Atomic-level defect characterization method and apparatus based on defect-sensitive exciton luminescence response
By applying controlled local mechanical action to the calibration region of a semiconductor heterostructure and combining it with exciton emission spectral signal analysis, the problem of difficulty in rapidly and accurately characterizing buried defects in semiconductor heterostructures in existing technologies has been solved, achieving non-destructive and quantitative defect characterization.
Patent Information
- Application Number
- CN202611100995.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-23
- Publication Date
- 2026-11-10
AI Technical Summary
Existing technologies are insufficient for rapidly screening atomic-level defects buried in semiconductor heterostructures over large areas. Conventional detection methods require stringent sample preparation procedures and are prone to altering the sample state. Traditional optical methods have failed to effectively quantify defect density and distribution.
By applying controlled local mechanical forces to the calibration region of a semiconductor heterostructure, atomic-level defects of different densities are introduced. Combined with exciton emission spectral signal analysis, the correspondence between defect density and optical parameters is established, achieving non-destructive and quantitative defect characterization.
It enables non-destructive and rapid assessment of buried defects inside devices in an atmospheric environment, avoiding interference from complex sample preparation procedures on the sample state and improving detection efficiency and accuracy.
Smart Images

Figure CN123066031A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of semiconductor interface defect technology, and in particular to an atomic-level defect characterization method and apparatus based on defect-sensitive exciton luminescence response. Background Technology
[0002] As the application of low-dimensional semiconductor materials and the van der Waals heterostructures formed by their stacking deepens in integrated optoelectronic chips, high-sensitivity photodetectors, and low-power information devices, the quality of the material interlayer interfaces has an increasingly significant impact on the overall performance, operational stability, and lifetime of these devices. During the transfer, stacking, cleaning, polishing, and subsequent semiconductor processing of two-dimensional materials, atomic-level defects such as lattice vacancies, adsorption residues, localized strain, and charge traps are easily formed in the subsurface or interface regions of semiconductor heterostructures due to interlayer interactions or external mechanical contact. These atomic-level defects exhibit tiny size and non-uniform spatial distribution in the microscopic space, and because they are often located within buried interfaces, conventional surface morphology measurement methods struggle to directly and effectively identify and locate their distribution.
[0003] In current semiconductor technology, conventional detection methods for these buried microscopic atomic-level defects heavily rely on high-resolution microscopy techniques such as transmission electron microscopy and scanning tunneling microscopy. However, these high-resolution microscopy techniques generally require extremely demanding sample preparation processes and typically operate in special testing environments such as high vacuum or extremely low temperatures. This results in extremely limited detection range, relatively low testing efficiency, and even some contact characterization may alter the original state of the sample to some extent, making them unsuitable for the large-area, rapid screening requirements at the chip level. While traditional photoluminescence and Raman spectroscopy offer the advantages of non-contact and rapid acquisition, existing optical schemes mostly focus on assessing the intrinsic luminescence quality or macroscopic strain state of materials. They fail to effectively establish a direct quantitative correlation between the fine spectral evolution characteristics of exciton luminescence behavior and the density, spatial distribution, and microscopic nonradiative recombination processes of local atomic-level defects at the interface, thus limiting their application in the precise characterization of atomic-level defects. Summary of the Invention
[0004] This invention provides an atomic-level defect characterization method and apparatus based on defect-sensitive exciton luminescence response, offering a non-contact, non-destructive, and quantitative optical detection approach. It enables non-destructive and rapid assessment of buried defects inside devices in an atmospheric environment, effectively avoiding interference from complex sample preparation processes on the original state of the sample.
[0005] In a first aspect, the present invention provides an atomic-level defect characterization method based on defect-sensitive exciton luminescence response, comprising: Controlled local mechanical forces are applied to a calibration region of a semiconductor heterostructure to introduce atomic-level defects of different densities into the calibration region without damage; wherein the semiconductor heterostructure is constructed to have defect-sensitive exciton luminescence characteristics. Based on the exciton emission spectrum signals of the calibration region under different atomic-level defect densities, at least one defect-sensitive optical parameter of the semiconductor heterostructure is obtained, and a defect response calibration curve between atomic-level defect density and the defect-sensitive optical parameter is established. The defect-sensitive optical parameters of the unknown region are obtained from the exciton emission spectrum signal of the unknown region in the semiconductor heterostructure, and the atomic-level defect information of the unknown region is obtained from the defect-sensitive optical parameters of the unknown region and the defect response calibration curve.
[0006] In some embodiments, the semiconductor heterostructure includes a semiconductor substrate, a bottom dielectric layer, a first two-dimensional semiconductor monolayer material layer, and a second two-dimensional semiconductor monolayer material layer stacked sequentially; wherein the interlayer relative rotation angle between the first two-dimensional semiconductor monolayer material layer and the second two-dimensional semiconductor monolayer material layer is a high-symmetry coupling angle under a symmetric lattice.
[0007] In some embodiments, the first two-dimensional semiconductor monolayer is a molybdenum diselenide monolayer film, the second two-dimensional semiconductor monolayer is a tungsten disulfide monolayer film, the bottom dielectric layer is a hexagonal boron nitride film, and the semiconductor substrate is a silicon wafer with a silicon dioxide coating on its surface.
[0008] In some embodiments, controlled local mechanical forces are applied to a calibration region of a semiconductor heterostructure to nondestructively introduce atomic-level defects of varying densities into the calibration region, including: By adjusting the process control parameters for applying the controlled local mechanical action using a preset process, lattice vacancy defects or local strain defects of different densities are introduced in stages within the calibrated area; wherein, the preset process includes at least one of controlled micro-area sliding friction process, nano-scrubbing process, and micro-area chemical mechanical polishing process, and the process control parameters include at least one of normal load, scanning speed, number of cycles, and scanning area size.
[0009] In some embodiments, the preset process is the controlled micro-area sliding friction process, and the process control parameters include normal load, number of cycles, and scanning area size; wherein, the normal load ranges from 50 nanoNewtons to 200 nanoNewtons, the scanning area size ranges from 2 micrometers by 2 micrometers to 5 micrometers by 5 micrometers, and the number of cycles ranges from 20 to 80.
[0010] In some embodiments, acquiring the exciton emission spectrum signal includes: The calibration region is irradiated with a continuous laser or a pulsed laser as the excitation source to obtain the exciton emission spectrum signal; wherein the wavelength of the excitation source covers the intrinsic exciton transition energy range of the two-dimensional semiconductor monolayer material in the semiconductor heterostructure, and the incident power of the excitation source is less than or equal to the incident power threshold.
[0011] In some embodiments, establishing a defect response calibration curve between atomic-level defect density and the defect-sensitive optical parameter includes: The peak energy and integrated luminescence intensity of the hybrid exciton emission peak in the exciton emission spectrum signal generated by the calibration region under different normal loads applied by mechanical force are obtained. Establish an energy level shift calibration curve between the normal load and the peak energy value, and establish an intensity attenuation calibration curve between the normal load and the integrated luminescence intensity, so as to jointly constitute the defect response calibration curve.
[0012] In some embodiments, after acquiring the exciton emission spectrum signal of an unknown region, the method further includes: When the exciton emission spectrum signal of the unknown region, compared with the exciton emission spectrum signal of the defect-free reference region, shows a decrease in the integrated emission intensity of the hybrid exciton emission peak and a redshift of the peak energy value to a lower energy direction, it is determined that there is an atomic-level defect in the unknown region.
[0013] In some embodiments, obtaining atomic-level defect information of the unknown region includes: The excitation light source is controlled to perform two-dimensional dot matrix scanning on the test plane of the semiconductor heterostructure to obtain the equivalent atomic level defect density value corresponding to each scanning point, and the equivalent atomic level defect density value corresponding to each scanning point is used as the atomic level defect information. The method further includes: mapping the equivalent atomic-level defect density value to spatial coordinates to obtain a two-dimensional defect morphology image showing the spatial non-uniform distribution of the atomic-level defects.
[0014] In some embodiments, after nondestructively introducing atomic-level defects of different densities into the calibration region, the method further includes: Obtain a ratio parameter as a second defect-sensitive optical parameter; wherein the ratio parameter is the ratio of the integrated luminescence intensity of the hybrid exciton emission peak in the exciton emission spectrum signal to the integrated luminescence intensity of the intrinsic exciton emission peak of the two-dimensional semiconductor monolayer material in the semiconductor heterostructure; Establish an auxiliary ratio calibration curve between the mechanically applied normal load and the ratio parameter; Based on the ratio parameter measured in the unknown region and the auxiliary ratio calibration curve, the atomic-level defect information is calibrated for environmental disturbance error.
[0015] In some embodiments, after nondestructively introducing atomic-level defects of different densities into the calibration region, the method further includes: A control voltage that is continuously scanned is applied to the semiconductor heterostructure; The differential modulation spectral line of the integral luminescence intensity of the hybrid exciton emission peak in the exciton emission spectrum signal as a function of the control voltage is obtained as the third defect-sensitive optical parameter. The charge state and deep energy level position of atomic-level defects in the unknown region are obtained by using the characteristic jump points in the differential modulation spectral lines.
