chamber 11. An insulator 25 is provided on the outside of the induction coil 23. One end of the induction coil 23 is connected to a fixing member 24, and the other end of the fixing member 24 is recessed into the insulator 25. The insulator 25 is located on the outside of the induction coil 23. The outer side of the conductor of the induction coil 23 is sequentially covered with an insulating varnish layer 234, a polyimide film layer 235, a mica tape layer 236, and a glass fiber tape layer 237. The insulator 25 can be a structure such as a bakelite column.
[0025] The smelting system 30 includes a segmented water-cooled copper crucible 31 and a crucible tilting mechanism 32. The segmented water-cooled copper crucible 31 is located inside the vacuum furnace chamber 11 and within the internal space of the induction coil 23. The water-cooled copper crucible adopts a segmented structure (12-36 segments, crucible inner diameter greater than 180mm). The segments of the segmented water-cooled copper crucible 31 are mutually insulated, allowing the electromagnetic field to penetrate the crucible to heat the raw materials and generate levitation force. The capacity of the segmented water-cooled copper crucible 31 is greater than 50kg. The crucible tilting mechanism 32 is used to drive the segmented water-cooled copper crucible 31 to tilt and pour out the melt; and when the segmented water-cooled copper crucible 31 tilts, the coaxial water-cooled electrode 22 and the induction coil 23 can tilt synchronously.
[0026] The cooling system 40 is used to supply cooling water to the coaxial water-cooled electrode 22 and the segmented water-cooled copper crucible 31. The cooling system 40 includes a chiller, and water pipes are respectively installed between the chiller and the coaxial water-cooled electrode 22 and the segmented water-cooled copper crucible 31. The chiller supplies cooling water to the coaxial water-cooled electrode 22 and the segmented water-cooled copper crucible 31 through the water pipes, and also provides cooling water return.
[0027] The crucible tilting mechanism 32 may include a tilting rod connected to the segmented water-cooled copper crucible 31. The tilting rod is inserted through the side wall of the vacuum furnace chamber 11 or is located entirely within the vacuum furnace chamber 11. The tilting rod can be driven to rotate by a structure such as a motor, thereby causing the segmented water-cooled copper crucible 31 to rotate and tilt.
[0028] The control system 50 includes a PLC programmable controller, which is connected to a power regulation module, a monitoring module, a temperature monitoring module, and other components. The power regulation module is connected to the inductive power supply 21, the monitoring module is connected to the measuring device 14, and the temperature monitoring module includes an infrared thermometer installed in the vacuum furnace chamber 11 for measuring the melt temperature and a water temperature sensor for measuring the cooling water temperature. The PLC programmable controller controls the operation of the inductive power supply 21 through the power regulation module; the PLC programmable controller receives measurement data from the measuring device 14 through the monitoring module, and thus controls the operation of the vacuum pumping unit 12, etc.; the PLC programmable controller receives measurement data from the infrared thermometer and the water temperature sensor through the temperature monitoring module, and thus controls the operation of the chiller and the inductive power supply 21. This structure achieves fully automated control of the entire process.
[0029] In this embodiment of the invention, the segments of the segmented water-cooled copper crucible 31 are arranged at intervals, and corundum sheets are filled between the segments. This structure ensures that the segments are mutually insulated.
[0030] In this embodiment of the invention, the induction power supply 21 adopts a low-voltage, high-power design with a rated power greater than 800KW and a rated voltage less than 500V, which is more than 30% lower than the voltage of the conventional induction coil 23, thereby reducing the risk of discharge in a high vacuum environment from the source.
[0031] In the above scheme, the induction power supply 21 adopts a low-voltage design to reduce the risk of discharge from the source; each turn of the induction coil undergoes quadruple high-voltage insulation treatment with insulating varnish, polyimide film, mica tape, and fiberglass tape; the fixing component 24 is recessed into the insulator 25 to eliminate the potential discharge hazard of sharp edges in a vacuum state. This structure reduces the risk of discharge, enabling high-power melting in a high-vacuum environment. Furthermore, it optimizes the layout of high-voltage circuit components within the vacuum furnace (e.g., increasing the insulation distance between the induction coil and other components to avoid electric field concentration), further reducing the risk of discharge.
