Electrode, wound electrode body, and secondary battery

By alternating high and low density regions on the current collector, the problem of uneven electrolyte penetration is solved, achieving uniform electrolyte diffusion and improving the performance of the electrode and the secondary battery.

CN123073014APending Publication Date: 2026-11-10TOYOTA JIDOSHA KK
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202610599333.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2025-05-08
Filing Date
2026-04-30
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

In existing secondary batteries, the electrolyte penetration within the composite material layer is uneven, making it difficult to diffuse across the entire surface and affecting electrode performance.

Method used

An electrode film was designed on a long strip current collector, with high-density and low-density regions alternately arranged along the length direction and facing each other in the thickness direction to promote electrolyte diffusion.

Benefits of technology

By optimizing the electrode structure, the uniform diffusion of the electrolyte was promoted, thereby improving the performance of the electrode and the secondary battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123073014A_ABST
    Figure CN123073014A_ABST
Patent Text Reader

Abstract

An electrode includes: a long strip-shaped current collector having a first main surface on one side in a thickness direction and a second main surface on the other side in the thickness direction, and extending along a length direction orthogonal to the thickness direction; a first electrode film provided to the first main surface; and a second electrode film provided to the second main surface, each of the first electrode film and the second electrode film including a plurality of high-density regions and a plurality of low-density regions, the plurality of high-density regions and the plurality of low-density regions being alternately arranged along the length direction, the high-density regions of the first electrode film and the low-density regions of the second electrode film being arranged along the thickness direction with the current collector interposed therebetween, and the low-density regions of the first electrode film and the high-density regions of the second electrode film being arranged along the thickness direction with the current collector interposed therebetween.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to electrodes, wound electrode bodies, and secondary batteries. Background Technology

[0002] Previously, as an electrode used in secondary batteries, International Publication No. 2021 / 132115 disclosed the following structure: each of the composite material layers disposed on both sides of the current collector contains a plurality of high-density regions and a plurality of low-density regions, and on both sides of the current collector, the high-density regions and low-density regions extending along the length direction are alternately arranged in the width direction orthogonal to the length direction. Summary of the Invention

[0003] In composite material layers containing both high-density and low-density regions, the electrolyte penetration in the high-density regions is less than that in the low-density regions. In the electrode described in International Publication No. 2021 / 132115, regions where high-density and low-density regions overlap in the thickness direction alternate in the width direction. Therefore, in the electrode described in International Publication No. 2021 / 132115, because the regions with high electrolyte penetration and those with low electrolyte penetration alternate in the width direction, there is a concern that the electrolyte may have difficulty diffusing across the entire surface.

[0004] As electrodes, sometimes a composite material layer formed by coating slurry is not used; instead, a structure in which an electrode film pre-formed as a film is attached to the current collector is employed. In this case, as described in International Publication No. 2021 / 132115 above, when regions with overlapping high-density areas in the thickness direction and regions with overlapping low-density areas in the thickness direction are alternately arranged in the width direction, the electrolyte is also difficult to diffuse across the entire surface.

[0005] This disclosure was made in view of the above-mentioned problems, and the purpose of this disclosure is to provide an electrode, a wound electrode body, and a secondary battery that can promote the diffusion of electrolyte.

[0006] The electrode according to this disclosure comprises: an elongated current collector having a first main surface on one side in the thickness direction and a second main surface on the other side in the thickness direction, and extending along a length direction orthogonal to the thickness direction; a first electrode film disposed on the first main surface; and a second electrode film disposed on the second main surface. Each of the first and second electrode films includes a plurality of high-density regions and a plurality of low-density regions. The plurality of high-density regions and the plurality of low-density regions are alternately arranged along the length direction. The high-density regions of the first electrode film and the low-density regions of the second electrode film are arranged along the thickness direction with the current collector sandwiched between them. The low-density regions of the first electrode film and the high-density regions of the second electrode film are arranged along the thickness direction with the current collector sandwiched between them.

[0007] According to the above configuration, high-density regions and low-density regions are alternately arranged along the length direction on both the first and second main surfaces of the current collector, and are arranged facing each other in the thickness direction. Thus, on both the first and second main surfaces of the current collector, the high-density and low-density regions are alternately arranged along the length direction, resulting in a substantially uniform distribution of the low-density and high-density regions. This, in turn, promotes electrolyte diffusion.

[0008] The wound electrode body based on this disclosure has the aforementioned electrode, which is wound along the aforementioned length direction.

[0009] Based on the above configuration, a wound electrode body can be provided that utilizes an electrode whose diffusion of the electrolyte is promoted.

[0010] The secondary battery based on this disclosure has the above-described wound electrode body and a housing housing that accommodates the wound electrode body.

[0011] Based on the above configuration, a secondary battery with a wound electrode body having an electrode configuration in which the diffusion of the electrolyte is promoted can be provided.

[0012] The above and other objects, features, aspects and advantages of the present invention will become apparent from the following detailed description of the invention in conjunction with the accompanying drawings. Attached Figure Description

[0013] Figure 1 This is a simplified cross-sectional view of the secondary battery involved in Embodiment 1.

[0014] Figure 2 This is a simplified top view of the positive electrode involved in Embodiment 1 after it has been unfolded.

[0015] Figure 3 This is a simplified cross-sectional view of the positive electrode involved in Embodiment 1.

[0016] Figure 4 This is a schematic diagram illustrating the manufacturing process of the positive electrode involved in Embodiment 1.

[0017] Figure 5 This is a schematic diagram illustrating the process of forming a positive electrode composite material sheet used in the positive electrode according to Embodiment 1.

[0018] Figure 6 This is a simplified cross-sectional view of the positive electrode involved in Embodiment 2. Detailed Implementation

[0019] Hereinafter, embodiments of the present disclosure will be described in detail with reference to the accompanying drawings. It should be noted that in the embodiments shown below, the same or common parts are labeled with the same reference numerals in the drawings, and their descriptions are omitted.

[0020] (Implementation Method 1)

[0021] (Secondary battery)

[0022] Figure 1 This is a simplified cross-sectional view of the secondary battery according to Embodiment 1. (Refer to...) Figure 1 The secondary battery 100 involved in Embodiment 1 is described.

[0023] The secondary battery 100 is, for example, a lithium-ion battery installed in a vehicle. It should be noted that the uses and types of the secondary battery 100 are not limited to the examples above.

[0024] The secondary battery 100 according to Embodiment 1 includes a wound electrode body 1, a housing 2, a positive terminal 3, a positive current collector 4, an external gasket 5, an internal gasket 6, and a negative current collector 7.

[0025] The electrode body 1 is wound into a spiral shape. The wound electrode body 1 is housed in the housing 2. The housing 2 has a cylindrical shape. That is, the secondary battery 100 is a cylindrical battery.

[0026] The wound electrode body 1 includes a positive electrode 10, a negative electrode 20, and a separator 30. The separator 30 is disposed between the positive electrode 10 and the negative electrode 20 in a radial direction R of the wound electrode body 1. The separator 30 separates the positive electrode 10 and the negative electrode 20. On the other hand, the separator 30 is configured to allow ions (e.g., lithium ions) to move back and forth between the positive electrode 10 (more precisely, the positive electrode active material) and the negative electrode 20 (more precisely, the negative electrode active material).

[0027] The wound electrode body 1 is composed of an electrode plate assembly formed by winding a positive electrode 10 and a negative electrode 20 through a diaphragm 30. It should be noted that in this embodiment, the positive electrode 10 and the negative electrode 20 are electrodes used in the wound electrode body 1, and their polarities are different. One of the positive electrode 10 and the negative electrode 20 corresponds to the first electrode, and the other of the positive electrode 10 and the negative electrode 20 corresponds to the second electrode.

[0028] The housing 2 has an upper surface 2a, a lower surface 2b, and a side surface 2c. The upper surface 2a is the side of the housing 2 located axially in the cylindrical shape. Viewed from the perspective of the wound electrode body 1, the upper surface 2a is located on one side Z1 along the axial direction Z of the wound electrode body 1. The lower surface 2b is the side of the housing 2 located on the other side Z2 along the axial direction Z of the cylindrical shape. Viewed from the perspective of the wound electrode body 1, the lower surface 2b is located on the other side along the axial direction Z of the wound electrode body 1. The side surface 2c has a cylindrical shape. The side surface 2c connects the upper surface 2a and the lower surface 2b. The housing 2 is formed of copper or aluminum, etc. It should be noted that the housing 2 also contains an electrolyte (not shown).