[0016] Secondly, the present invention also provides an atomic-level defect characterization device based on defect-sensitive exciton luminescence response, comprising: A defect introduction module is used to control the application of controlled local mechanical forces in a calibration region of a semiconductor heterostructure to introduce atomic-level defects of different densities into the calibration region without damage; wherein the semiconductor heterostructure is constructed to have defect-sensitive exciton luminescence characteristics; The calibration establishment module is used to obtain at least one defect-sensitive optical parameter of the semiconductor heterostructure based on the exciton emission spectrum signal of the calibration region under different atomic-level defect densities, and to establish a defect response calibration curve between the atomic-level defect density and the defect-sensitive optical parameter. The defect characterization module is used to obtain the defect-sensitive optical parameters of the unknown region based on the exciton emission spectrum signal of the unknown region in the semiconductor heterostructure, and to obtain the atomic-level defect information of the unknown region based on the defect-sensitive optical parameters of the unknown region and the defect response calibration curve.
[0017] Thirdly, the present invention also provides an electronic device, including a processor and a memory storing a computer program, wherein the processor executes the computer program to implement the steps of the atomic-level defect characterization method based on defect-sensitive exciton luminescence response as described in the first aspect.
[0018] Fourthly, the present invention also provides a non-transitory computer-readable storage medium having a computer program stored thereon, wherein the computer program, when executed by a processor, implements the atomic-level defect characterization method based on defect-sensitive exciton luminescence response as described in the first aspect.
[0019] This invention provides a non-contact, non-destructive, and quantitative optical detection method by converting the density of microscopic atomic-level defects, which is difficult to count directly, into a highly sensitive spectral physical quantity evolution. Compared with traditional contact or high-vacuum characterization methods such as transmission electron microscopy, it greatly improves detection efficiency and realizes non-destructive and rapid assessment of buried defects inside devices in an atmospheric environment, effectively avoiding interference from complex sample preparation processes on the original state of the sample. Attached Figure Description
[0020] To more clearly illustrate the technical solutions in this invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced one by one below. Obviously, the drawings described below are some embodiments of this invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.
[0021] Figure 1 This is a schematic flowchart of an atomic-level defect characterization method based on defect-sensitive exciton luminescence response provided in an embodiment of the present invention; Figure 2 This is a three-dimensional structural schematic diagram of a semiconductor heterostructure with defect-sensitive exciton luminescence characteristics provided in an embodiment of the present invention; Figure 3 This is a schematic diagram comparing the photoluminescence spectra of a semiconductor heterostructure and a monolayer material provided in an embodiment of the present invention; Figure 4 This is a schematic diagram illustrating the test results of obtaining the relative orientation of a semiconductor heterostructure through second harmonic testing, provided by an embodiment of the present invention. Figure 5 This is a schematic diagram illustrating the non-destructive introduction of atomic-level defects of different densities into a calibration area using an atomic force microscope sliding friction process, as provided in an embodiment of the present invention. Figure 6 This is a schematic diagram of the surface morphology of an atomic force microscope in a calibration area after being subjected to different normal loads, provided by an embodiment of the present invention. Figure 7 This is a schematic diagram showing the comparison of photoluminescence spectra of the calibration region extracted under different friction loads, provided by an embodiment of the present invention. Figure 8 This is a schematic diagram illustrating the relationship between the peak energy value of a hybrid exciton emission peak and the processing load, provided in an embodiment of the present invention. Figure 9 This is a schematic diagram illustrating the relationship between the integrated luminescence intensity of a hybrid exciton emission peak and the processing load, provided in an embodiment of the present invention. Figure 10 This is a schematic diagram of the structure of an atomic-level defect characterization device based on defect-sensitive exciton luminescence response provided in an embodiment of the present invention; Figure 11 This is a schematic diagram of the structure of an electronic device provided in an embodiment of the present invention. Detailed Implementation
[0022] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions of this invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of this invention. Based on the embodiments of this invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this invention.
[0023] With the continuous development of applications of two-dimensional semiconductors and their van der Waals heterostructures in light-emitting devices, photoelectric detection, low-power information devices, and integrated optoelectronic systems, the impact of interface quality on device performance and reliability is becoming increasingly prominent. During transfer, stacking, cleaning, friction contact, polishing, or subsequent processing, atomic-level defects such as vacancies, adsorption residues, localized strain, interface roughness, or charge traps may form on the material surface, encapsulation layer, or heterojunction interface. These defects are small in size, spatially non-uniform, and often located at the interface or subsurface region, making them difficult to identify directly through conventional surface morphology measurements.
[0024] Currently, atomic-level defect detection mainly relies on transmission electron microscopy, scanning tunneling microscopy, scanning transmission electron microscopy, atomic force microscopy, or related near-field characterization methods. While these methods offer high spatial resolution, they typically require complex sample preparation, vacuum or special testing environments, have limited detection areas, low testing efficiency, and some methods may even alter the sample state. Specifically, existing techniques for atomic-level defect detection and characterization in two-dimensional heterostructures have the following main shortcomings: First, existing detection methods largely rely on high-resolution microscopy, making it difficult to achieve rapid detection over large areas. While transmission electron microscopy (TEM) or scanning tunneling microscopy (STM) offer high spatial resolution, they suffer from stringent testing conditions, low detection efficiency, and limitations in device-level applications. Second, existing optical methods primarily focus on the intrinsic luminescence properties of materials, lacking the ability to quantitatively characterize defect-induced nonradiative recombination processes. Traditional photoluminescence or Raman spectroscopy typically reflects average signals, making it difficult to distinguish between the localized luminescence quenching effect caused by defects and changes in the intrinsic properties of the material. Third, there is a lack of effective methods for characterizing the spatial distribution of defects based on luminescence response. Due to the locality of atomic-level defects, their influence on exciton recombination behavior exhibits significant spatial non-uniformity, and existing methods struggle to achieve spatial localization and distribution analysis of defects using simple optical means.
[0025] Traditional photoluminescence and Raman spectroscopy offer advantages such as non-contact, rapid, and easily integrated testing. However, existing methods are primarily used to determine the intrinsic luminescence quality, layer number, or strain state of materials, lacking a technical solution that directly correlates changes in defect-sensitive exciton luminescence with interfacial atomic-level defect density, defect spatial distribution, and defect-induced nonradiative recombination processes. To address the issues of uncontrollable defect introduction, difficulty in achieving high-sensitivity detection methods, and the challenge of establishing a quantitative correlation between defect density and luminescence response in existing technologies, the applicant discovered that in van der Waals heterostructures of transition metal chalcogenides at near-zero degrees or specific turns, interlayer electron coupling can form defect-sensitive excitons with both intralayer and interlayer components. The luminescence intensity, peak position, linewidth, and spatial distribution of these defect-sensitive excitons are highly sensitive to local electronic structure, nonradiative recombination channels, and interlayer coupling states. When atomic-level defects exist at the interface or subsurface, these defects can introduce localized trap states, potential fluctuations, and nonradiative recombination channels, causing energy dissipation in defect-sensitive excitons before radiative recombination. This manifests as decreased luminescence intensity, peak position shift, linewidth variation, or uneven luminescence spatial distribution. Therefore, the defect-sensitive exciton luminescence response can serve as a non-contact, non-destructive, and spatially scannable defect-sensitive probe.
[0026] Therefore, this invention proposes an atomic-level defect characterization method based on defect-sensitive exciton luminescence response. This method introduces atomic-level defects of varying densities into a calibrated region of a semiconductor heterostructure by applying controlled local mechanical forces. The intensity and spatial distribution of defect-sensitive exciton luminescence are analyzed using exciton luminescence spectral signals to establish a correlation between atomic-level defect density and luminescence quenching degree, thereby enabling the identification and quantitative assessment of defect regions. This invention belongs to the fields of two-dimensional materials, van der Waals heterostructures, optical nondestructive testing, and semiconductor interface defect characterization. Specifically, it relates to a method for nondestructively identifying, locating, and quantitatively or semi-quantitatively evaluating atomic-level defects, especially those at the interface or subsurface of two-dimensional van der Waals heterostructures, using defect-sensitive exciton luminescence response. This method is applicable to two-dimensional semiconductor heterostructures with interlayer coupling or defect-sensitive exciton luminescence characteristics, such as tungsten disulfide / molybdenum diselenide, molybdenum disulfide / tungsten diselenide, and molybdenum diselenide / tungsten diselenide, and can also be extended to other low-dimensional semiconductor systems capable of forming defect-sensitive exciton luminescence responses.