[0032] In this embodiment of the invention, the induction coil 23 has an upper heat-preserving coil 231 and a lower main heating coil 232 that can be controlled separately. The upper heat-preserving coil 231 and the lower main heating coil 232 are isolated by a high-voltage resistant insulating partition 233. The high-voltage resistant insulating partition 233 can be made of ceramic or similar materials. The upper heat-preserving coil 231 and the lower main heating coil 232 are tightly coupled in the vertical direction, sharing the same magnetic field space of the segmented water-cooled copper crucible 31, and can be individually controlled for power supply (both frequency and power are adjustable). The above structure allows the induction coil 23 to be controlled in segments, upper and lower. Specifically, the lower main heating coil 232 is supplied with a high-frequency (6KHZ-20KHZ) high-power current (accounting for more than 60% of the total power). This frequency range takes into account both excellent magnetic penetration depth and skin effect. Its main function is to provide strong levitation force to drive the melt to detach from the crucible wall and generate violent convection to accelerate the floating of inclusions. The upper heat preservation coil 231 is supplied with a lower frequency (1KHZ-5KHZ) current (accounting for less than 40% of the total power). The low-frequency magnetic field has stronger penetrating power and can effectively penetrate the upper liquid surface of the molten pool 61. Its main function is to replenish the heat at the top of the molten pool 61, suppress heat radiation heat dissipation, and gently stir the surface melt to prevent the low melting point elements from burning or splashing due to local overheating of the surface of the molten pool 61 under extreme power input.
[0033] In some embodiments, the vacuum pumping unit 12 includes a rotary vane pump 121, a roots pump 122, a first fore-stage valve 123, a magnetic levitation molecular pump 124, a first vacuum valve 125, and a roughing valve 126. The rotary vane pump 121, the roots pump 122, the first fore-stage valve 123, the magnetic levitation molecular pump 124, the first vacuum valve 125, and the vacuum chamber 11 are connected in series. The roughing valve 126 is connected in parallel between the inlet of the first vacuum valve 125 and the outlet of the first fore-stage valve 123 through a pipe.
[0034] In some embodiments, the vacuum system 10 further includes a condenser pump group 13 connected in parallel with the vacuum pumping unit 12, i.e., the vacuum pumping unit 12 and the condenser pump group 13 are connected in parallel to the vacuum furnace chamber. The condenser pump group 13 includes a dry mechanical pump 131, a second fore-stage valve 132, a cryogenic condenser pump 133, and a second vacuum valve 134. The dry mechanical pump 131, the second fore-stage valve 132, the cryogenic condenser pump 133, the second vacuum valve 134, and the vacuum furnace chamber 11 are connected in series. A water-cooled metal vapor condenser plate is installed on one side of the vacuum chamber of the second vacuum valve 134.
[0035] In the above scheme, the magnetic levitation molecular pump 124 has an extremely high compression ratio and pumping rate for light gases (especially hydrogen and helium); the cryogenic condensation pump 133 utilizes cryogenic condensation of residual gases (mainly H2O, CO2, and residual impurity gases) below 20K. The magnetic levitation molecular pump 124 adopts an oil-free design, using pure magnetic levitation bearings without mechanical contact, and the pump body does not require oil-based sealing media, completely eliminating the risk of C and H contamination of the melt by oil vapor backflow. In the later stages of refining, the cryogenic condensation pump 133 can be started to specifically "deeply remove" the trace residual gases continuously released from the molten pool, further reducing the microporosity in the casting to below 0.1%.
