An ion conductor material, a preparation method and application thereof

By preparing ionic conductor materials with high ionic conductivity, wide electrochemical window, and flame retardancy, the safety and stability issues of lithium-ion batteries have been solved, achieving high energy density and good mechanical properties, making them suitable for various battery types.

CN123073153APending Publication Date: 2026-11-10CHINA PETROLEUM & CHEMICAL CORP +2
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202510582128.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-07
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing liquid electrolytes for lithium-ion batteries suffer from lithium dendrite growth, leakage, volatilization, and safety hazards, while polymer electrolytes are mechanically fragile, have unstable interfacial contact, and limited electrochemical stability. There is an urgent need to develop elastic materials with high ionic conductivity, wide electrochemical window, and high flame retardancy.

Method used

Materials with high ionic conductivity, wide electrochemical window and flame retardancy are prepared by using ionic conductor materials including monomers, modifiers, initiators, crosslinking agents and metal salts through click reaction or free radical polymerization. Small molecule modifiers and inorganic fillers are used to improve the compatibility and mechanical properties of the polymer substrate.

Benefits of technology

It achieves synergistic optimization of high ionic conductivity, wide electrochemical window and high flame retardancy, improving battery safety and energy density, and is suitable for lithium batteries, metal batteries, flexible batteries and hybrid energy storage devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123073153A_ABST
    Figure CN123073153A_ABST
Patent Text Reader

Abstract

The application discloses an ion conductor material and a preparation method and application thereof. The ion conductor material is prepared from raw materials including monomers, modifiers, initiators, crosslinking agents and metal salts. The monomers include at least one of polyethylene glycol diacrylate, polynorbomene, polyacrylate, polybutadiene, polyisoprene, polychloroprene, styrene butadiene rubber and vinyl silicone oil. The modifiers include at least one of mercaptopropionic acid, 3-mercapto propionitrile, 2-mercaptoethylamine, 3-mercapto-1-propane sulfonic acid sodium, 2-mercapto-3-pentanone, 8-mercapto-1-octanol, 4-mercaptobenzyl alcohol, vinyl sulfonic acid sodium, propylene glycol monoacrylate, 3-vinyl aniline, N-vinyl acetamide and butyl mercaptopropionate. The ion conductor material is suitable for being used as a separator, a solid-state electrolyte or a binder in a metal battery, a secondary ion battery, a flexible battery, a capacitor or a hybrid power storage device.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of battery technology, specifically relating to an ion conductor material, its preparation method, and its application. Background Technology

[0002] With population growth and industrial development, the excessive consumption of fossil fuels has triggered a severe energy and environmental crisis. Therefore, developing new energy sources is an inevitable choice for global development. Lithium-ion batteries (LIBs), with their advantages of high specific capacity, high operating voltage, and no memory effect, have received widespread attention and are the most promising rechargeable batteries and the fastest-growing chemical energy source. However, their energy density can no longer meet the growing demand for higher energy density energy storage devices. Lithium metal has a specific energy density of 3860 mA hg. -1 High specific capacity ratio graphite anode (372mA hg) -1 The energy density of lithium dendrites (LMBs) is more than 10 times higher than that of lithium ions, thus greatly improving the battery's energy density. However, LMBs based on liquid electrolytes suffer from severe lithium dendrite growth problems, which can lead to battery short circuits. Furthermore, due to their liquid nature, they are prone to leakage and volatilization, and under extreme conditions such as high temperatures or overcharging, they may pose a risk of instability or even combustion and explosion, presenting significant safety hazards.

[0003] Compared to liquid electrolytes, solid polymer electrolytes contain no liquid components. They are non-volatile, leak-proof, and have good thermal stability, offering excellent safety and making them a promising alternative. Solid electrolytes are generally divided into two categories: inorganic solid electrolytes and organic polymer solid electrolytes. Inorganic solid electrolytes maintain good chemical stability over a wide temperature range, possess good mechanical strength, and high room-temperature ionic conductivity. However, they are brittle, have poor processing performance, and poor interfacial contact, resulting in higher impedance. Compared to inorganic solid electrolytes, all-solid polymer electrolytes have lower ionic conductivity and a narrower operating temperature range. However, due to their strong adhesion, good compatibility with electrodes, and malleability, they are suitable for batteries of any shape, easier to design and process, and more suitable for mass production, showing better development prospects in safe lithium batteries.