[0027] Meanwhile, the method of this invention should meet the following conditions or technical requirements: First, the macroscopic structure remains stable. During the introduction of atomic-level defects, no significant material peeling, thickness loss, or damage to the macroscopic morphology of the interface occurs, thus ensuring the stability of the overall heterostructure structure and interlayer contact state. Second, the atomic-level defect density is controllable and repeatable. By adjusting the process control parameters of the controlled local mechanical action, the atomic-level defect density can be continuously adjusted, exhibiting good batch repeatability and regional consistency. Third, the detection results are quantifiable. By extracting defect-sensitive optical parameters from the exciton emission spectrum signal, a quantitative or semi-quantitative assessment of the defect's influence can be achieved. Fourth, it has strong spatial resolution, enabling the location and distribution characterization of defect regions based on the spatial non-uniformity of the emission signal. Fifth, it has applicability and integrability. This method can be applied to van der Waals heterostructures in different two-dimensional material systems and can be implemented as a non-destructive testing method in device fabrication or integration processes to meet the needs of subsequent device performance evaluation.
[0028] Figure 1 This is a flowchart illustrating an atomic-level defect characterization method based on defect-sensitive exciton emission response provided in an embodiment of the present invention. The atomic-level defect characterization method based on defect-sensitive exciton emission response can be executed by the atomic-level defect characterization device based on defect-sensitive exciton emission response provided in this embodiment of the invention. This atomic-level defect characterization device can be implemented using software and / or hardware. Figure 1 As shown, the atomic-level defect characterization method based on defect-sensitive exciton luminescence response includes the following steps: S101. Controlled local mechanical action is applied to the calibration region of the semiconductor heterostructure to introduce atomic-level defects of different densities into the calibration region without damage; wherein the semiconductor heterostructure is constructed to have defect-sensitive exciton luminescence characteristics.
[0029] S102. Obtain at least one defect-sensitive optical parameter of the semiconductor heterostructure based on the exciton emission spectrum signal of the calibration region under different atomic-level defect densities, and establish a defect response calibration curve between atomic-level defect density and defect-sensitive optical parameter.
[0030] S103. Obtain the defect-sensitive optical parameters of the unknown region based on the exciton emission spectrum signal of the unknown region in the semiconductor heterostructure, and obtain the atomic-level defect information of the unknown region based on the defect-sensitive optical parameters and defect response calibration curve of the unknown region.
[0031] Specifically, defect-sensitive exciton luminescence response refers to the sensitive optical response phenomenon in which the intensity, energy level position, and other spectral characteristics of excitons undergo radiative recombination luminescence due to microscopic defects within a semiconductor heterostructure. A semiconductor heterostructure refers to a microscopic composite structure formed by the tight bonding of at least two layers of semiconductor materials with different band structures through interlayer interactions. A calibration region refers to a selected standard experimental measurement area on the sample surface used to artificially introduce a known mechanical gradient, serving as a reference for subsequent quantitative back-calculation. Controlled local mechanical action refers to the application of microscopic local mechanical behaviors within a defined spatial range, where the magnitude, speed, and number of applications can be quantitatively controlled through external precision micro / nano fabrication or topography manipulation equipment. Atomic-level defects refer to microstructural incompleteness occurring at the lattice scale, including atomic vacancies, localized lattice distortions, microscopic strain, and lattice perturbations caused by interface residues.
[0032] Defect-sensitive optical parameters refer to physical characteristic parameters extracted from acquired spectral signals that exhibit monotonic correlation or high sensitivity to atomic-level defect density.
[0033] A defect response calibration curve is a pre-established mathematical mapping curve that quantitatively reflects the one-to-one correspondence between externally applied mechanical parameters or their induced defect density and extracted defect-sensitive optical parameters. An unknown region refers to the target measurement area on the sample under test that has not undergone artificial mechanical treatment, and whose internal defect state and density distribution are unknown. Atomic-level defect information refers to quantitative or semi-quantitative data used to characterize the defect state of the unknown region, including equivalent defect density, defect existence determination, and the degree of energy dissipation caused by the defect.
[0034] First, a controllable local mechanical force is applied to a selected calibration region to repeatedly induce microscopic atomic-level defects of varying densities without disrupting the macroscopic continuity of the material. Since this semiconductor heterostructure possesses defect-sensitive exciton emission characteristics, these artificially introduced atomic-level defects act as local nonradiative recombination centers to capture excitons when they move and recombine at the interface region, or perturb the exciton's ground state energy level through localized potential fluctuations. By collecting the exciton emission spectra emitted from calibration regions with different defect densities and extracting their sensitive optical parameters, a standard calibration curve can be mathematically established between the external mechanical load and the defect density, i.e., the evolution of the optical parameters. Finally, when the unknown region is irradiated using the same excitation environment, by capturing the exciton emission spectra of the unknown region and extracting the same optical parameters, and then referring back to the previously established calibration curve, a reverse quantitative deduction of the atomic-level defect information within the unknown region can be achieved.
[0035] Therefore, the embodiments of the present invention provide a non-contact, non-destructive, and quantitative optical detection method by transforming the density of microscopic atomic-level defects, which is difficult to count directly, into a highly sensitive spectral physical quantity evolution. Compared with traditional contact or high-vacuum characterization methods such as transmission electron microscopy, the detection efficiency is greatly improved, and non-destructive rapid assessment of buried defects inside devices is achieved in an atmospheric environment, effectively avoiding interference from complex sample preparation processes on the original state of the sample.
[0036] Figure 2 This is a three-dimensional structural schematic diagram of a semiconductor heterostructure with defect-sensitive exciton luminescence characteristics provided in an embodiment of the present invention. For example... Figure 2 As shown, the semiconductor heterostructure includes a semiconductor substrate, a bottom dielectric layer, a first two-dimensional semiconductor monolayer material layer, and a second two-dimensional semiconductor monolayer material layer stacked sequentially; wherein, the interlayer relative rotation angle between the first two-dimensional semiconductor monolayer material layer and the second two-dimensional semiconductor monolayer material layer is a high-symmetry coupling angle under a symmetric lattice.
[0037] Specifically, a semiconductor substrate refers to a rigid support substrate used to support the upper functional thin film materials. It is a polished single-crystal material, such as a silicon wafer (Si) with a 300-nanometer-thick silicon dioxide coating. The bottom dielectric layer refers to an ultrathin insulating material layer sandwiched between the semiconductor substrate and the two-dimensional material, providing an atomically flat surface and serving as electrical insulation or optical interference enhancement. Examples include hexagonal boron nitride (h-BN) films with a thickness ranging from 25 to 40 nanometers. The first and second two-dimensional semiconductor monolayers refer to ultrathin semiconductor material wafers with a thickness of only a single atomic layer or a single unit cell. Examples of first two-dimensional semiconductor monolayers include tungsten disulfide (WS2) monolayer films, and examples of second two-dimensional semiconductor monolayers include molybdenum diselenide (MoSe2) monolayer films. The interlayer relative rotation angle refers to the angle formed in the two-dimensional plane between the principal axes of the respective lattice frameworks of two two-dimensional materials when they are stacked together. The high symmetry coupling angle under a symmetric lattice refers to the specific rotation angle at which the degree of atomic overlap between two layers of material reaches a local maximum due to the lattice symmetry of the two-dimensional material itself, resulting in extremely strong interlayer electron coupling.
[0038] Using dry transfer and other processes, a first two-dimensional semiconductor monolayer and a second two-dimensional semiconductor monolayer are sequentially stacked on a semiconductor substrate that has undergone bottom dielectric layer planarization. When the relative rotation angle between the two two-dimensional semiconductor monolayers is at a high symmetry coupling angle, their lattice wavefunction overlap in the vertical direction reaches a relatively high level. Under external light excitation, due to the extremely strong interlayer electron coupling, electrons and holes can be distributed or deeply hybridized across the interface, thereby generating interlayer excitons or hybrid excitons that are extremely sensitive to interlayer contact states and local potential interference, thus forming the defect-sensitive exciton luminescence characteristics described in the aforementioned embodiments.
[0039] Therefore, the embodiments of the present invention isolate the dangling bonds and impurity charge interference on the surface of the semiconductor substrate through the bottom dielectric layer, ensuring the intrinsic cleanliness of the substrate, and limiting the relative rotation angle between layers to a high symmetry coupling angle, which can ensure the maximization and stabilization of the interlayer electronic coupling strength, thereby significantly improving the response sensitivity of subsequent exciton luminescence to interface defects, and ensuring the benchmark reliability of the detection scale from the source.
[0040] In some embodiments, controlling the application of controlled local mechanical forces in a calibration region of a semiconductor heterostructure to introduce atomic-level defects of different densities into the calibration region non-destructively includes: introducing lattice vacancy defects or local strain defects of different densities in the calibration region by adjusting process control parameters of a preset process for applying controlled local mechanical forces; wherein the preset process includes at least one of controlled micro-area sliding friction process, nano-scrubbing process, and micro-area chemical mechanical polishing process, and the process control parameters include at least one of normal load, scanning speed, number of cycles, and scanning area size. In some embodiments, the preset process is a controlled micro-area sliding friction process, and the process control parameters include normal load, number of cycles, and scanning area size; wherein the normal load ranges from 50 nanoNewtons to 200 nanoNewtons, the scanning area size ranges from 2 micrometers x 2 micrometers to 5 micrometers x 5 micrometers, and the number of cycles ranges from 20 to 80.