[0029] The height dimension (dimension along the Z-axis) of the housing 2 is, for example, 50 mm or more, 60 mm or more, 70 mm or more, or 80 mm or more. The larger the height dimension (dimension along the Z-axis) of the housing 2, the larger the battery capacity of the secondary battery 100. Conversely, the height dimension (dimension along the Z-axis) of the housing 2 is, for example, 150 mm or less, 100 mm or less, or 80 mm or less. The smaller the height dimension (height dimension) along the Z-axis of the housing 2, the lower the height of the module housing the secondary battery 100 can be.

[0030] The diameter (radial dimension R) of the housing 2 is, for example, 15mm or more, 20mm or more, 25mm or more, 30mm or more, 40mm or more, 45mm or more, or 46mm or more. The larger the diameter (maximum radial dimension R) of the housing 2, the larger the battery capacity of the secondary battery 100. The diameter (radial dimension R) of the housing 2 is, for example, less than 100mm, less than 75mm, less than 50mm, or less than 46mm. The smaller the diameter (radial dimension R) of the housing 2, the more compactly the secondary battery 100 can be arranged within the module.

[0031] The positive terminal 3 is located on one side Z1 in the axial direction Z relative to the wound electrode body 1. The positive terminal 3 includes a disc portion 3a and a riveting portion 3b. The riveting portion 3b is connected to the disc portion 3a. The riveting portion 3b is configured to extend from the center of the disc portion 3a toward the other side Z2 in the axial direction Z. It should be noted that the positive terminal 3 is made of aluminum. The disc portion 3a is disposed on the upper surface portion 2a of the housing 2. A through hole 2d is provided on the upper surface portion 2a of the housing 2. The riveting portion 3b extends from the disc portion 3a disposed on the outside of the housing 2 through the through hole 2d into the interior of the housing 2.

[0032] The positive current collector 4 is housed within the housing 2. The positive current collector 4 is positioned on one side Z1 in the Z-axis direction relative to the wound electrode body 1. The positive current collector 4 is welded to the composite material unformed portion 12a of the positive electrode plate 10. Thus, the positive current collector 4 is positively charged. The positive current collector 4 is welded to the end of the riveting portion 3b on the other side Z2 in the Z-axis direction. Thus, the positive terminal 3 is positively charged.

[0033] An external gasket 5 is disposed between the disk portion 3a of the positive terminal 3 and the upper surface portion 2a of the housing 2. Thus, the positive terminal 3 and the housing 2 are insulated from each other.

[0034] An internal gasket 6 is disposed inside the housing 2 between the housing 2 and the positive current collector 4. Thus, the housing 2 and the positive current collector 4 are mutually insulated. It should be noted that the riveting part 3b contacts the positive current collector 4 by passing through the internal gasket 6.

[0035] The negative electrode current collector 7 is housed within the housing 2. The negative electrode current collector 7 is located on the opposite side Z2 in the axial direction Z relative to the wound electrode body 1. The negative electrode current collector 7 is welded to the unformed portion 22a of the composite material of the negative electrode 20. Thus, the negative electrode current collector 7 carries a negative charge. The negative electrode current collector 7 is in contact with the housing 2. Specifically, the negative electrode current collector 7 is in contact with the lower surface portion 2b and the side surface portion 2c. Thus, the housing 2 carries a negative charge. Furthermore, the upper surface portion 2a carries a negative charge.

[0036] Figure 2 This is a simplified top view of the positive electrode of the wound electrode body according to the embodiment after it has been unfolded. Figure 3 This is a simplified cross-sectional view of the positive electrode of the wound electrode body according to the embodiment. It should be noted that... Figure 3 It is along Figure 2 The sectional view shown is taken along line III-III. (Refer to...) Figure 2 as well as Figure 3 This describes the positive electrode 10 involved in the implementation method.

[0037] In its unfolded state, the positive electrode 10 has a strip-like shape extending along its length direction D1 (long side direction). The length direction D1 is orthogonal to the thickness direction T of the positive electrode 10. Furthermore, the length direction D1 is the direction in which the winding direction X is unfolded into a straight line. The positive electrode 10 has a first end 10a and a second end 10b along the length direction D1. The first end 10a is the end located on the inner circumferential side of the wound electrode body 1 (the inner circumferential end). The second end 10b is the end located on the outer circumferential side of the wound electrode body 1 (the outer circumferential end).

[0038] The positive electrode 10 includes a positive current collector 11, a first positive electrode film 13, and a second positive electrode film 14. The positive current collector 11 is made of a metal foil such as aluminum. The positive current collector 11 has a first main surface 11a and a second main surface 11b arranged along the thickness direction T. The first main surface 11a is located at one end of the positive current collector 11 in the thickness direction T. The second main surface 11b is located at the other end of the positive current collector 11 in the thickness direction T. In the state of winding the electrode body 1, that is, in the wound state after the positive electrode 10 is wound, the first main surface 11a faces the inner peripheral side, and the second main surface 11b faces the outer peripheral side.

[0039] The positive electrode 10 has a composite material unformed portion 12a and a composite material formed portion 12b. The composite material unformed portion 12a is the portion of the positive electrode current collector 11 exposed from both the first positive electrode film 13 and the second positive electrode film 14. The composite material formed portion 12b is the portion of the positive electrode 10 in which both the first positive electrode film 13 and the second positive electrode film 14 are formed. The composite material unformed portion 12a extends from the composite material formed portion 12b toward the side in the width direction D2. In the wound state, the composite material unformed portion 12a is exposed from the composite material formed portion 12b toward the side Z1 in the axial direction Z of the wound electrode body 1.

[0040] The first positive electrode film 13 is disposed on the first main surface 11a. The first positive electrode film 13 is disposed on the first main surface 11a with the first main surface 11a exposed on one side of the width direction D2, which is orthogonal to the aforementioned length direction D1. It should be noted that the width direction D2 is the direction parallel to the axial direction Z in the winding electrode body 1.

[0041] The second positive electrode film 14 is disposed on the second main surface 11b. The second positive electrode film 14 is disposed on the second main surface 11b on one side of the width direction D2, which is orthogonal to the aforementioned length direction D1, with the second main surface 11b exposed. The second positive electrode film 14 is arranged to overlap with the first positive electrode film 13 in the thickness direction T of the positive electrode 10. The dimensions of the second positive electrode film 14 are substantially the same as the dimensions of the first positive electrode film 13.

[0042] The first positive electrode film 13 and the second positive electrode film 14 each include a plurality of high-density regions R1 and a plurality of low-density regions R2. The plurality of high-density regions R1 and the plurality of low-density regions R2 are alternately arranged in the first positive electrode film 13 and the second positive electrode film 14 along the aforementioned length direction D1. The plurality of high-density regions R1 and the plurality of low-density regions R2 extend along the aforementioned width direction D2, which is orthogonal to the aforementioned thickness direction T and the aforementioned length direction D1.

[0043] The high-density region R1 of the first positive electrode film 13 and the low-density region R2 of the second positive electrode film 14 are arranged along the thickness direction T, with the positive current collector 11 sandwiched in between.

[0044] In the first positive electrode film 13, the lengths of the high-density region R1 and the low-density region R2 in the length direction are each less than the thickness of the first positive electrode film 13 in the thickness direction T. Similarly, in the second positive electrode film 14, the lengths of the high-density region R1 and the low-density region R2 in the length direction are each less than the thickness of the second positive electrode film 14 in the thickness direction T.

[0045] In the first positive electrode film 13 and the second positive electrode film 14, the density of the multiple high-density regions R1 is more than 1.1 times and less than 1.5 times the density of the multiple low-density regions R2.

[0046] The first positive electrode film 13 and the second positive electrode film 14 are respectively composed of electrode films 131 and 132 (described later) containing positive electrode active materials. Figure 4 )constitute.

[0047] Since the structure of the negative electrode 20 is basically the same as that of the positive electrode 10, its unfolded view and cross-sectional view are not shown. The negative electrode 20 also has a strip-like shape extending along the length direction D1 in its unfolded state. The negative electrode 20 has a first end and a second end in the length direction D1. The first end is the end located on the inner circumferential side of the wound electrode body 1 (wound inner circumferential end). The second end is the end located on the outer circumferential side of the wound electrode body 1 (wound outer circumferential end).