[0036] Reference Figure 5 The present invention also provides a suspension melting and purification method based on the above-mentioned high-power high-vacuum suspension melting and purification equipment, which includes the following steps: S1. Charging: Load the raw material to be smelted into the segmented water-cooled copper crucible 31 and close the vacuum furnace chamber 11. S2. Vacuuming: Start the vacuum pumping unit 12 to evacuate the vacuum furnace chamber 11, so that the vacuum degree of the vacuum furnace chamber 11 is not higher than 6.67×10-3Pa. S3, Electric melting: Start the induction power supply 21, and the electromagnetic field generated by the induction coil 23 penetrates the segmented water-cooled copper crucible 31 to heat the raw material. Under the action of electromagnetic force, the raw material melts to form a melt, and a molten pool 61 is generated in the segmented water-cooled copper crucible 31, and the melt is suspended. S4. High-vacuum refining: The melt is refined by electromagnetic stirring for 10-120 minutes to remove impurities; and the vacuum degree in the vacuum furnace chamber 11 is controlled to be no higher than 0.01 Pa by the operation of the vacuum pump unit 12; during this process, the high vacuum environment promotes the removal of gaseous impurities such as hydrogen, oxygen, and nitrogen; high-power electromagnetic stirring accelerates the volatilization of low-melting-point impurities and the floating of non-metallic inclusions; the suspended state avoids the introduction of crucible impurities; when the vacuum system 10 is equipped with a condensation pump unit 13, the low-temperature condensation pump 133 can be started at the end of the refining stage for deep residual gas removal; S5. Casting: The molten material is poured into mold 33; S6. Cooling and Removal: The melt is cooled into a casting under vacuum or protective atmosphere, and the casting is removed from the vacuum furnace chamber 11.
[0037] During the energized melting process in step S3, the electromagnetic field generated by the energized induction coil 23 penetrates the segmented water-cooled copper crucible 31 to heat the raw material. The process of the raw material melting into a melt under the action of electromagnetic force includes: The induction coil 23 is energized with a preset initial power (e.g., 300-500KW) to preheat the raw material (the preheating time can be set to 10-20 minutes); this process slowly heats the raw material to avoid splashing. The induction coil 23 gradually increases its power until all the raw material is melted; when all the raw material is melted, the induction coil 23 increases its power to the first level. During the high-vacuum refining process in step S4, the induction coil 23 is energized with a second power, and the second power is not less than the first power; wherein, the first power and the second power mentioned above are the total power of the upper heat preservation coil 231 and the lower main heating coil 232.
[0038] In some embodiments, the upper heat-insulating coil 231 and the lower main heating coil 232 can operate as a whole at the same frequency to implement the energized melting process S3 and the high-vacuum refining process S4. In this case, the power of the induction coil 23 during the energized melting process and the high-vacuum refining process is the total power of the upper heat-insulating coil 231 and the lower main heating coil 232. Alternatively, only the lower main heating coil 232 operates to implement the energized melting process S3 and the high-vacuum refining process S4. In this case, the power of the induction coil 23 during the energized melting process and the high-vacuum refining process is the same as the power of the lower main heating coil 232.
[0039] In some embodiments, the upper heat-preserving coil 231 and the lower main heating coil 232 operate in a dual-frequency coordinated mode. Specifically, during the energized melting process in S3, the lower main heating coil 232 operates to melt the raw material (during this process, the lower main heating coil 232 uses a preset initial power for preheating + power increase until all the raw material is melted); during the high-vacuum refining process in S4, the lower main heating coil 232 uses a preset constant power (not lower than the power at the end of S3), the upper heat-preserving coil 231 starts working and uses variable power, and the frequency of the upper heat-preserving coil 231 is lower than the frequency of the lower main heating coil 232. In this embodiment, during the energized melting process, the power of the induction coil 23 is the same as the power of the lower main heating coil 232; during the high-vacuum refining process, the power of the induction coil 23 is the total power of the upper heat-preserving coil 231 and the lower main heating coil 232.