[0041] Specifically, process control parameters refer to the core process variables that can be quantitatively adjusted and continuously input through software or hardware in micro / nano mechanical manipulation equipment. Lattice vacancy defects refer to unoccupied vacant positions left by one or more intrinsic atoms in a crystal lattice after gaining external energy and detaching from their original positions. Localized strain defects refer to the microscopic lattice constant distortion and elastic strain field caused by localized non-uniform external forces of compression or stretching. Controlled micro-area sliding friction technology refers to the operation process of using a micro-rigid probe to perform reciprocating friction within a micrometer-scale region with a set pressure and trajectory. Nanoscale scribing technology refers to the operation process of using micro / nano probes to apply continuous loads and perform unidirectional scribing at the nanoscale to produce microscopic deformation. Micro-area chemical mechanical polishing technology refers to the process of locally repairing the material surface at the micrometer scale by combining chemical etching solutions with micro-mechanical friction.
[0042] Within a selected calibration region, at least one of the following processes is executed: controlled micro-area sliding friction, nano-scrubbing, or micro-area chemical mechanical polishing. As the micro-rigid contact body moves across the material surface, by precisely adjusting at least one of the process control parameters—normal load, scanning speed, number of cycles, or scanning area size—the externally input mechanical energy overcomes part of the intrinsic lattice binding energy of the two-dimensional material. Within a safe threshold that does not disrupt the macroscopic, large-scale layered continuity of the material, this localized shear force and normal stress will, with a high probability, strip away trace amounts of weakly bonded atoms or induce lattice dislocations, thereby hierarchically forming lattice vacancy defects or localized strain defects of varying densities from low to high within the calibration region. This achieves precisely controlled artificial introduction of microscopic defect density.
[0043] Therefore, the embodiments of the present invention solve the technical bottleneck of randomness and uncontrollability in the introduction of atomic-level defects in traditional technologies. Through the synergistic complementarity of various mechanical processes and parameters, it is possible to achieve continuous, hierarchical and highly repeatable adjustment of defect density in a very small micrometer-level region, providing a physical basis for the subsequent establishment of highly accurate defect response calibration curves.
[0044] Figure 3 This is a schematic diagram comparing the photoluminescence spectra of a semiconductor heterostructure and a monolayer material provided in an embodiment of the present invention. Figure 3As shown, the horizontal axis represents energy in electron volts (eV), and the vertical axis represents luminescence intensity in relative units. Three independent emission spectrum curves are presented. The bottom curve represents the intrinsic emission peak of a monolayer tungsten disulfide film, located at approximately 2.01 eV. The middle curve represents the intrinsic emission peak of a monolayer molybdenum diselenide film, located at approximately 1.57 eV. The top curve represents the spectral signal of a semiconductor heterostructure, exhibiting a high-intensity emission peak at approximately 1.53 eV. This peak is shifted by 40 millielectron volts towards lower energies compared to the intrinsic emission peak of the monolayer molybdenum diselenide film, i.e., a redshift. This characteristic emission peak is the hybrid exciton emission peak of this embodiment of the invention, demonstrating the successful construction of the interlayer coupling effect in this embodiment.
[0045] Figure 4 This is a schematic diagram illustrating a test result for obtaining the relative orientation of a semiconductor heterostructure through second harmonic testing, provided by an embodiment of the present invention. Figure 4 As shown, the polar coordinate polarization spectrum includes spatial angle scales of 0 degrees, 90 degrees, 180 degrees and 270 degrees, as well as two nonlinear optical polarization response curves composed of gray solid lines and scattered dots, which are distributed in a petal-like multi-leaf pattern, corresponding to molybdenum diselenide monolayer film and tungsten disulfide monolayer film, respectively. Figure 4 The overlapping trend of the main axis lobes shown indicates that the interlayer relative rotation angle between the first two-dimensional semiconductor monolayer and the second two-dimensional semiconductor monolayer is maintained at a high symmetry coupling angle of 0 degrees under the symmetric lattice, in order to ensure the excitation efficiency of hybrid excitons.
[0046] In some embodiments, obtaining an exciton emission spectrum signal includes: using a continuous laser or a pulsed laser as an excitation source to irradiate a calibration region to obtain an exciton emission spectrum signal; wherein the wavelength of the excitation source covers the intrinsic exciton transition energy range of the two-dimensional semiconductor monolayer material in the semiconductor heterostructure, and the incident power of the excitation source is less than or equal to the incident power threshold.
[0047] Specifically, continuous laser and pulsed laser refer to laser beams that output energy continuously in time or periodically in the form of extremely short pulses, respectively. An excitation source refers to an external optical energy source used to input energy into semiconductor materials to generate non-equilibrium electron-hole pairs. The intrinsic exciton transition energy range refers to the characteristic energy range required for the direct formation of intrinsic excitons within a single layer of a two-dimensional semiconductor material due to light absorption without defect interference. The incident power threshold refers to the maximum safe power limit for excitation; if this value is exceeded, the thermal effect caused by the incident light energy will lead to physical ablation, interlayer delamination, or uncontrolled thermal defects in the two-dimensional material.
[0048] A continuous or pulsed laser beam is focused into a micrometer-scale spot using a microscope objective to illuminate a calibrated or unknown region. The wavelength of the excitation source is precisely selected within the intrinsic exciton transition energy range covering the components of the two-dimensional material. This ensures that photon energy is efficiently absorbed by the material and converted into primary electron-hole pairs. These primary carriers, under strong interlayer coupling, rapidly relax and recombine to form excitons with defect-sensitive properties. Simultaneously, the incident power of the excitation source is strictly limited below the incident power threshold using components such as optical attenuators. This ensures that only pure optical excitation and recombination processes occur within the sample during testing, without any unexpected thermally induced structural morphology degradation.
[0049] Therefore, the embodiments of the present invention ensure the non-destructive and intrinsic nature of the characterization method. By accurately matching the excitation wavelength and strictly capping the incident power threshold, the secondary damage to the two-dimensional semiconductor structure caused by the testing process itself is reduced to the greatest extent, ensuring that the measured spectral signal can truly and objectively reflect the inherent micro-defect distribution state of the material.
[0050] In some embodiments, establishing a defect response calibration curve between atomic-level defect density and defect-sensitive optical parameters includes: obtaining the peak energy value and integrated luminescence intensity of the hybrid exciton emission peak in the exciton emission spectrum signal generated by excitation in the calibration region under different mechanically applied normal loads; establishing an energy level shift calibration curve between the normal load and the peak energy value; and establishing an intensity attenuation calibration curve between the normal load and the integrated luminescence intensity, so as to jointly constitute the defect response calibration curve.
[0051] Specifically, the hybrid exciton emission peak refers to the characteristic emission spectral peak generated in the photoluminescence spectrum due to the deep hybridization of the interlayer wavefunctions between the first and second two-dimensional semiconductor monolayers. The peak energy value refers to the energy value on the abscissa corresponding to the highest point of the emission peak, expressed in electron volts. The integrated luminescence intensity refers to the total geometric area enclosed by the emission peak curve and the abscissa within a certain spectral energy band, representing the total number of photons emitted by radiative recombination. The energy level shift calibration curve is a broken line or fitted curve with the mechanical normal load as the abscissa and the change in peak energy of the hybrid exciton emission peak as the ordinate. The intensity decay calibration curve is a broken line or fitted curve with the mechanical normal load as the abscissa and the decrease in the integrated luminescence intensity of the hybrid exciton emission peak as the ordinate.
[0052] After applying different mechanical normal loads to the calibration region, the exciton emission spectrum signals generated in each region were measured one by one, and the characteristic hybrid exciton emission peaks were located from the measured spectra. As the applied normal load gradually increases, the density of artificially introduced lattice vacancy defects or local strain defects increases monotonically. First, the increase in defects introduces a large number of local deep-level traps, which easily trap excitons during movement and cause nonradiative recombination, resulting in a sharp decrease in the total number of emitted photons, which is manifested in a continuous decrease in the integral emission intensity in the macroscopic spectrum. Second, atomic-level defects disrupt the original periodic potential field of the interface, causing perturbations in the local electronic structure or changes in the interface Coulomb shielding effect, which leads to a shift of the ground state bound energy level of the exciton to a lower energy direction, which is manifested in a continuous redshift of the peak energy value in the macroscopic spectrum. The peak energy values extracted under different normal loads and the integral emission intensity are respectively connected by discrete points or fitted by functions to construct the corresponding energy level shift calibration curve and intensity attenuation calibration curve, which are combined to form the defect response calibration curve.
[0053] Therefore, by introducing the joint calibration of energy level and intensity as dual physical quantities, the embodiments of the present invention largely overcome the saturation phenomenon or signal fluctuation error that is prone to occur with a single optical parameter. The energy level shift calibration curve and the intensity attenuation calibration curve are independent of each other but complementary to each other, which greatly improves the mathematical stability and quantitative back-calculation resolution of the entire calibration curve, laying the foundation for the accurate quantification of micro-defect density.