[0048] For example Figure 1 As shown, the negative electrode 20 includes a negative electrode current collector 21, a second negative electrode film 23, and a second negative electrode composite material layer 24. The negative electrode current collector 21 is made of a metal foil such as copper. The negative electrode current collector 21 has a first main surface 21a and a second main surface 21b arranged along the thickness direction. In the state of winding the electrode body 1, that is, in the wound state after the negative electrode 20 is wound, the first main surface 21a faces the inner peripheral side, and the second main surface 21b faces the outer peripheral side.

[0049] The negative electrode 20 has a composite material unformed portion 22a and a composite material formed portion. The composite material unformed portion 22a is the portion of the negative electrode current collector 21 exposed from both the second negative electrode film 23 and the second negative electrode composite material layer 24. The composite material formed portion is the portion of the negative electrode 20 where both the second negative electrode film 23 and the second negative electrode composite material layer 24 are formed. The composite material unformed portion 22a extends from the composite material formed portion to the other side in the width direction. In the wound state, the composite material unformed portion 22a is exposed from the composite material formed portion to the other side Z2 in the axial direction Z of the wound electrode body 1.

[0050] The second negative electrode film 23 is disposed on the first main surface 21a. The second negative electrode film 23 is disposed on the first main surface 21a on the other side of the width direction orthogonal to the aforementioned length direction, with the first main surface 21a exposed.

[0051] The second negative electrode composite material layer 24 is disposed on the second main surface 21b. The second negative electrode composite material layer 24 is disposed on the second main surface 21b on the other side in the width direction orthogonal to the aforementioned length direction, with the second main surface 21b exposed. The second negative electrode composite material layer 24 is arranged to overlap with the second negative electrode film 23 in the thickness direction of the negative electrode 20. The dimensions of the second negative electrode composite material layer 24 are substantially the same as those of the second negative electrode film 23.

[0052] The second negative electrode film 23 and the second negative electrode composite material layer 24 each include a plurality of high-density regions and a plurality of low-density regions. The plurality of high-density regions and the plurality of low-density regions are alternately arranged in the second negative electrode film 23 and the second negative electrode composite material layer 24 along the aforementioned length direction. The plurality of high-density regions R1 and the plurality of low-density regions R2 extend along the aforementioned width direction.

[0053] The high-density region of the second negative electrode film 23 and the low-density region R2 of the second negative electrode composite material layer 24 are arranged along the thickness direction, with the negative electrode current collector 21 sandwiched in between.

[0054] In the second negative electrode film 23, the lengths of the high-density regions and low-density regions in the longitudinal direction are each less than the thickness of the second negative electrode film 23 in the thickness direction. Similarly, in the second negative electrode composite material layer 24, the lengths of the high-density regions and low-density regions in the longitudinal direction are each less than the thickness of the second negative electrode composite material layer 24 in the thickness direction.

[0055] In the second negative electrode film 23 and the second negative electrode composite material layer 24, the density of multiple high-density regions is more than 1.1 times and less than 1.5 times the density of multiple low-density regions.

[0056] The second negative electrode film 23 and the second negative electrode composite material layer 24 can also be composed of a negative electrode film containing a negative electrode active material.

[0057] (Electrode plate manufacturing process)

[0058] Figure 4 This is a schematic diagram illustrating the manufacturing process of the positive electrode involved in Embodiment 1. (As shown...) Figure 4 As shown, the positive electrode 10 can be manufactured by attaching the electrode films 131 and 132 of the aforementioned positive electrode to the positive electrode current collector 11.

[0059] The positive electrode film 131 has a first surface 131a and a second surface 131b arranged along the thickness direction T. The first surface 131a has a wave-like shape with alternating peaks and valleys in the length direction. The second surface 131b is formed to be flat.

[0060] The positive electrode film 132 has a first surface 132a and a second surface 132b arranged along the thickness direction T. The first surface 132a has a wave-like shape with alternating peaks and valleys in the length direction. The second surface 132b is formed to be flat.

[0061] A positive electrode film 131 is disposed on the first main surface 11a with the first main surface 11a having a wave-shaped first surface 131a facing the first main surface 11a of the positive current collector 11, and a positive electrode film 132 is disposed on the second main surface 11b with the first main surface 132a having a wave-shaped first surface facing the second main surface 11b of the positive current collector 11. In this state, the positive electrode films 131 and 132 and the positive current collector 11 are transported and pressed by the pressing device 90.

[0062] The pressing device 90 includes a pair of rollers 91 and 92. When a positive current collector 11, on the first main surface 11a side with a positive electrode film 131 and on the second main surface 11b side with a positive electrode film 132, passes between the pair of rollers 91 and 92, it is pressed using the pair of rollers 91 and 92. At this time, on the first main surface 11a side, the positive electrode film 131 is attached to the first main surface 11a while the first surface 131a is formed flat, and on the second main surface 11b side, the positive electrode film 132 is attached to the second main surface 11b while the first surface 132a is formed flat.

[0063] The positive electrode film 131 has a peak P1 and a valley P2 along the length direction D1, and a midpoint P3 between these peaks P1 and valleys P2. On the first main surface 11a side, the portion of the positive electrode film 131 between the midpoint P3, where the peaks P1 are located in the middle, is pressed to form a high-density region R1. Similarly, the portion of the positive electrode film 131 between the midpoint P3, where the valleys P2 are located in the middle, is pressed to form a low-density region R2.

[0064] By pressing the electrode film 131 of the positive electrode, a first positive electrode film 13 is formed by alternating high-density regions R1 and low-density regions R2 along the length direction D1.

[0065] Similarly, on the second main surface 11b side, the portion of the positive electrode film 132 between the intermediate positions P3, where the peak P1 is located in the middle, is pressed to form a high-density region R1. Additionally, the portion of the positive electrode film 132 between the intermediate positions P3, where the valley P2 is located in the middle, is pressed to form a low-density region R2. By pressing the positive electrode film 132, a second positive electrode film 14 is formed, in which the high-density region R1 and the low-density region R2 alternate along the length direction D1.

[0066] The positive electrode film 131 and the positive electrode film 132 are arranged such that the peaks P1 are staggered in the length direction D1. With the peaks P1 of the positive electrode film 131 and the valleys P2 of the positive electrode film 132 facing each other in the thickness direction T, and the valleys P2 of the positive electrode film 131 and the peaks P1 of the positive electrode film 132 facing each other in the thickness direction T, the positive electrode film 131 and the positive electrode film 132 are disposed on the positive current collector 11.

[0067] Therefore, when the positive electrode current collector 11 is disposed between the positive electrode films 131 and 132, and the positive electrode current collector 11 is pressed, the high-density region R1 of the first positive electrode film 13 and the low-density region R2 of the second positive electrode film 14 are arranged along the thickness direction T, sandwiching the positive electrode current collector 11 in the middle. Furthermore, the low-density region R2 of the first positive electrode film 13 and the high-density region R1 of the second positive electrode film 14 are arranged along the thickness direction T, sandwiching the positive electrode current collector 11 in the middle.

[0068] Figure 5 This is a schematic diagram illustrating the process of forming a sheet of positive electrode composite material used in the positive electrode according to Embodiment 1. Figure 5As shown, when preparing the aforementioned positive electrode films 131 and 132 with a wave-shaped positive electrode, for example, the positive electrode films 131 and 132, whose front and back sides are flat plates, are passed between a first roller 91A with an uneven surface and a second roller 92A with a smooth surface. This produces a positive electrode film 131 and 132 with a wave-shaped first surface 131a and 132a on the first roller 91A side and a flat second surface 131b and 132b on the second roller 92A side. The unevenness of the surface of the first roller 91A can also be periodically arranged.

[0069] The above examples illustrate cases where the surface of the first roller 91A has an uneven shape, but are not limited to this. Both the first roller 91A and the second roller 92A may also have smooth surfaces. In this case, ultrasonic vibration may be applied to one of the first roller 91A and the second roller 92A in a direction facing each other using an ultrasonic vibration device, while the electrode films 131 and 132, which are flat plates on both sides, pass between the first roller 91A and the second roller 92A.

[0070] It should be noted that since the negative electrode 20 is formed in essentially the same way as the positive electrode 10, detailed descriptions of the manufacturing process are omitted.