[0040] In the process of heating the upper insulation coil 231 using variable power, when the infrared thermometer detects that the temperature gradient between the surface and bottom of the molten pool 61 exceeds a set threshold (e.g., 30℃), the power of the upper insulation coil 231 is automatically adjusted to ensure that the longitudinal temperature gradient of the molten pool 61 does not exceed 50℃, significantly improving the compositional segregation problem of high-melting-point refractory alloys. This dual-frequency structure can increase the suspension height of the molten pool 61 by 15%-20%, while improving the aggregation effect of the oxide film (slag) on the surface of the molten pool 61 by more than 30%. In the above scheme, by adjusting the power of the upper insulation coil 231 in advance, thermal inertia can be avoided from causing the longitudinal temperature gradient of the molten pool 61 to exceed the limit.
[0041] In some embodiments, when the vacuum system 10 is equipped with a condenser pump group 13, after starting the vacuum pumping unit 12 to evacuate the vacuum furnace chamber 11 in step S2, the process further includes: closing the second vacuum valve 134, starting the dry mechanical pump 131, opening the second fore-stage valve 132 to evacuate the cryogenic condenser pump 133, and closing the second fore-stage valve 132 when the vacuum level in the cryogenic condenser pump 133 is lower than 40 Pa, and starting the cryogenic condenser pump 133 to cool the pump to 20 K. Furthermore, in step S4, 3-30 minutes before the end of high-vacuum refining, the second vacuum valve 134 is opened to purge residual gas from the vacuum furnace chamber 11 until the high-vacuum refining is completed.
[0042] The following are some methods for smelting metals.
[0043] Example 1: Smelting and purification of titanium alloy (Ti-6Al-4V) This embodiment adopts the basic equipment scheme; the raw materials are sponge titanium (purity 99.5%), aluminum briquettes, and aluminum-vanadium master alloy, with a total loading of 150kg. The equipment parameters are as follows: the inner diameter of the segmented water-cooled copper crucible is about 280mm; the induction coil operates at a single frequency (the upper heat preservation coil and the lower main heating coil operate at the same frequency, and the two are regarded as a whole coil; or only the lower main heating coil operates).
[0044] Smelting steps: (1) Put the sponge titanium, aluminum briquettes and aluminum-vanadium master alloy into a segmented water-cooled copper crucible according to the Ti-6Al-4V composition ratio, and close the furnace door. (2) Start vacuum pumping: pre-pump the rotary vane pump to 10Pa, start the Roots pump to 1Pa, and start the magnetic levitation molecular pump to evacuate to no higher than 6.67×10. -3 Pa. (3) Start the induction power supply: preheat at 300kW for 10 minutes, gradually increase to 1000kW to melt all the furnace charge (i.e., the melting process and power increase are carried out at the same time, and the power is 1000KW when all the charge is melted), and then increase to 1200kW for refining. (4) Refine for 30 minutes at 1200kW power and a vacuum degree not higher than 0.01Pa. Electromagnetic stirring causes the molten pool to convect violently, promoting gas removal and impurity floating. (5) After refining, reduce the power to 1000kW and pour the melt into the water-cooled mold 33. (6) Cool the casting to below 200℃ under vacuum, break the vacuum and take it out.
[0045] Effects: Oxygen content decreased from approximately 1200 ppm before smelting to no more than 450 ppm; hydrogen content decreased from approximately 50 ppm before smelting to no more than 8 ppm (e.g., Figure 6 (As shown); the casting has a uniform structure and is free from defects such as porosity and inclusions.
[0046] Example 2: Preparation of High-Purity Nickel The raw material in this embodiment is electrolytic nickel (99.95% purity), with a loading of 200 kg. The equipment parameters are the same as in Embodiment 1, but the induction coil adopts dual frequency (the upper heat preservation coil and the lower main heating coil are controlled separately).