[0054] Figure 5 This is a schematic diagram illustrating the non-destructive introduction of atomic-level defects of different densities into a calibration area using an atomic force microscope sliding friction process, as provided in an embodiment of the present invention. Figure 5 As shown, the image includes the contact probe (AFM tip) of an atomic force microscope, the functional layers of a stacked semiconductor heterostructure, and four discrete micro-cube calibration regions defined on the surface of a molybdenum diselenide monolayer film. These four calibration regions are labeled with normal load parameters of 50 nanoNewtons, 100 nanoNewtons, 150 nanoNewtons, and 200 nanoNewtons, respectively. Figure 5 This visually demonstrates the micro-nano mechanical manipulation process that introduces lattice vacancy defects or local strain defects of different densities into the subsurface layer of a heterostructure by controlling the application of different mechanical process control parameters to different regions using a probe.
[0055] Figure 6 This is a schematic diagram of the surface morphology of a calibration region after being subjected to different normal loads, provided by an embodiment of the present invention. (See diagram below.) Figure 6As shown, the image uses a grayscale height rendering mode to display the microscopic undulations of the material surface. Below is a height rendering bar, with a height scale ranging from 0 nanometers to 130 nanometers, representing the relative height corresponding to colors from dark to light. The physical length of the line segment scale is 10 micrometers. The image clearly outlines four marked areas (1, 2, 3, and 4) that have undergone controlled sliding friction treatment. Their surface morphology remains relatively flat and continuous, without obvious macroscopic peeling, material loss, or breakage, proving that the introduced defects are non-destructive in terms of macroscopic structure.
[0056] In some embodiments, after obtaining the exciton emission spectrum signal of the unknown region, the method further includes: when the exciton emission spectrum signal of the unknown region, compared with the exciton emission spectrum signal of the defect-free reference region, shows a decrease in the integrated emission intensity of the hybrid exciton emission peak and a redshift of the peak energy value to a lower energy direction, it is determined that there is an atomic-level defect in the unknown region.
[0057] Specifically, a defect-free reference region refers to a well-preserved area on the sample under test that has not been subjected to external mechanical damage and maintains excellent intrinsic lattice integrity, serving as an optical reference for qualitative comparison. Redshift refers to the physical phenomenon where the center position or energy peak of a spectral peak shifts towards a lower energy and longer wavelength. After obtaining the spectrum of the unknown region, it is compared one-to-one with the spectrum of the defect-free reference region under the same testing environment. If the spectral signal of the unknown region is within the hybrid exciton characteristic band and simultaneously satisfies the following two physical characteristics: a significant decrease in the integrated luminescence intensity of the hybrid exciton emission peak, and a clear redshift of the peak's energy value towards lower energies, then the decrease in integrated luminescence intensity proves the existence of a relatively efficient non-radiative recombination energy dissipation channel within the micro-region, while the redshift of the peak's energy value confirms that the local electronic band structure has been strongly perturbed by deep-level defect states. Only when both characteristics are simultaneously present can it be uniquely confirmed that the change is caused by atomic-level defects, thus determining the existence of atomic-level defects in the unknown region.
[0058] Therefore, this invention establishes a highly reliable joint criterion for qualitative identification of atomic-level defects. Since macroscopic non-defect factors such as environmental pollution and substrate fluctuations usually only cause local changes in luminescence intensity, and rarely cause a characteristic redshift of the interlayer hybrid exciton energy level, this dual-feature joint criterion largely eliminates the interference of external stray signals and effectively avoids false alarms and false negatives in defect identification.
[0059] In some embodiments, obtaining atomic-level defect information in an unknown region includes: controlling an excitation light source to perform a two-dimensional dot matrix scan on the test plane of a semiconductor heterostructure to obtain the equivalent atomic-level defect density value corresponding to each scan point, and using the equivalent atomic-level defect density value corresponding to each scan point as atomic-level defect information; the method further includes: mapping the equivalent atomic-level defect density value to spatial coordinates to obtain a two-dimensional defect morphology imaging map showing the spatial non-uniform distribution of atomic-level defects.
[0060] Specifically, two-dimensional dot matrix scanning refers to controlling the focused micron-sized spot of the excitation light source to perform grid-like point-by-point illumination measurement on the plane under test according to a set row and column step size. The equivalent atomic-level defect density value refers to the spectral parameters measured at a certain scanning point in an unknown region, calculated by referring to a standard calibration curve, and equivalent to the microscopic defect concentration value corresponding to the force of mechanical friction experienced. Spatial coordinate mapping refers to the process of using a computer data processing system to bind the two-dimensional coordinates of each scanning point in physical space to the calculated defect density value at that point. Two-dimensional defect morphology imaging refers to using different colors or gray levels to represent different defect density values, ultimately outputting a two-dimensional pixel-mapped image that intuitively displays the spatial arrangement and non-uniform distribution characteristics of defects on the material surface and subsurface. The equivalent atomic-level defect density value is a specific quantitative representation of the atomic-level defect information described in the aforementioned embodiments under spatial scanning mode; that is, by converting discrete spectral signals point by point into specific density values, the abstract defect information obtains a clear physical spatial dimension mapping.
[0061] Using a precision two-dimensional moving stage or galvanometer scanning mirror, the excitation spot is driven to perform a grid-like two-dimensional dot matrix scan on the test plane of the semiconductor heterostructure. Each time the spot moves to a discrete coordinate point, the spectrometer simultaneously acquires the exciton emission spectrum signal of that local micro-region, extracts its sensitive optical parameters, and refers back to the defect response calibration curve described in the previous embodiments. The system then automatically calculates and outputs the equivalent atomic-level defect density value specific to that point. After completing the full-area scan, the data processing module performs spatial coordinate mapping on the equivalent atomic-level defect density values of all coordinate points, converting them into corresponding image pixel matrices, and finally outputs a two-dimensional defect morphology image.
[0062] Thus, the embodiments of the present invention achieve a technological leap from isolated point measurement to intuitive imaging of large-area defects. Since atomic-level defects have high spatial non-uniformity in interface transfer and processing, this imaging technology can help engineers intuitively locate weak areas and damage trajectories of material interfaces at the micrometer to millimeter scale, providing extremely intuitive and traceable data support for evaluating the overall uniformity of semiconductor devices.
[0063] Figure 7This is a schematic diagram comparing the photoluminescence spectra of a calibration region extracted under different frictional loads, provided by an embodiment of the present invention. Figure 7 As shown, the horizontal axis represents energy in electron volts, and the vertical axis represents luminescence intensity in counts. From top to bottom, there are four exciton emission spectrum curves that show a monotonically collapsing trend. The four curves are pointed to by arrows and correspond to mechanical normal loads of 50 nanonewtons, 100 nanonewtons, 150 nanonewtons, and 200 nanonewtons, respectively. Figure 7 The spectral evolution features shown clearly demonstrate the microscopic nonradiative recombination energy dissipation law of the hybrid exciton emission peak, which shows a significant decrease in the integrated luminescence intensity as the normal load increases, the atomic-level defect density increases, and the energy value of the peak center gradually shifts to the left, i.e., redshift.
[0064] Figure 8 This is a schematic diagram illustrating the relationship between the peak energy value of a hybrid exciton emission peak and the processing load, according to an embodiment of the present invention. Figure 8 As shown, the energy level shift calibration curve in the defect response calibration curve described in the aforementioned embodiment represents the mechanical normal load on the horizontal axis, in nanonewtons, and the vertical axis represents the peak energy value, in electron volts. Figure 8 The broken line clearly records the evolution of the hybrid exciton peak energy as the load increases from 50 nanonewtons to over 100 nanonewtons, from nearly 1.543 electron volts to about 1.541 electron volts, and then tends to level off. This is used to establish a calibration benchmark for defect-induced energy level distortion.
[0065] Figure 9 This is a schematic diagram illustrating the relationship between the integrated luminescence intensity of a hybrid exciton emission peak and the processing load, according to an embodiment of the present invention. Figure 9 As shown, the intensity attenuation calibration curve in the defect response calibration curve described in the aforementioned embodiment represents the mechanical normal load on the horizontal axis, with the unit being nanonewtons, and the vertical axis representing the integrated luminescence intensity, expressed in relative numerical values. Figure 9 The broken line clearly shows the evolution trend of the integral luminescence intensity value linearly decreasing from 26.8 to about 13.4 as the load monotonically increases and the equivalent defect density increases, which is used to establish a calibration benchmark for defect-induced nonradiative composite quenching.