[0071] (Electrode film)

[0072] The electrode films 131 and 132 of the positive electrode can be made of self-supporting films. Similarly, the electrode film of the negative electrode can also be made of self-supporting films.

[0073] Self-supporting membranes are characterized by their ability to maintain their shape even without a support structure. For example, self-supporting membranes possess sufficient strength to withstand processes such as roller conveying, even without a support structure like a current collector (described later). The tensile strength range of a self-supporting membrane can be, for example, a range with only an upper or lower limit obtained by selecting any value from the group consisting of 0.1 MPa, 0.2 MPa, 0.3 MPa, 0.5 MPa, 0.6 MPa, 0.7 MPa, 0.8 MPa, 0.9 MPa, and 1.0 MPa, or a range with both an upper and lower limit obtained by selecting any two values. The range may or may not include endpoints. The tensile strength range of a self-supporting membrane can be, for example, 0.1 MPa to 1.0 MPa. The tensile strength range of a self-supporting membrane can also be, for example, 0.5 MPa or higher. Having a tensile strength of 0.5 MPa or higher in a self-supporting membrane is expected to facilitate processes such as roll material handling.

[0074] The tensile strength of each of the above electrode films can be determined, for example, by the following method: A specimen is cut from the electrode film. The planar dimensions of the specimen are, for example, approximately 30 mm × 30 mm. A tensile test is performed on the specimen using a texture analyzer (e.g., manufactured by Eihong Seiki Co., Ltd.) at a speed of 2 mm / s. The maximum load during tension is measured. The tensile strength is calculated using the following formula. The tensile strength value is the arithmetic mean of three specimens.

[0075] Rm=(F×0.0098) / (t・W)

[0076] Rm: Tensile strength [MPa]

[0077] F: Maximum load [g]

[0078] t: Sample thickness [mm]

[0079] W: Sample width [mm]

[0080] The electrode film can have any planar shape. For example, the planar shape of the electrode film can be strip-shaped, rectangular, circular, etc. The dimensions of the electrode film (thickness, length, width, etc.) can be arbitrarily changed according to the electrode design. The thickness range of the electrode film can be, for example, a range with only an upper or lower limit obtained by selecting any value from the group consisting of 5μm, 10μm, 25μm, 50μm, 75μm, 100μm, 150μm, 200μm, 250μm, 300μm, 400μm, 500μm, 600μm, 700μm, 800μm, 900μm, and 1000μm, or a range with both an upper and lower limit obtained by selecting any two values. The range may or may not include endpoints. The thickness range of the electrode film can be, for example, 5μm to 1000μm. The density range of the electrode film can be, for example, from 0.5g / cm³. 3 1.0g / cm 3 1.5g / cm 3 2.0g / cm 3 2.5g / cm 3 3.0g / cm 3 3.5g / cm 3 4.0g / cm 3 4.5g / cm 3 5.0g / cm 3 The range formed by selecting any one value can be a range with only an upper or lower limit, or a range with both an upper and lower limit can be obtained by selecting any two values. The range may or may not include endpoints. For example, the density range of the electrode film could be 0.5 g / cm³. 3 ~5.0g / cm 3 .

[0081] (composition)

[0082] The electrode membrane contains an electrode active material and a first binder. The first binder contains a fibrous binder. That is, the electrode membrane contains an electrode active material and a fibrous binder. The electrode membrane may further contain, for example, a second binder, a conductive material, a solid electrolyte, etc. For example, the electrode membrane contains, by mass fraction, 0.1% to 10% of the first binder, 0% to 10% of the second binder, 0% to 10% of the conductive material, 0% to 30% of the solid electrolyte, and the balance being the electrode active material.

[0083] (Electrode active material)

[0084] The electrode active material is a powder. The particle size distribution of the electrode active material can be, for example, a unimodal distribution. The particle size distribution can be a volume distribution or a number distribution. Volume distribution can be determined by laser diffraction. Number distribution can be determined by microscopy. "D50" represents the particle size at which the cumulative frequency reaches 50% in the cumulative distribution. The range of D50 for the electrode active material can be, for example, a range with only an upper or lower limit obtained by selecting any one value from the group consisting of 0.1 μm, 0.5 μm, 1 μm, 3 μm, 5 μm, 10 μm, 15 μm, 20 μm, 25 μm, and 30 μm, or a range with both an upper and lower limit obtained by selecting any two values. The range may or may not include endpoints. For example, the D50 range of the electrode active material can be 0.1 μm to 30 μm.

[0085] The particle size distribution of electrode active materials can be bimodal or multimodal. For example, in the case of a bimodal particle size distribution (frequency distribution), particles belonging to the peak with the larger particle size are called "large particles," and particles belonging to the peak with the smaller particle size are called "small particles." The mode particle size of each peak can be considered as the particle size of each particle. The "mode particle size" represents the particle size at the peak of the frequency distribution. The particle size of large particles is "D". L "Relative to the particle size of small particles" D S The ratio of "D" to " L / D S The range can be, for example, a range with only an upper or lower limit obtained by selecting any one value from the group consisting of 1.2, 1.5, 2.0, 3.0, 4.0, and 5.0, or a range with both an upper and lower limit obtained by selecting any two values. The range may or may not include endpoints. For example, a range can satisfy "1.2 ≦ D". L / D S Relationships such as ≦5.0”.

[0086] Electrode active materials can be primary or secondary particles. They can have any particle shape, such as spherical, ellipsoidal, scaly, plate-like, columnar, blocky, or irregular shapes.

[0087] The electrode active material can be a granulated body. Granulated bodies can be formed by any method. For example, they can be formed by spray drying, stirring granulation, etc. By granulation, the sphericity of the granulated body (secondary particles) can be adjusted. "Sphericity" refers to the roundness in an SEM image (two-dimensional image). Sphericity (roundness) is calculated using the following formula. Sphericity can be taken as the arithmetic mean of 10 particles.

[0088] ψ=4πS / L 2

[0089] ψ: Sphericity (roundness)

[0090] π: Pi

[0091] S: Cross-sectional area of ​​the particle (the area enclosed by the particle's outline)

[0092] L: The perimeter of the particle (the length of the particle's outline).

[0093] The range of sphericity "ψ" of the electrode active material can be, for example, a range with only an upper or lower limit obtained by selecting any value from the group consisting of 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, and 1.0, or a range with both an upper and lower limit obtained by selecting any two values. The range may or may not include endpoints. For example, it can satisfy relationships such as "0.1 ≤ ψ ≤ 1.0".

[0094] In the negative electrode film, a negative electrode active material is used as the electrode active material. The negative electrode active material may contain at least one material selected from the group consisting of natural graphite (flake graphite, spherical graphite), artificial graphite, soft carbon, hard carbon, silicon, silicon oxide, silicon-based alloys, silicon-carbon composites "Si-C", lithium silicate, tin, tin oxide, tin-based alloys, and lithium titanate. Spherical graphite may be coated with amorphous carbon, for example. For example, natural graphite, artificial graphite, soft carbon, and hard carbon can be collectively referred to as "carbon-based active materials". Silicon may contain any crystalline phase. Silicon may contain at least one material selected from the group consisting of cage-like type I phase, cage-like type II phase, and diamond phase. Si-C represents composite particles containing at least one of silicon and silicon oxide with carbon. For example, silicon may be loaded into the internal voids of carbon particles. Carbon particles may be graphite particles or amorphous carbon particles. For example, silicon, silicon oxide, silicon-based alloys, and silicon-carbon composites can be collectively referred to as "silicon-based active materials".

[0095] The negative electrode active material can be, for example, a mixture of natural graphite and artificial graphite. The range of the mass ratio "natural graphite:artificial graphite" can be, for example, a range with any two pairs of values ​​selected from the groups consisting of "1:9", "2:8", "3:7", "4:6", "5:5", "6:4", "7:3", "8:2", and "9:1" as endpoints. For example, a mass ratio such as "natural graphite:artificial graphite = 1:9 to 9:1" can be satisfied.

[0096] The negative electrode active material can be, for example, a mixture of carbon-based and silicon-based active materials. The range of the mass ratio "carbon-based active material: silicon-based active material" can be, for example, a range with any two groups selected as endpoints from the groups consisting of "1:99", "5:95", "10:90", "20:80", "30:70", "40:60", "50:50", "60:40", "70:30", "80:20", "90:10", "95:5", and "99:1". For example, a mass ratio of "carbon-based active material: silicon-based active material = 1:99 to 99:1" can be satisfied.