[0047] Smelting steps: (1) Load the electrolytic nickel into the segmented water-cooled copper crucible and close the furnace door. (2) Start vacuum pumping: The vacuum degree of the vacuum furnace chamber shall not exceed 6.67×10 -3 Pa. (3) Start the induction power supply: use the lower main heating coil (frequency 10KHZ) to melt at 1100kW power (preheat at 300KW for 10 minutes first, then increase the power, and the power is 1100KW when it is completely melted). After it is completely melted, switch to the dual-frequency synergistic mode (lower main heating coil at full power of 1200kW, upper heat preservation coil (frequency 3KHZ) dynamically adjusts the power (300-500kW) according to infrared temperature measurement for refining). (4) Maintain the dual-frequency synergistic refining for 40 minutes. High-power electromagnetic stirring promotes the removal of volatile impurities such as Pb, Zn, Ag, and Bi. At the same time, the upper low-frequency heating suppresses surface overheating and ensures that the longitudinal temperature difference of the molten pool is not higher than 15℃. (5) After refining, cast and remove after vacuum cooling.
[0048] Effects: Nickel purity increased from 99.95% to 99.995% (4N5 grade); oxygen content not exceeding 15 ppm; hydrogen content not exceeding 3 ppm (e.g., ...). Figure 7 (As shown); the ingot surface is smooth, without localized oxide scale or spatter defects.
[0049] Example 3: Preparation of High-Purity Copper The raw material in this embodiment is electrolytic copper (99.97% purity), with a loading capacity of 150 kg. The equipment parameters are as follows: equipped with a vacuum pump unit and a condenser pump unit (using an oil-free magnetic levitation molecular pump); the induction coil operates at a single frequency (the upper insulation coil and the lower main heating coil operate at the same frequency, and the two are regarded as a whole coil; or only the lower main heating coil operates).
[0050] Smelting steps: (1) Load the electrolytic copper into the segmented water-cooled copper crucible and close the furnace door. (2) Start the rotary vane pump and the Roots pump in sequence, and start the magnetic levitation molecular pump when the vacuum degree is 1 Pa. Evacuate to a vacuum degree not higher than 5.0 × 10 -3Pa. (3) Start the dry mechanical pump, open the second pre-vacuum valve to evacuate the cryogenic condenser pump, and close the second pre-vacuum valve when the vacuum level in the cryogenic condenser pump is lower than 40 Pa. Start the cryogenic condenser pump to cool the pump to 20 K, but do not open the second vacuum valve. (4) Start the induction power supply and preheat at 300 kW for 10 minutes, gradually increasing to 1100 kW to melt all the furnace charge (the melting process is accompanied by power increase, and the power is 1100 KW when all the charge is melted); during this process, the vacuum level in the furnace first decreases and then gradually increases. (5) When the vacuum level returns to 5.0 × 10 Pa, -3 At Pa, increase the power to 1200kW and refine for 25 minutes; open the second vacuum valve, ensuring the vacuum level in the vacuum furnace chamber does not exceed 1.0×10⁻⁶. -3 Continue refining for 10 minutes under the Pa environment, and use a cryogenic condensation pump to deeply capture the trace residual gas released from the molten pool. (5) After refining, cast the mixture and remove it after vacuum cooling.
[0051] Results: Copper purity increased from 99.97% to 99.999% (5N grade); oxygen content not exceeding 5ppm; hydrogen content not exceeding 2ppm; carbon increase not exceeding 3ppm (eliminating hydrocarbon contamination in oil diffusion pumps).
[0052] Example 4: Preparation of Tungsten-Molybdenum High Melting Point Alloy The raw materials in this embodiment are tungsten powder, molybdenum powder, and other alloying elements, with a total loading of 30 kg. The equipment parameters are as follows: equipped with a vacuum pump unit (using an oil-free magnetic levitation molecular pump); the induction coil uses dual frequency.