[0066] In some embodiments, after nondestructively introducing atomic-level defects of different densities into the calibration region, the method further includes: obtaining a ratio parameter as a second defect-sensitive optical parameter; wherein the ratio parameter is the ratio of the integrated luminescence intensity of the hybrid exciton emission peak in the exciton emission spectrum signal to the integrated luminescence intensity of the intrinsic exciton emission peak of the two-dimensional semiconductor monolayer material in the semiconductor heterostructure; establishing an auxiliary ratio calibration curve between the mechanically applied normal load and the ratio parameter; and calibrating the atomic-level defect information for environmental disturbance error based on the ratio parameter measured in the unknown region and the auxiliary ratio calibration curve.
[0067] Specifically, the second defect-sensitive optical parameter refers to a newly introduced composite multi-characteristic parameter, distinct from the single type of absolute optical parameter described in the aforementioned embodiments. The ratio parameter refers to a relative scaling physical quantity obtained by mathematically dividing the intensities of two emission peaks from different physical origins. The intrinsic exciton emission peak refers to the material's inherent radiation emission peak, generated by the direct recombination of electrons and holes within each layer of the first or second two-dimensional semiconductor monolayer, and relatively insensitive to interface defects. The auxiliary ratio calibration curve refers to another standard reference curve established with the mechanically applied normal load as the abscissa and the calculated ratio parameter as the ordinate. Environmental disturbance error calibration refers to using a relative ratio stabilization mechanism to deduct measurement errors caused by external non-defect environmental noise such as light source power divergence and slight unevenness in substrate reflectivity. In terms of execution order, this step is started simultaneously after the non-destructive introduction of atomic-level defects of different densities in the calibration area is completed. By adding a parallel calculation branch to extract ratio parameters and establish auxiliary ratio calibration curves while acquiring spectral signals, and performing cross-validation and error subtraction with the defect response calibration curve when finally obtaining defect information.
[0068] When the excitation source irradiates the material, the spectrometer simultaneously acquires the intrinsic exciton emission peak of the two-dimensional semiconductor monolayer while collecting the hybrid exciton emission peak. The data processing module divides the integrated luminescence intensity of the hybrid exciton emission peak by the integrated luminescence intensity of the intrinsic exciton emission peak to obtain the ratio parameter. External environmental disturbances, such as slow drift in laser output power, slight defocusing of the microscope, and local thickness fluctuations in the substrate silicon dioxide layer, will proportionally amplify or reduce the overall luminescence intensity in the micro-region. Therefore, although the absolute intensities of the intrinsic peak and the hybrid peak change, their ratio remains largely constant. Conversely, atomic-level defects are located at the interface between the two layers. Because the wavefunction of the hybrid exciton is distributed across the interface, the probability of it being trapped by the interface defect and undergoing nonradiative recombination is much higher than that of the intrinsic exciton moving within the monolayer material. Therefore, when the load increases and the number of defects increases, the intensity of the hybrid exciton peak drops sharply, while the intensity of the intrinsic exciton peak changes only slightly. This causes the ratio parameter to exhibit an extremely sensitive monotonous and drastic decline. By establishing an auxiliary ratio calibration curve and using this ratio for cross-referencing when measuring in unknown regions, environmental disturbance error calibration can be effectively achieved.
[0069] Therefore, this invention introduces an optical internal standard calibration mechanism, which completely eliminates the interference of external environmental fluctuations on the quantitative results of defects in terms of physical mechanism. This significantly reduces the dependence of the characterization method on the stability of the optical hardware system. Even under complex working conditions such as slight vibration, light source drift or uneven chip surface thickness in industrial field, it can still output highly reliable atomic-level quantitative defect data.
[0070] In some embodiments, after nondestructively introducing atomic-level defects of different densities into the calibration region, the method further includes: controlling the application of a continuously scanning control voltage to the semiconductor heterostructure; obtaining the differential modulation spectral line of the integral luminescence intensity of the hybrid exciton emission peak in the exciton emission spectrum signal as a function of the control voltage, as a third defect-sensitive optical parameter; and obtaining the charge state of the atomic-level defects in the unknown region and the location of the deep energy level of the defects through the characteristic jump points in the differential modulation spectral line.
[0071] Specifically, the control voltage refers to the external bias electric field voltage applied to the control electrode of the heterostructure, whose magnitude changes linearly or stepwise with time. The differential modulation spectral line refers to the differential emission spectrum characteristic curve obtained by taking the first-order or higher-order mathematical derivative of the collected hybrid exciton emission intensity as a function of the control voltage. The third defect-sensitive optical parameter refers to the electro-optic recombination physical parameter obtained through active electric field modulation, containing the dynamic charging and discharging characteristics of the defect energy levels. The characteristic jump point refers to the peak, trough, or inflection point appearing on the differential modulation spectral line due to a discontinuous abrupt change in the response rate of emission intensity to voltage. The charged state refers to the electrostatic properties exhibited by the defect in the microcrystalline lattice, including neutral state, positively charged donor state, or negatively charged acceptor state. The deep energy level position of the defect refers to the precise energy position of the atomic-level defect within the semiconductor bandgap, representing the potential well depth of its bound excitons or charge carriers. In terms of execution sequence, after applying controlled local mechanical action, during the acquisition of spectral signals, this step actively and synchronously applies a control voltage via an external control electrode. At this point, it no longer passively extracts steady-state optical parameters, but instead aligns spectral acquisition and voltage scanning in time, obtaining differentially modulated spectral lines as the third defect-sensitive optical parameter. This is used to output the electrical properties and deep energy level information of the defects in addition to the defect density. The two are nested and synchronously run in a progressive relationship on the time axis.
[0072] By applying a continuously scanning control voltage to a semiconductor heterostructure through control electrodes, a micro-modulated electric field is established in the vertical or bias direction. Due to the extremely high surface area of two-dimensional semiconductor materials, the external electric field can efficiently electrostatically dope them, driving continuous up-and-down movement of the Fermi level within the semiconductor. When the Fermi level, driven by the voltage, happens to pass over the bound energy level of the atomic-level defect at the interface, the defect undergoes micro-charging and discharging behavior. The change in the defect's charge state causes a sudden change in the surrounding local Coulomb scattering field, resulting in a precipitous change in the nonradiative recombination cross-section of the trapped excitons. Macroscopically, this manifests as a dramatic nonlinear jump in the hybrid exciton luminescence intensity at a specific voltage point. By mathematically differentiating the luminescence intensity-voltage curve, these minute jumps are amplified into characteristic jump points on the differential modulation spectrum. By recording the control voltage value corresponding to these characteristic jump points and combining it with a semiconductor bandgap model, the charge state of the atomic-level defect and the position of its deep energy level can be accurately calculated.
[0073] The following is a detailed explanation of the atomic-level defect characterization method based on defect-sensitive exciton luminescence response, using a specific example: The core idea of this invention is to use the energy dissipation of defect-sensitive excitons as a probe that is highly sensitive to atomic-level defects at the interface, extract the intensity and energy level of the emission peak of defect-sensitive excitons in the exciton emission spectrum signal, establish the correspondence between defects, nonradiative recombination, and spectral response, and achieve non-destructive characterization of atomic-level defects.
[0074] First, device and sample construction is performed. Specifically, a molybdenum diselenide / tungsten disulfide heterostructure device is fabricated. The semiconductor heterostructure includes a semiconductor substrate, a bottom dielectric layer, a first two-dimensional semiconductor monolayer, and a second two-dimensional semiconductor monolayer, stacked sequentially. For example, the bottom dielectric layer is hexagonal boron nitride, the first two-dimensional semiconductor monolayer is a single layer of tungsten disulfide, and the second two-dimensional semiconductor monolayer is a single layer of molybdenum diselenide. The entire device is assembled onto a silicon wafer with a 300 nm thick silicon dioxide layer using a dry transfer method. Before or during device assembly, controlled local mechanical forces are applied to a calibrated region of the semiconductor heterostructure. For example, controlled friction treatment is performed on the top molybdenum diselenide surface using a contact atomic force microscope probe to introduce subsurface atomic-level disorder or vacancy defects with adjustable density. The process control parameters for the controlled local mechanical forces can be characterized by normal load, scan rate, number of cycles, and scan area size. Preferably, the atomic force microscope probe applies a load of 50 to 200 nanonewtons, the scanning area size is 2 to 5 micrometers by 2 to 5 micrometers, and the number of scanning cycles is 20 to 80. By adjusting the applied load or the number of scans, the atomic-level defect density can be graded. Furthermore, this controlled local mechanical action can also be replaced by other controlled micro-area sliding friction processes, nano-scrubbing processes, or micro-area chemical mechanical polishing processes to introduce different types or densities of atomic-level defects.
[0075] Then, spectral measurements are performed. Specifically, in this embodiment of the invention, the sample is excited using exciton emission spectral signals, and its emission signals are collected. During the test, a continuous laser or pulsed laser is selected as the excitation source, with the excitation wavelength covering the exciton transition energy range of monolayer materials, preferably a laser source in the range of 600 to 800 nanometers. The excitation light is focused onto the sample surface through a microscope objective, forming a micrometer-scale spot to achieve localized excitation. By adjusting the excitation power, the incident power is kept within a range that will not cause thermal effects or structural damage to the sample, preferably in the nanowatt to microwatt range. The light signal emitted by the sample is collected by the objective and then dispersed in a spectrometer, and the exciton emission spectral signal is recorded by a high-sensitivity detector.