[0097] In the positive electrode film, a positive electrode active material is used as the electrode active material. The positive electrode active material may contain at least one compound selected from the group consisting of layered compounds, rock salt compounds, spinel compounds, and olivine compounds. For example, the positive electrode active material may be a mixture of layered compounds and olivine compounds. The range of the mass ratio "layered compound: olivine compound" may, for example, be a range with any two groups selected as endpoints from the group consisting of "1:9", "2:8", "3:7", "4:6", "5:5", "6:4", "7:3", "8:2", and "9:1". For example, a mass ratio relationship such as "layered compound: olivine compound = 1:9 to 9:1" may be satisfied.

[0098] The positive electrode active material may contain at least one material selected from the group consisting of Li(NiCoMn)O2 (layered compound), Li(NiCoAl)O2 (layered compound), LiMnO2 (rock salt compound), Li(NiMn)2O4 (spinel compound), and Li(MnFe)PO4 (olivine compound). It should be noted that the use of terms like (NiCoMn) indicates that the total composition ratio within parentheses is 1. As long as the total is 1, the composition ratio of each component within parentheses can be arbitrary. For example, it is also permissible for some components to have a composition ratio of 0.

[0099] Layered compounds, for example, can have the general formula "Li x Ni a Co b M cO y The formula represents the composition. The range of "x" in the formula can be, for example, a range with only an upper or lower limit obtained by selecting any one value from the group consisting of 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, or a range with both an upper and lower limit obtained by selecting any two values. The range may or may not include endpoints. For example, it can satisfy relationships such as "0.1≦x≦1.5". The formula satisfies the relationship "a+b+c=1". As long as this relationship is satisfied, the ranges of "a", "b", and "c" can be independently obtained by selecting any one value from the group consisting of 0, 0.05, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, each with only an upper or lower limit. This can be a range with upper and lower limits obtained by selecting any two values. The range may or may not include endpoints. For example, it can satisfy relationships such as "0≦a≦1", "0≦b≦1", "0≦c≦1", etc. Similarly, it can satisfy relationships such as "0.5≦a≦0.9", "0.05≦b≦0.5", "0.05≦c≦0.5", etc. In the formula, "M" can be, for example, a range selected from the group consisting of Mn and A1. One less. The range of "y" in the formula can be, for example, a range with only an upper or lower limit obtained by selecting any one value from the group consisting of 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, and 2.4, or a range with both an upper and lower limit obtained by selecting any two values. The range may or may not include endpoints. For example, it can satisfy relationships such as "1.6 ≦ y ≦ 2.4".

[0100] Layered compounds, for example, can be derived from Li x NiO y Li x CoO y Li x MnO y Li x Ni 1 / 3 Co 1 / 3 Mn 1 / 3 O y Li x Ni 0.4 Co 0.3 Mn 0.3 O y Li x Ni 0.5 Co 0.2 Mn 0.3 O y Lix Ni 0.5 Co 0.3 Mn 0.2 O y Li x Ni 0.5 Co 0.4 Mn 0.1 O y Li x Ni 0.5 Co 0.1 Mn 0.4 O y Li x Ni 0.6 Co 0.3 Mn 0.1 O y Li x Ni 0.6 Co 0.2 Mn 0.2 O y Li x Ni 0.6 Co 0.1 Mn 0.3 O y Li x Ni 0.7 Co 0.2 Mn 0.1 O y Li x Ni 0.7 Co 0.1 Mn 0.2 O y Li x Ni 0.8 Co 0.1 Mn 0.1 O y Li x Ni 0.8 Co 0.15 Al 0.05 O y and Li x Ni 0.9 Co 0.05 Mn 0.05 O y The selected group must be at least one of the following. For example, the formula can satisfy relationships such as "0.1≦x≦1.5" and "1.6≦y≦2.4".

[0101] Peridotite-type compounds may, for example, have a composition represented by the general formula "LiMPO4". In the formula, "M" may be at least one selected from the group consisting of Fe, Ni, Co, and Mn.

[0102] Peridotite-type compounds, for example, can have the general formula "Li x Mn 1-a Fe a PO y The formula represents the composition. The range of "x" can be, for example, a range with only an upper or lower limit obtained by selecting any one value from the group consisting of 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, and 1.5, or a range with both an upper and lower limit obtained by selecting any two values. The range may or may not have endpoints. For example, it can satisfy relationships such as "0.1 ≦ x ≦ 1.5". The range of "a" can be, for example, a range obtained by selecting any one value from the group consisting of 0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, and 1.0. The range of values ​​can be obtained by selecting any two values, which may or may not contain endpoints. For example, it can satisfy relationships such as "0 ≦ a ≦ 1.0" and "0.1 ≦ a ≦ 0.5". Similarly, the range of "y" can be obtained by selecting any value from the group consisting of 3.6, 3.7, 3.8, 3.9, 4.0, 4.1, 4.2, 4.3, and 4.4, which may or may not contain endpoints. For example, it can satisfy relationships such as "3.6 ≦ y ≦ 4.4".

[0103] Peridotite-type compounds may, for example, contain compounds derived from Li x MnPO y Li x Mn 0.9 Fe 0.1 PO y Li x Mn 0.8 Fe 0.2 PO y Li x Mn 0.7 Fe 0.3 PO y Li x Mn 0.6 Fe 0.4 PO y Li x Mn 0.5 Fe 0.5 PO y Li x Mn 0.4 Fe 0.6PO y Li x Mn 0.3 Fe 0.7 PO y Li x Mn 0.2 Fe 0.8 PO y Li x Mn 0.1 Fe 0.9 PO y and Li x FePO y The selected group must be at least one of the following. For example, the expression can satisfy relationships such as "0.1≦x≦1.5" and "3.6≦y≦4.4".

[0104] Any dopant can be introduced into the positive electrode active material. The dopant can be interstitial or substitutional. For example, the dopant can include at least one element selected from the group consisting of B, C, N, halogens, Si, Na, Mg, Al, Mn, Co, Cr, Sc, Ti, V, Cu, Zn, Ga, Ge, Se, Sr, Y, Zr, Nb, Mo, In, Pb, Bi, Sb, Sn, W, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, and actinides. The molar fraction (doping amount) of the dopant can be, for example, a range with only an upper or lower limit obtained by selecting any value from the group consisting of 0.01%, 0.1%, 1%, 3%, and 5%, or a range with both an upper and lower limit obtained by selecting any two values. The range may or may not include endpoints. The doping amount can range from, for example, 0.01% to 5%.

[0105] (Conductive materials)

[0106] Conductive materials can form electron conduction pathways within the electrode film. Conductive materials may include, for example, at least one material selected from the group consisting of acetylene black, Ketjen black (registered trademark), thermal cracking carbon black, furnace black, carbon fibers, carbon nanotubes, graphene sheets, metal fibers, and metal powders. When the electrode active material is a positive electrode active material, the group of materials constituting the conductive material may further include, for example, natural graphite and artificial graphite.

[0107] The conductive material can be, for example, a powder. The conductive material can have a smaller D50 compared to the electrode active material. The range of the D50 of the conductive material can be, for example, a range with only an upper or lower limit obtained by selecting any value from the group consisting of 0.01 μm, 0.05 μm, 0.1 μm, 0.5 μm, 1 μm, 3 μm, and 5 μm, or a range with both an upper and lower limit obtained by selecting any two values. The range may or may not include endpoints. The D50 range of the conductive material can be, for example, 0.01 μm to 5 μm.

[0108] The range of the mass fraction of conductive material in the electrode film can be, for example, a range with only an upper or lower limit obtained by selecting any value from the group consisting of 0%, 0.1%, 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, and 10%, or a range with both an upper and lower limit obtained by selecting any two values. The range may or may not include endpoints. For example, the range of the mass fraction of conductive material can be 0% to 10%.