[0053] Melting steps: (1) Press the mixed powder into blocks and place them into a crucible. (2) Evacuate the vacuum furnace to a vacuum level not exceeding 5.0 × 10⁻⁶. -4 Pa. (3) Start the lower main heating coil for heating and melting (preheat at 300KW for 10 minutes, then increase the power to 1100KW when fully melted). After complete melting, turn on the upper heat preservation coil and enter the dual-frequency collaborative refining mode (lower main heating coil power 1200kW, upper heat preservation coil power dynamically adjusted). Refining time is 45 minutes. (4) During the refining process, infrared temperature measurement is fed back in real time, and the power of the upper heat preservation coil is dynamically adjusted to control the temperature difference between the top and bottom of the molten pool to no more than 12℃, effectively preventing molybdenum element deposition and segregation at the bottom. (5) After refining, cast and remove after vacuum cooling.
[0054] Results: The uniformity of alloy composition is greatly improved, and the segregation is reduced by 40% compared with single-frequency melting; the oxygen content is no higher than 200ppm and the hydrogen content is no higher than 5ppm; the castings have high density and no macroscopic segregation.
[0055] The embodiments of the present invention have been described in detail above with reference to the accompanying drawings. However, the present invention is not limited to the above embodiments. Within the scope of knowledge possessed by those skilled in the art, various changes can be made without departing from the spirit of the present invention.
Claims
1. A high-power, high-vacuum suspension melting and purification device, characterized in that, It includes a vacuum system (10), a heating system (20), a melting system (30), and a cooling system (40). The vacuum system (10) includes a vacuum furnace chamber (11) and a vacuum pumping unit (12), wherein the vacuum furnace chamber (11) is connected to the vacuum pumping unit (12); The heating system (20) includes an induction power supply (21), a coaxial water-cooled electrode (22) and an induction coil (23), which are connected in sequence, and the induction coil (23) is located inside the vacuum furnace chamber (11); The smelting system (30) includes a segmented water-cooled copper crucible (31) and a crucible tilting mechanism (32). The segmented water-cooled copper crucible (31) is located in a vacuum furnace chamber (11), and the segments of the segmented water-cooled copper crucible (31) are insulated from each other. The crucible tilting mechanism (32) is used to drive the segmented water-cooled copper crucible (31) to tilt and pour out the melt. The cooling system (40) is used to supply cooling water to the coaxial water-cooled electrode (22) and the segmented water-cooled copper crucible (31); An insulator (25) is provided on the outside of the induction coil (23). One end of the induction coil (23) is connected to a fixing member (24), and the other end of the fixing member (24) is recessed into the insulator (25). The outer side of the conductor of the induction coil (23) is sequentially covered with an insulating varnish layer (234), a polyimide film layer (235), a mica tape layer (236), and a glass fiber tape layer (237).
2. The high-power high-vacuum suspension melting and purification equipment according to claim 1, characterized in that, The induction coil (23) has an upper heat preservation coil (231) and a lower main heating coil (232) that can be controlled separately, and the upper heat preservation coil (231) and the lower main heating coil (232) are isolated by a high-voltage resistant insulating partition (233).
3. The high-power high-vacuum suspension melting and purification equipment according to claim 1, characterized in that, The vacuum pumping unit (12) includes a rotary vane pump (121), a roots pump (122), a first fore-stage valve (123), a magnetic levitation molecular pump (124), a first vacuum valve (125), and a roughing valve (126). The rotary vane pump (121), the roots pump (122), the first fore-stage valve (123), the magnetic levitation molecular pump (124), the first vacuum valve (125), and the vacuum furnace chamber (11) are connected in series. The roughing valve (126) is connected in parallel between the inlet of the first vacuum valve (125) and the outlet of the first fore-stage valve (123).
4. The high-power high-vacuum suspension melting and purification equipment according to claim 3, characterized in that, The vacuum system (10) also includes a condenser pump group (13) connected in parallel with the vacuum pumping unit (12). The condenser pump group (13) includes a dry mechanical pump (131), a second fore-stage valve (132), a cryogenic condenser pump (133), and a second vacuum valve (134). The dry mechanical pump (131), the second fore-stage valve (132), the cryogenic condenser pump (133), the second vacuum valve (134), and the vacuum furnace chamber (11) are connected in series. A water-cooled metal vapor condenser plate is installed on one side of the vacuum chamber of the second vacuum valve (134).