[0076] Subsequently, spectral analysis was performed. Specifically, the exciton emission spectrum signal was analyzed to extract the intensity and energy level of the emission peak of defect-sensitive excitons. The obtained exciton emission spectrum signal was analyzed, focusing on extracting the integrated emission intensity and peak energy information of the defect-sensitive exciton emission peak. In defect-free or low-defect regions, defect-sensitive excitons typically exhibit strong and stable emission signals, with their peak positions remaining largely consistent. However, in regions with atomic-level defects, the introduction of nonradiative recombination channels by the defects causes energy dissipation of excitons before recombination, resulting in a significant decrease in emission intensity. Simultaneously, atomic-level defects induce local electronic structure perturbations, leading to changes in exciton energy levels, which are manifested in the spectrum as a redshift of the emission peak position. As the degree of atomic-level defects increases, the emission peak position gradually shifts towards lower energies. By normalizing the emission intensity in different regions and analyzing the peak position changes, a correlation between atomic-level defect density and emission intensity attenuation and peak redshift can be established.
[0077] Finally, defect determination is performed. Specifically, under fixed interlayer rotation angle and consistent testing conditions, the exciton emission spectra of the target region and the reference region are compared and analyzed. When the target region simultaneously exhibits a decrease in the emission intensity of defect-sensitive excitons and a redshift of the emission peak position towards lower energies, this characteristic combination can be used as a spectral criterion for identifying the presence of atomic-level defects. Based on the joint criterion of emission intensity change and peak position shift, the identification and quantitative characterization of atomic-level defects are achieved by analyzing the intensity reduction and spectral redshift characteristics. Furthermore, by normalizing the emission intensity and calculating the degree of intensity change of the target region relative to the reference region, combined with the shift of the emission peak position, the change in emission response caused by defects can be quantitatively or semi-quantitatively characterized, thereby achieving an assessment of the degree of defect impact.
[0078] In summary, this invention uses defect-sensitive exciton luminescence response as a non-destructive optical probe for interface or subsurface atomic-level defects. The integrated luminescence intensity, peak energy, linewidth, and spatial inhomogeneity of defect-sensitive exciton peaks are extracted through exciton luminescence spectral signals or spatially resolved exciton luminescence imaging and used for defect identification. Atomic-level defects are identified based on a joint criterion of integrated luminescence intensity quenching, peak energy shift, and changes in linewidth or spatial inhomogeneity. An atomic-level defect density gradient is constructed using controlled micro-area sliding friction, nano-scratching, micro-area chemical mechanical polishing, or other controllable contact processes, and a defect response calibration curve is established. Quantitative or semi-quantitative evaluation of atomic-level defects is achieved using normalized intensity quenching factors, peak offset, linewidth variation, or a comprehensive defect response index. The defect response calibration curve or comprehensive defect response index is used for estimating atomic-level defect density in unknown regions, imaging defect spatial distribution, and screening process reliability. This method can be applied to two-dimensional van der Waals heterostructures, hexagonal boron nitride packaging structures, gate-controlled heterostructures, or other semiconductor heterostructures with defect-sensitive exciton luminescence responses.
[0079] Therefore, the defect-sensitive exciton response can be read from the exciton emission spectrum signal without destroying the sample structure or requiring complex cross-sectional sample preparation. Utilizing the sensitivity of defect-sensitive excitons to interlayer coupling, localized trapped states, and non-radiative recombination channels, the influence of atomic-level defects that are difficult to identify in ordinary morphology images can be amplified. The two-dimensional distribution of the defect response can be obtained through spectral scanning or imaging spectroscopy, suitable for rapid screening in the micrometer to millimeter scale region. By constructing a calibration region through controlled local mechanical action, a quantitative or semi-quantitative relationship between the degree of atomic-level defects and the emission response can be established. This can be integrated with two-dimensional material transfer, encapsulation, gated device fabrication, localized tribology, micro-area polishing, and reliability testing processes. In addition to molybdenum diselenide / tungsten disulfide, it can also be extended to other two-dimensional semiconductor heterostructures with defect-sensitive exciton emission characteristics.
[0080] It should be noted that the materials, structures, wavelengths, loads, number of scans, fitting functions, and threshold ranges given in the embodiments of the present invention are all preferred embodiments and should not be construed as limiting the scope of protection of the present invention. All technical solutions that achieve non-destructive identification, localization, classification, or quantitative evaluation of atomic-level defects based on defect-sensitive exciton luminescence response should be included in the scope of protection of the present invention.
[0081] This invention also provides an atomic-level defect characterization device based on defect-sensitive exciton luminescence response. Figure 10 This is a schematic diagram of an atomic-level defect characterization device based on defect-sensitive exciton luminescence response provided in an embodiment of the present invention. Figure 10As shown, the atomic-level defect characterization device based on defect-sensitive exciton emission response includes: a defect introduction module 201, used to control the application of controlled local mechanical action in the calibration region of a semiconductor heterostructure to introduce atomic-level defects of different densities into the calibration region without damage; wherein, the semiconductor heterostructure is constructed to have defect-sensitive exciton emission characteristics; a calibration establishment module 202, used to obtain at least one defect-sensitive optical parameter of the semiconductor heterostructure based on the exciton emission spectrum signal of the calibration region under different atomic-level defect densities, and to establish a defect response calibration curve between the atomic-level defect density and the defect-sensitive optical parameter; and a defect characterization module 203, used to obtain the defect-sensitive optical parameter of the unknown region based on the exciton emission spectrum signal of the unknown region in the semiconductor heterostructure, and to obtain the atomic-level defect information of the unknown region based on the defect-sensitive optical parameter of the unknown region and the defect response calibration curve.
[0082] This invention also provides an electronic device. Figure 11 This is a schematic diagram of the structure of an electronic device provided in an embodiment of the present invention. Figure 11 As shown, the electronic device may include: a processor 401, a communication interface 402, a memory 403, and a communication bus 404, wherein the processor 401, the communication interface 402, and the memory 403 communicate with each other via the communication bus 404. The processor 401 can call logical instructions in the memory 403 to execute an atomic-level defect characterization method based on defect-sensitive exciton luminescence response, including: Controlled local mechanical forces are applied to a calibration region of a semiconductor heterostructure to introduce atomic-level defects of different densities into the calibration region without damage; wherein the semiconductor heterostructure is constructed to have defect-sensitive exciton luminescence characteristics; At least one defect-sensitive optical parameter of the semiconductor heterostructure is obtained based on the exciton emission spectrum signal of the calibration region under different atomic-level defect densities, and a defect response calibration curve between atomic-level defect density and defect-sensitive optical parameter is established. The defect-sensitive optical parameters of the unknown region are obtained from the exciton emission spectrum signal of the unknown region in the semiconductor heterostructure, and the atomic-level defect information of the unknown region is obtained from the defect-sensitive optical parameters and defect response calibration curve of the unknown region.
[0083] Furthermore, the logical instructions in the aforementioned memory 403 can be implemented as software functional units and, when sold or used as independent products, can be stored in a computer-readable storage medium. Based on this understanding, the technical solution of the present invention, essentially, or the part that contributes to the prior art, or a part of the technical solution, can be embodied in the form of a software product. This computer software product is stored in a storage medium and includes several instructions to cause a computer device (which may be a personal computer, server, or network device, etc.) to execute all or part of the steps of the methods of the various embodiments of the present invention. The aforementioned storage medium includes various media capable of storing program code, such as USB flash drives, portable hard drives, read-only memory (ROM), random access memory (RAM), magnetic disks, or optical disks.
[0084] This invention also provides a computer program product, which includes a computer program that can be stored on a non-transitory computer-readable storage medium. When the computer program is executed by a processor, the computer can perform the above-described atomic-level defect characterization method based on defect-sensitive exciton luminescence response, including: Controlled local mechanical forces are applied to a calibration region of a semiconductor heterostructure to introduce atomic-level defects of different densities into the calibration region without damage; wherein the semiconductor heterostructure is constructed to have defect-sensitive exciton luminescence characteristics; At least one defect-sensitive optical parameter of the semiconductor heterostructure is obtained based on the exciton emission spectrum signal of the calibration region under different atomic-level defect densities, and a defect response calibration curve between atomic-level defect density and defect-sensitive optical parameter is established. The defect-sensitive optical parameters of the unknown region are obtained from the exciton emission spectrum signal of the unknown region in the semiconductor heterostructure, and the atomic-level defect information of the unknown region is obtained from the defect-sensitive optical parameters and defect response calibration curve of the unknown region.