[0109] (Solid electrolyte)

[0110] Solid electrolytes can form ion conduction pathways within the electrode film. Solid electrolytes may include at least one selected from the group consisting of sulfide solid electrolytes, halide solid electrolytes, oxide solid electrolytes, hydride solid electrolytes, and nitride solid electrolytes. Sulfide solid electrolytes may include at least one selected from the group consisting of amorphous phases, crystalline phases, and glass-ceramic phases (crystalline glass). Crystalline phases may include, for example, argentite-germanium sulfide type, LGPS type, etc. Sulfide solid electrolytes may contain, for example, LiI-LiBr-Li3PS4, Li2S-SiS2, LiI-Li2S-SiS2, LiI-Li2S-P2S5, LiI-Li2O-Li2S-P2S5, LiI-Li2S-P2O5, LiI-Li3PO4-P2S5, Li2S-GeS2-P2S5, Li2S-P2S5, Li 10 GeP2S 12 Li4P2S6, Li7P3S 11At least one of the following groups must be selected: LiI, LiBr, and Li7PS6. For example, "LiI-LiBr-Li3PS4" indicates a sulfide solid electrolyte formed by mixing LiI, LiBr, and Li3PS4 in any molar ratio. For example, a sulfide solid electrolyte can be generated by a mechanochemical method. The mixing ratio can be determined by marking numbers before each raw material. For example, "10LiI-15LiBr-75Li3PS4" indicates a mixing ratio (molar ratio) of "LiI:LiBr:Li3PS4 = 10:15:75".

[0111] Sulfide solid electrolytes can, for example, have a composition represented by the general formula "yLiI-zLiBr-(100-yz)[xLi2S-(1-x)P2S5]". The range of "x" in the formula can be, for example, a range with only an upper or lower limit obtained by selecting any value from the group consisting of 0.1, 0.2, 0.25, 0.3, 0.4, 0.5, 0.6, 0.7, 0.75, 0.8, and 0.9, or a range with both an upper and lower limit obtained by selecting any two values. The range may or may not include endpoints. For example, it can satisfy relationships such as "0.1≦x≦0.9". The formula also satisfies the relationship "0<100-yz≦100". As long as this relationship is satisfied, the ranges of "y" and "z" can be independently obtained by selecting any one value from the group consisting of 0, 5, 10, 15, 20, 25, and 30, resulting in a range with only an upper or lower limit. Alternatively, they can be obtained by selecting any two values, resulting in a range with both an upper and lower limit. The range may or may not include endpoints. For example, relationships such as "0≦y≦30" and "0≦z≦30" can be satisfied.

[0112] Sulfide solid electrolytes, for example, can have the general formula "Li4-xM 1-x P x S4 represents the composition. The range of "x" in the formula can be, for example, a range with only an upper or lower limit obtained by selecting any one value from the group consisting of 0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, and 1, or a range with both an upper and lower limit obtained by selecting any two values. The range may or may not include endpoints. For example, it can satisfy the relationship "0 < x < 1". "M" in the formula can, for example, contain at least one value selected from the group consisting of Al, Zn, In, Ge, Si, Sn, Sb, Ga, and Bi.

[0113] Sulfide solid electrolytes, for example, can have the general formula "Li 10+x Ge 1+x P 2-xS 12 The formula represents the composition. The range of "x" in the formula can be, for example, a range with only an upper or lower limit obtained by selecting any value from the group consisting of 0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, and 0.7, or a range with both an upper and lower limit obtained by selecting any two values. The range may or may not include endpoints. For example, it can satisfy a relationship such as "0 < x ≤ 0.7". A sulfide solid electrolyte represented by this formula may, for example, contain an LGPS-type crystalline phase.

[0114] Halogenated solid electrolytes, for example, can have the general formula "Li 6-na M a The composition is represented by "X6". In the formula, "n" represents the oxidation number of "M". "M" may, for example, contain atoms with an oxidation number of +3. "M" may, for example, contain atoms with an oxidation number of +4. "M" may, for example, contain at least one element selected from the group consisting of Y, Al, Ti, Zr, Ca, and Mg. For example, it may satisfy the relationship "0 < a < 2". "X" may, for example, contain at least one element selected from the group consisting of F, Cl, Br, and I.

[0115] Solid electrolytes can be, for example, powders. Solid electrolytes can have a smaller D50 compared to electrode active materials. The range of D50 for solid electrolytes can be, for example, a range with only an upper or lower limit obtained by selecting any value from the group consisting of 0.01 μm, 0.05 μm, 0.1 μm, 0.5 μm, 1 μm, 3 μm, and 5 μm, or a range with both an upper and lower limit obtained by selecting any two values. The range may or may not include endpoints. The D50 range of solid electrolytes can be, for example, 0.01 μm to 5 μm.

[0116] The volume fraction of the solid electrolyte in the electrode membrane can be, for example, a range with only an upper or lower limit obtained by selecting any value from the group consisting of 0%, 1%, 5%, 10%, 20%, 30%, 40%, 50%, 60%, and 70%, or a range with both an upper and lower limit obtained by selecting any two values. The range may or may not include endpoints. For example, the volume fraction of the solid electrolyte can range from 0% to 70%.

[0117] (First adhesive)

[0118] The first binder includes a fibrous binder. The first binder may also be substantially composed of a fibrous binder. The fibrous binder can be fibrillated, for example, by applying shear force to the granular binder (aggregates). For example, by feeding a composite material containing a granular binder to be converted into a fibrous binder and an electrode active material into the roll gap, shear force can be applied to the granular binder. By forming the granular binder into a fibrous binder, an electrode film can be formed. The rolling process can be performed once or repeatedly. Before the rolling process, shear force can be applied to the composite material, for example, by using a jet mill or a mixing granulator. For example, heating to 30°C to 150°C on top of the shear force can promote fibrillation. The granular binder can be completely or partially fibrillated. That is, the first binder may also contain granular components.

[0119] "Fibrous" indicates an aspect ratio (the ratio of the major diameter to the minor diameter) of 10 or higher. Materials with an aspect ratio less than 10 are considered "granular." The aspect ratio (the ratio of fiber length to fiber diameter) of fibrous materials can, for example, be 100 or higher. The minor diameter, major diameter, fiber diameter, and fiber length are determined by microscopy. The aspect ratio is the arithmetic mean of 10 measured samples. The length of the short side of the smallest bounding rectangle "MBR" of the measured sample is considered the minor diameter, and the length of the long side is considered the major diameter. The fiber diameter represents the dimension in the direction orthogonal to the axis of the measured sample. The fiber length represents the total length along the axial direction.

[0120] The fibrous adhesive may, for example, comprise a polymer composition. The polymer composition may be a homopolymer, copolymer, polymer blend, or polymer alloy. The fibrous adhesive may, for example, comprise polytetrafluoroethylene (PTFE). The fibrous adhesive may also contain any additives in addition to PTFE. Additives may include, for example, at least one selected from the group consisting of polyolefins, cellulose, polyethers, and polysiloxanes. The additives and PTFE may form at least one selected from the group consisting of polymer blends, polymer alloys, and copolymers. The range of the mass fraction of PTFE in the fibrous adhesive, or the range of the mass fraction of the tetrafluoroethylene (TFE) derivative, may be, for example, a range with only an upper or lower limit obtained by selecting any one value from the group consisting of 0%, 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80%, 90%, 95%, 99%, and 100%, or a range with both an upper and lower limit obtained by selecting any two values. The range may or may not include endpoints. The mass fraction of PTFE in fibrous binders can range from, for example, 0% to 100%.

[0121] The number-average molecular weight "Mn" of the polymer constituting the fibrous binder can, for example, be in the range of 10 × 10⁻⁶. 4 50×10 4 100×10 4 150×10 4 200×10 4 300×10 4 400×10 4 500×10 4 1000×10 4 2000×10 4 3000×10 4 The range formed by selecting any one value can be a range with only an upper or lower limit, or a range with both an upper and lower limit can be obtained by selecting any two values. The range may or may not include endpoints. For example, the range for number-average molecular weight could be 10 × 10⁻⁶. 4 ~3000×10 4 Number-average molecular weight can be obtained, for example, from standard specific gravity. Test samples are prepared according to ASTM D-4895 98. Standard specific gravity is determined using the water displacement method according to ASTM D-792.

[0122] The range of fiber diameter (fiber diameter) of the fibrous adhesive can be, for example, a range with only an upper or lower limit obtained by selecting any value from the group consisting of 1nm, 5nm, 10nm, 15nm, 20nm, 50nm, 100nm, 200nm, 500nm, and 1000nm, or a range with both an upper and lower limit obtained by selecting any two values. The range may or may not include endpoints. For example, the fiber diameter range can be 1nm to 1000nm.