5. The high-power high-vacuum suspension melting and purification equipment according to claim 1, characterized in that, The rated power of the inductive power supply (21) is greater than 800KW and the rated voltage is less than 500V; The inner diameter of the segmented water-cooled copper crucible (31) is greater than 108 mm.
6. The high-power high-vacuum suspension melting and purification equipment according to claim 1, characterized in that, The segments of the segmented water-cooled copper crucible (31) are arranged at intervals, and corundum sheets are filled between the segments of the segmented water-cooled copper crucible (31).
7. The suspension melting and purification method based on the high-power high-vacuum suspension melting and purification equipment according to claim 2, characterized in that, include: S1. Loading: Load the raw materials to be smelted into the segmented water-cooled copper crucible (31) and close the vacuum furnace chamber (11). S2. Vacuuming: Start the vacuum pumping unit (12) to evacuate the vacuum chamber (11) so that the vacuum degree of the vacuum chamber (11) is not higher than 6.67×10-3Pa; S3, Electric melting: Start the induction power supply (21), the electromagnetic field generated by the induction coil (23) penetrates the segmented water-cooled copper crucible (31) to heat the raw material, and the raw material melts under the action of electromagnetic force to form a melt, and the melt is in a suspended state; S4. High vacuum refining: The melt is electromagnetically stirred and refined for 10-120 minutes to remove impurities; and the vacuum degree in the vacuum furnace (11) is controlled to be no higher than 0.01 Pa; S5, Casting: The melt is poured into the mold (33); S6. Cooling and removal: The melt is cooled into a casting under vacuum or protective atmosphere, and the casting is removed from the vacuum furnace chamber (11).
8. The suspension melting and purification method according to claim 7, characterized in that, In step S3, the electromagnetic field generated by the energized induction coil (23) penetrates the segmented water-cooled copper crucible (31) to heat the raw material. Under the action of electromagnetic force, the raw material melts to form a melt, including: The induction coil (23) is energized with a preset initial power to preheat the raw materials; The induction coil (23) gradually increases its power until all the raw materials are melted; and increases its power to the first level when all the raw materials are melted. In step S4, the induction coil (23) is energized with a second power, and the second power is not less than the first power.
9. The suspension melting and purification method according to claim 7, characterized in that, In step S4, the lower main heating coil (232) uses a preset constant power, the upper heat preservation coil (231) uses a variable power, and the longitudinal temperature difference of the molten pool (61) is not greater than 50°C; and the frequency of the upper heat preservation coil (231) is less than the frequency of the lower main heating coil (232).
10. The suspension smelting and purification method according to claim 7, characterized in that, The vacuum system (10) also includes a condenser pump group (13), which includes a dry mechanical pump (131), a second fore-stage valve (132), a cryogenic condenser pump (133), and a second vacuum valve (134). The dry mechanical pump (131), the second fore-stage valve (132), the cryogenic condenser pump (133), the second vacuum valve (134), and the vacuum furnace chamber (11) are connected in series. In step S2, after the vacuum pumping unit (12) is started to evacuate the vacuum furnace chamber (11), the following steps are also included: closing the second vacuum valve (134), starting the dry mechanical pump (131), opening the second pre-valve (132) to evacuate the cryogenic condenser pump (133), closing the second pre-valve (132) when the vacuum degree in the cryogenic condenser pump (133) is lower than 40 Pa, starting the cryogenic condenser pump (133) to cool the pump to 20 K; In step S4, 3-30 minutes before the end of high vacuum refining, the second vacuum valve (134) is opened to remove residual gas from the vacuum furnace chamber (11) until the end of high vacuum refining.