[0085] In another aspect, the present invention also provides a non-transitory computer-readable storage medium having a computer program stored thereon, which, when executed by a processor, is implemented to perform the above-described atomic-level defect characterization method based on defect-sensitive exciton luminescence response, comprising: Controlled local mechanical forces are applied to a calibration region of a semiconductor heterostructure to introduce atomic-level defects of different densities into the calibration region without damage; wherein the semiconductor heterostructure is constructed to have defect-sensitive exciton luminescence characteristics; At least one defect-sensitive optical parameter of the semiconductor heterostructure is obtained based on the exciton emission spectrum signal of the calibration region under different atomic-level defect densities, and a defect response calibration curve between atomic-level defect density and defect-sensitive optical parameter is established. The defect-sensitive optical parameters of the unknown region are obtained from the exciton emission spectrum signal of the unknown region in the semiconductor heterostructure, and the atomic-level defect information of the unknown region is obtained from the defect-sensitive optical parameters and defect response calibration curve of the unknown region.
[0086] The device embodiments described above are merely illustrative. The units described as separate components may or may not be physically separate, and the components shown as units may or may not be physical units; that is, they may be located in one place or distributed across multiple network units. Some or all of the modules can be selected to achieve the purpose of this embodiment according to actual needs. Those skilled in the art can understand and implement this without any creative effort.
[0087] Through the above description of the embodiments, those skilled in the art can clearly understand that each embodiment can be implemented by means of software plus necessary general-purpose hardware platforms, and of course, it can also be implemented by hardware. Based on this understanding, the above technical solutions, in essence or the part that contributes to the prior art, can be embodied in the form of a software product. This computer software product can be stored in a computer-readable storage medium, such as ROM / RAM, magnetic disk, optical disk, etc., and includes several instructions to cause a computer device, which may be a personal computer, server, or network device, etc., to execute the methods of various embodiments or some parts of embodiments.
[0088] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. An atomic-level defect characterization method based on defect-sensitive exciton luminescence response, characterized in that, include: Controlled local mechanical forces are applied to a calibration region of a semiconductor heterostructure to introduce atomic-level defects of different densities into the calibration region without damage; wherein the semiconductor heterostructure is constructed to have defect-sensitive exciton luminescence characteristics. Based on the exciton emission spectrum signals of the calibration region under different atomic-level defect densities, at least one defect-sensitive optical parameter of the semiconductor heterostructure is obtained, and a defect response calibration curve between atomic-level defect density and the defect-sensitive optical parameter is established. The defect-sensitive optical parameters of the unknown region are obtained from the exciton emission spectrum signal of the unknown region in the semiconductor heterostructure, and the atomic-level defect information of the unknown region is obtained from the defect-sensitive optical parameters of the unknown region and the defect response calibration curve.
2. The atomic-level defect characterization method based on defect-sensitive exciton luminescence response according to claim 1, characterized in that, The semiconductor heterostructure includes a semiconductor substrate, a bottom dielectric layer, a first two-dimensional semiconductor monolayer material layer, and a second two-dimensional semiconductor monolayer material layer stacked sequentially; wherein the interlayer relative rotation angle between the first two-dimensional semiconductor monolayer material layer and the second two-dimensional semiconductor monolayer material layer is a high-symmetry coupling angle under a symmetric lattice.
3. The atomic-level defect characterization method based on defect-sensitive exciton luminescence response according to claim 2, characterized in that, The first two-dimensional semiconductor monolayer material layer is a molybdenum diselenide monolayer thin film, the second two-dimensional semiconductor monolayer material layer is a tungsten disulfide monolayer thin film, the bottom dielectric layer is a hexagonal boron nitride thin film, and the semiconductor substrate is a silicon wafer with a silicon dioxide coating on its surface.
4. The atomic-level defect characterization method based on defect-sensitive exciton luminescence response according to claim 1, characterized in that, Controlled local mechanical forces are applied to a calibrated region of a semiconductor heterostructure to non-destructively introduce atomic-level defects of varying densities into the calibrated region, including: By adjusting the process control parameters for applying the controlled local mechanical action using a preset process, lattice vacancy defects or local strain defects of different densities are introduced in stages within the calibrated area; wherein, the preset process includes at least one of controlled micro-area sliding friction process, nano-scrubbing process, and micro-area chemical mechanical polishing process, and the process control parameters include at least one of normal load, scanning speed, number of cycles, and scanning area size.
5. The atomic-level defect characterization method based on defect-sensitive exciton luminescence response according to claim 4, characterized in that, The preset process is the controlled micro-area sliding friction process, and the process control parameters include normal load, number of cycles, and scanning area size; wherein, the normal load ranges from 50 nanoNewtons to 200 nanoNewtons, the scanning area size ranges from 2 micrometers by 2 micrometers to 5 micrometers by 5 micrometers, and the number of cycles ranges from 20 to 80.
6. The atomic-level defect characterization method based on defect-sensitive exciton luminescence response according to claim 1, characterized in that, Acquiring the exciton emission spectrum signal includes: The calibration region is irradiated with a continuous laser or a pulsed laser as the excitation source to obtain the exciton emission spectrum signal; wherein the wavelength of the excitation source covers the intrinsic exciton transition energy range of the two-dimensional semiconductor monolayer material in the semiconductor heterostructure, and the incident power of the excitation source is less than or equal to the incident power threshold.
7. The atomic-level defect characterization method based on defect-sensitive exciton luminescence response according to claim 1, characterized in that, Establishing a defect response calibration curve between atomic-level defect density and the defect-sensitive optical parameter includes: The peak energy and integrated luminescence intensity of the hybrid exciton emission peak in the exciton emission spectrum signal generated by the calibration region under different normal loads applied by mechanical force are obtained. Establish an energy level shift calibration curve between the normal load and the peak energy value, and establish an intensity attenuation calibration curve between the normal load and the integrated luminescence intensity, so as to jointly constitute the defect response calibration curve.
8. The atomic-level defect characterization method based on defect-sensitive exciton luminescence response according to claim 1, characterized in that, After obtaining the exciton emission spectrum signal of the unknown region, the process also includes: When the exciton emission spectrum signal of the unknown region, compared with the exciton emission spectrum signal of the defect-free reference region, shows a decrease in the integrated emission intensity of the hybrid exciton emission peak and a redshift of the peak energy value to a lower energy direction, it is determined that there is an atomic-level defect in the unknown region.
9. The atomic-level defect characterization method based on defect-sensitive exciton luminescence response according to claim 1, characterized in that, Obtaining atomic-level defect information in the unknown region includes: The excitation light source is controlled to perform two-dimensional dot matrix scanning on the test plane of the semiconductor heterostructure to obtain the equivalent atomic level defect density value corresponding to each scanning point, and the equivalent atomic level defect density value corresponding to each scanning point is used as the atomic level defect information. The method further includes: mapping the equivalent atomic-level defect density value to spatial coordinates to obtain a two-dimensional defect morphology image showing the spatial non-uniform distribution of the atomic-level defects.
10. The atomic-level defect characterization method based on defect-sensitive exciton luminescence response according to any one of claims 1-9, characterized in that, After non-destructively introducing atomic-level defects of different densities into the calibration region, the process further includes: Obtain a ratio parameter as a second defect-sensitive optical parameter; wherein the ratio parameter is the ratio of the integrated luminescence intensity of the hybrid exciton emission peak in the exciton emission spectrum signal to the integrated luminescence intensity of the intrinsic exciton emission peak of the two-dimensional semiconductor monolayer material in the semiconductor heterostructure; Establish an auxiliary ratio calibration curve between the mechanically applied normal load and the ratio parameter; Based on the ratio parameter measured in the unknown region and the auxiliary ratio calibration curve, the atomic-level defect information is calibrated for environmental disturbance error.
11. The atomic-level defect characterization method based on defect-sensitive exciton luminescence response according to any one of claims 1-9, characterized in that, After non-destructively introducing atomic-level defects of different densities into the calibration region, the process further includes: A control voltage that is continuously scanned is applied to the semiconductor heterostructure; The differential modulation spectral line of the integral luminescence intensity of the hybrid exciton emission peak in the exciton emission spectrum signal as a function of the control voltage is obtained as the third defect-sensitive optical parameter. The charge state and deep energy level position of atomic-level defects in the unknown region are obtained by using the characteristic jump points in the differential modulation spectral lines.
12. An atomic-level defect characterization device based on defect-sensitive exciton luminescence response, characterized in that, include: A defect introduction module is used to control the application of controlled local mechanical forces in a calibration region of a semiconductor heterostructure to introduce atomic-level defects of different densities into the calibration region without damage; wherein the semiconductor heterostructure is constructed to have defect-sensitive exciton luminescence characteristics; The calibration establishment module is used to obtain at least one defect-sensitive optical parameter of the semiconductor heterostructure based on the exciton emission spectrum signal of the calibration region under different atomic-level defect densities, and to establish a defect response calibration curve between the atomic-level defect density and the defect-sensitive optical parameter. The defect characterization module is used to obtain the defect-sensitive optical parameters of the unknown region based on the exciton emission spectrum signal of the unknown region in the semiconductor heterostructure, and to obtain the atomic-level defect information of the unknown region based on the defect-sensitive optical parameters of the unknown region and the defect response calibration curve.