[0123] Fibrous binders can form a fibrous matrix. For example, the fibrous matrix can be used to hold the electrode active material (powder) in place, thus maintaining the shape of the electrode membrane. The fibrous matrix can be evaluated, for example, by fiber density. Fiber density can be determined, for example, by the following method: Prepare a cross-sectional SEM image of the electrode membrane. In the cross-sectional SEM image, mark a 20 μm straight line at any location. Calculate the fiber density (unit: strands / 20 μm) by counting the fibrous portions intersecting this line. Measure the fiber density at at least three locations within the cross-sectional SEM image. Use the arithmetic mean of the three or more locations as the fiber density. The range of fiber density can be, for example, a range with only an upper or lower limit obtained by selecting any one value from the group consisting of 1, 2, 5, 10, 20, 40, 60, 80, and 100, or a range with both an upper and lower limit obtained by selecting any two values. The range may or may not include endpoints. The range of fiber density can be, for example, 1 to 100.

[0124] The range of the mass fraction of the first binder in the electrode film can be, for example, a range with only an upper or lower limit obtained by selecting any value from the group consisting of 0.1%, 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, and 10%, or a range with both an upper and lower limit obtained by selecting any two values. The range may or may not include endpoints. The range of the mass fraction of the first binder in the electrode film can be, for example, 0.1% to 10%.

[0125] (Second adhesive)

[0126] The form of the second adhesive is arbitrary. For example, the second adhesive can be granular, film-like, fibrous, etc. For example, the second adhesive can have a greater adhesive force than the first adhesive. For example, the electrode film can be fixed to the current collector by the second adhesive. The second adhesive may contain at least one component selected from the group consisting of polyvinylidene fluoride (PVdF), polyvinylidene fluoride-hexafluoropropylene copolymer (PVdF-HFP), carboxymethyl cellulose (CMC), polyacrylic acid (PAA), polyvinyl alcohol (PVA), polyvinylpyrrolidone (PVP), polyethylene oxide (PEO), styrene-butadiene rubber (SBR), nitrile rubber (NBR), polyethylene (PE), polypropylene (PP), polyacrylonitrile (PAN), polyoxyethylene alkyl ether, polyimide (PI), polyamide-imide (PAI), and derivatives thereof.

[0127] The range of the mass fraction of the second binder in the electrode film can be, for example, a range with only an upper or lower limit obtained by selecting any value from the group consisting of 0%, 0.1%, 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, and 10%, or a range with both an upper and lower limit obtained by selecting any two values. The range may or may not include endpoints. The range of the mass fraction of the second binder in the electrode film can be, for example, 0% to 10%.

[0128] The range of the mass ratio "first adhesive: second adhesive" can be, for example, a range with any two pairs of pairs selected from the groups consisting of "1:9", "2:8", "3:7", "4:6", "5:5", "6:4", "7:3", "8:2", "9:1", and "10:0" as endpoints. For example, a mass ratio of "first adhesive: second adhesive = 1:9 to 10:0" can be satisfied.

[0129] (Added ingredients)

[0130] The electrode film can contain any additives. These additives may include, for example, inorganic fillers, organic fillers, surface modifiers, dispersants, lubricants, flame retardants, protective agents, fluxes, coupling agents, and adsorbents. Other additives may include, for example, polyoxyethylene allyl phenyl ether phosphate, zeolite, silane coupling agents, molybdenum sulfide, and tungsten oxide.

[0131] (Summary)

[0132] As described above, in the electrode according to Embodiment 1, in the current collector of at least one of the positive current collector 11 and the negative current collector 21, high-density regions and low-density regions are alternately arranged along the length direction on both the first and second main surfaces of the current collector, and the high-density regions and low-density regions are arranged facing each other in the thickness direction. Therefore, by alternately arranging high-density and low-density regions along the length direction on the first and second surfaces of at least one current collector, the low-density and high-density regions are arranged substantially uniformly. As a result, electrolyte diffusion can be promoted.

[0133] It should be noted that in both the positive electrode current collector 11 and the negative electrode current collector 21, high-density regions and low-density regions are alternately arranged along the length direction on the first main surface and the second main surface, and in the thickness direction, the high-density regions and low-density regions are arranged facing each other. Under such circumstances, the diffusion of electrolyte can be promoted more efficiently.

[0134] Furthermore, in the composite material layer having high-density and low-density regions, the lengths of the high-density and low-density regions in the length direction are smaller than the thickness of the composite material layer in the thickness direction, allowing the low-density regions to be precisely arranged within the plane. This, in turn, efficiently promotes electrolyte diffusion.

[0135] Furthermore, in this embodiment, by setting the density of the high-density region R1 in both the positive electrode 10 and the negative electrode 20 to be more than 1.1 times and less than 1.5 times the density of the low-density region R2, the wound electrode body 1 can be appropriately given flexibility.

[0136] It should be noted that, as described above, when one of the positive electrode 10 and the negative electrode 20 includes the aforementioned high-density region R1 and low-density region R2, by setting the density of the high-density region R1 to be more than 1.1 times and less than 1.5 times the density of the low-density region R2, it is also possible to impart flexibility to the wound electrode body 1 to a certain extent.

[0137] Furthermore, the same effect can be obtained in the wound electrode body 1 and the secondary battery 100 that use the electrodes according to Embodiment 1.

[0138] (Implementation Method 2)

[0139] Figure 6 This is a simplified cross-sectional view of the positive electrode according to Embodiment 2. (Refer to...) Figure 6 Explain the positive electrode 10A involved in Implementation Method 2.

[0140] like Figure 6 As shown, the positive electrode 10A in Embodiment 2 differs from the positive electrode 10 in Embodiment 1 in the shape of the positive current collector 11A, the shape of the first positive electrode film 13A, and the shape of the second positive electrode film 14A. Other components are essentially the same.

[0141] The positive current collector 11A has a wave-like shape that meanders in the thickness direction T relative to the length direction. Thus, the first main surface 11a of the positive current collector 11A includes alternating protrusions P11 and concave portions P12 in the length direction, and an intermediate portion P13 located between the protrusions P11 and the concave portions P12.

[0142] The convex portion P11 is the portion that protrudes toward the first positive electrode film 13A in the thickness direction T, and the concave portion P12 is the portion that is recessed toward the second positive electrode film 14A in the thickness direction T.

[0143] A first region and a second region are formed on the first main surface 11a. The first region is the portion between a pair of intermediate portions P13 that are adjacent to each other in the length direction with a convex portion P11 in the middle. The second region is the portion between a pair of intermediate portions P13 that are adjacent to each other in the length direction with a concave portion P12 in the middle.

[0144] The second main surface 11b of the positive current collector 11A includes a protrusion P21 and a concave portion P22 arranged alternately along the length direction, and an intermediate portion P23 located between the protrusion P21 and the concave portion P22.

[0145] The convex portion P21 is the portion that protrudes toward the first positive electrode film 13A in the thickness direction T, and the concave portion P22 is the portion that is recessed toward the second positive electrode film 14A in the thickness direction T.

[0146] A first region and a second region are formed on the second main surface 11b. The first region is the portion between a pair of intermediate portions P23 that are adjacent to each other in the length direction with a convex portion P21 in the middle. The second region is the portion between a pair of intermediate portions P23 that are adjacent to each other in the length direction with a concave portion P22 in the middle.

[0147] The first positive electrode film 13A has a first surface 13a that contacts the first main surface 11a, and a second surface 13b located on the opposite side of the first surface 13a in the thickness direction T. The first surface 13a has a wave-like shape that follows the first main surface 11a. The second surface 13b is formed to be flat.

[0148] In the length direction, the region along the first main surface 11a of the first positive electrode film 13A is formed as a high-density region R1, and the region along the second main surface 11a of the first positive electrode film 13A is formed as a low-density region R2.

[0149] The second positive electrode film 14A has a first surface 14a that contacts the second main surface 11b, and a second surface 14b located on the opposite side of the first surface 14a in the thickness direction T. The first surface 14a has a wave-like shape that follows the second main surface 11b. The second surface 14b is formed to be flat.

[0150] In the length direction, the region of the first region along the second main surface 11b in the second positive electrode film 14A is formed as a low-density region R2, and the region of the second region along the second main surface 11b in the second positive electrode film 14A is formed as a high-density region R1.

[0151] It should be noted that the negative electrode 20 can also be constructed in the same manner as the positive electrode 10. Specifically, the negative electrode current collector has a wave-like shape, just like the positive electrode current collector 11A. In this case, the second negative electrode film has a first surface that contacts the first main surface of the negative electrode current collector and forms a wave-like shape following the first main surface, and a second surface that is located on the opposite side of the first surface in the thickness direction and is formed as flat. Similarly, the second negative electrode composite material layer has a first surface that contacts the second main surface of the negative electrode current collector and forms a wave-like shape following the second main surface, and a second surface that is located on the opposite side of the first surface in the thickness direction and is formed as flat. In addition, the positional relationship between the high-density region R1 and the low-density region R2 in the second negative electrode film and the second negative electrode composite material layer is the same as that of the positive electrode 10 described above.

[0152] With the above configuration, the electrodes (positive electrode 10 or negative electrode 20) involved in Embodiment 2 can achieve essentially the same effects as in Embodiment 1. Furthermore, the same effects can also be achieved in the wound electrode body 1 and the secondary battery 100 using the electrodes involved in Embodiment 2.

[0153] (Manufacturing process)

[0154] The manufacturing process of the electrode according to Embodiment 2 is based on the manufacturing process of the electrode according to Embodiment 1. In Embodiment 2, a positive electrode film 131 is disposed on the first main surface 11a with the first main surface 11a having a wave-shaped first surface 131a facing the first main surface 11a of the positive current collector 11, and a positive electrode film 132 is disposed on the second main surface 11b with the first main surface 132a having a wave-shaped first surface facing the second main surface 11b of the positive current collector 11. In this state, the positive electrode films 131 and 132 and the positive current collector 11 are conveyed and pressed by the pressing device 90. At this time, the positive current collector 11 forms a wave-shaped shape due to the wave-shaped first main surface 131a and the second main surface 132a.

[0155] It should be noted that in Embodiments 1 and 2, the second main surfaces 131b and 132b were described as being formed flat when the electrode film 131, the current collector 11, and the electrode film 132 of the positive electrode were pressed using a pair of rollers 91 and 92. However, this is not a limitation. During the pressing process, the second main surfaces 131b and 132b may also be wavy. In this case, a planarization process may also be included to make the second main surfaces 131b and 132b flat. The same applies when manufacturing the negative electrode 20.

[0156] (Other variations)

[0157] The above description illustrates a case where both the positive electrode 10 and the negative electrode 20 contain multiple high-density regions and multiple low-density regions, but is not limited to this. It is sufficient that at least one of the positive electrode 10 and the negative electrode 20 contains multiple high-density regions and multiple low-density regions. In this case, if the electrode of one of the positive electrode 10 and the negative electrode 20 does not contain multiple high-density regions and multiple low-density regions, that electrode can be formed by coating a current collector with a paste.

[0158] (Postscript)

[0159] As described above, this implementation method includes the following disclosures.

[0160] [Component 1]

[0161] An electrode having:

[0162] A strip-shaped current collector has a first main surface on one side in the thickness direction and a second main surface on the other side in the thickness direction, and extends along a length direction orthogonal to the thickness direction;

[0163] A first electrode film, disposed on the first main surface; and

[0164] A second electrode film is disposed on the second main surface.

[0165] The first electrode film and the second electrode film each comprise multiple high-density regions and multiple low-density regions.

[0166] The plurality of high-density regions and the plurality of low-density regions are alternately arranged along the length direction.

[0167] The high-density region of the first electrode film and the low-density region of the second electrode film are arranged along the thickness direction, with the current collector sandwiched in between.

[0168] The low-density region of the first electrode film and the high-density region of the second electrode film are arranged along the thickness direction in a state in which the current collector is sandwiched in the middle.

[0169] [Component 2]

[0170] According to the electrode described in configuration 1, wherein...

[0171] The width of each of the plurality of high-density regions along the length direction and the width of each of the plurality of low-density regions are less than the thickness of the first electrode film and the second electrode film.

[0172] [Component 3]

[0173] According to the electrode configuration described in 1 or 2, wherein,

[0174] The density of the plurality of high-density regions is more than 1.1 times and less than 1.5 times the density of the plurality of low-density regions.

[0175] [Composition 4]

[0176] According to the electrode constituted in any one of 1 to 3, wherein,

[0177] At least one of the first electrode film and the second electrode film is composed of a self-supporting film.

[0178] The at least one electrode film comprises active material powder and fibrillated binder.

[0179] [Component 5]

[0180] According to the electrode constituted in any one of 1 to 4, wherein,

[0181] The current collector has a wave-like shape that meanders in the thickness direction relative to the length direction.

[0182] [Composition 6]

[0183] According to the electrode described in configuration 5, wherein...

[0184] The first main surface and the second main surface of the current collector include alternating protrusions and recesses along the length direction, and an intermediate portion located between the protrusions and the recesses.

[0185] On the first main surface and the second main surface, a first region and a second region are alternately formed along the length direction. The first region is the portion between a pair of adjacent intermediate portions along the length direction, with the protrusion located in the middle. The second region is the portion between a pair of adjacent intermediate portions along the length direction, with the concave portion located in the middle.

[0186] Along the length direction, the region of the first electrode film along the first region is formed as the high-density region, and the region of the first electrode film along the second region is formed as the low-density region.

[0187] In the length direction, the region along the first region in the second electrode film is formed as the low-density region, and the region along the second region in the second electrode film is formed as the high-density region.

[0188] [Component 7]

[0189] A type of wound electrode body,

[0190] Equipped with the electrodes as described in any one of 1 to 6,

[0191] The electrode is wound along the length direction.

[0192] [Composition 8]

[0193] A secondary battery, comprising:

[0194] The wound electrode body described in 7; and

[0195] A housing housing that contains the wound electrode.

[0196] The embodiments of the present invention have been described above, but it should be considered that the embodiments disclosed herein are merely illustrative in all respects and are not restrictive. The scope of the present invention is set forth in the claims and is intended to include all modifications of the same meaning and scope as the claims.

Claims

1. An electrode comprising: A strip-shaped current collector has a first main surface on one side in the thickness direction and a second main surface on the other side in the thickness direction, and extends along a length direction orthogonal to the thickness direction; A first electrode film is disposed on the first main surface; as well as A second electrode film is disposed on the second main surface. The first electrode film and the second electrode film each comprise multiple high-density regions and multiple low-density regions. The plurality of high-density regions and the plurality of low-density regions are alternately arranged along the length direction. The high-density region of the first electrode film and the low-density region of the second electrode film are arranged along the thickness direction, with the current collector sandwiched in between. The low-density region of the first electrode film and the high-density region of the second electrode film are arranged along the thickness direction in a state in which the current collector is sandwiched in the middle.

2. The electrode according to claim 1, wherein, The width of each of the plurality of high-density regions along the length direction and the width of each of the plurality of low-density regions are less than the thickness of the first electrode film and the second electrode film.

3. The electrode according to claim 1 or 2, wherein, The density of the plurality of high-density regions is more than 1.1 times and less than 1.5 times the density of the plurality of low-density regions.

4. The electrode according to any one of claims 1 to 3, wherein, At least one of the first electrode film and the second electrode film is composed of a self-supporting film. The at least one electrode film comprises active material powder and fibrillated binder.

5. The electrode according to any one of claims 1 to 4, wherein, The current collector has a wave-like shape that meanders in the thickness direction relative to the length direction.

6. The electrode according to claim 5, wherein, The first main surface and the second main surface of the current collector include alternating protrusions and recesses along the length direction, and an intermediate portion located between the protrusions and the recesses. On the first main surface and the second main surface, a first region and a second region are alternately formed along the length direction. The first region is the portion between a pair of adjacent intermediate portions along the length direction, with the protrusion located in the middle. The second region is the portion between a pair of adjacent intermediate portions along the length direction, with the concave portion located in the middle. Along the length direction, the region of the first electrode film along the first region is formed as the high-density region, and the region of the first electrode film along the second region is formed as the low-density region. In the length direction, the region along the first region in the second electrode film is formed as the low-density region, and the region along the second region in the second electrode film is formed as the high-density region.

7. A wound electrode body, Having the electrode as described in any one of claims 1 to 6, The electrode is wound along the length direction.

8. A secondary battery, comprising: The wound electrode body according to claim 7; and A housing housing that contains the wound electrode.

Citation Information

Patent Citations

  • Electrode for secondary batteries, and secondary battery