[0004] Although polymer matrices can provide a closer contact with the electrode than inorganic solid electrolytes, they still undergo irreversible plastic deformation because their mechanical elasticity is insufficient to accommodate the repeated volume fluctuations of the lithium anode during long-term charge-discharge cycles. This deformation inevitably leads to unstable interfacial contacts. Simultaneously, due to the extremely high reducing power of lithium metal and the oxidative decomposition reaction occurring near the 4V cathode, most polymers exhibit limited stability and a relatively narrow electrochemical stability window. CN118572184A provides an in-situ polymer electrolyte component. This electrolyte component is obtained through an in-situ polymerization reaction, but it suffers from problems such as containing organic solvents, poor self-film-forming properties, the need for a separate separator as a support structure, complex preparation, and low safety. Furthermore, its electrochemical performance also has certain drawbacks in various aspects.

[0005] In summary, there is an urgent need in this field to develop an elastic material with high ionic conductivity, a wide electrochemical window, and high flame retardancy. Summary of the Invention

[0006] To address the problems existing in the prior art, this invention provides an ionic conductor material, its preparation method, and its applications. The ionic conductor material of this invention is suitable for use as a separator, solid electrolyte, or binder in metal batteries, secondary ion batteries, flexible batteries, capacitors, or hybrid energy storage devices. It achieves synergistic optimization of high ionic conductivity, a wide electrochemical window (≥5V), elastic mechanical properties, and flame retardancy, making it particularly suitable for lithium batteries.

[0007] The first aspect of the present invention provides an ion conductor material, wherein the ion conductor material is prepared using raw materials comprising: monomer, modifier, initiator, crosslinking agent, and metal salt.

[0008] According to the present invention, the monomer comprises at least one selected from polyethylene glycol diacrylate, polynorbornene, polyacrylate, polybutadiene, polyisoprene, polychloroprene, styrene-butadiene rubber, and vinyl silicone oil, preferably vinyl silicone oil. The weight average molecular weight of the monomer is 5,000 to 20,000, preferably 8,000 to 20,000.

[0009] According to the present invention, the modifier is a small molecule modifier. The modifier includes at least one selected from the following: mercaptopropionic acid, 3-mercaptopropionitrile, 2-mercaptoethylamine, sodium 3-mercapto-1-propanesulfonate, 2-mercapto-3-pentanone, 8-mercapto-1-octanol, 4-mercaptobenzyl alcohol, sodium vinyl sulfonate, propylene glycol monoacrylate, 3-vinylaniline, N-vinylacetamide, and butyl mercaptopropionate, preferably butyl mercaptopropionate.

[0010] According to the present invention, more preferably, the raw material of the ion conductor material may further include inorganic fillers. The inorganic fillers are selected from at least one of hydroxyapatite, lithium-doped hydroxyapatite, tin disulfide, barium titanate, and fumed silica, and are preferably lithium-doped hydroxyapatite.

[0011] According to the present invention, the initiator is selected from at least one of photoinitiators and thermal initiators. The photoinitiator includes at least one of 2-hydroxy-methylphenylpropane-1-one, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]-1-propanone, and 2,2-dimethoxy-2-phenylacetophenone. The thermal initiator includes at least one of azobisisobutyronitrile, azobisisoheptanenitrile, cumene hydroperoxide, tert-butyl hydroperoxide, benzoyl peroxide, and dicyclohexyl peroxide.

[0012] According to the present invention, the crosslinking agent is selected from at least one of pentaerythritol tetrakis(3-mercaptopropionic acid), 4,4′-dimercaptodiphenyl ether, and 2,2′-(1,2-ethylenedioxy)diethylthiol.

[0013] According to the present invention, the metal salt includes at least one selected from lithium sulfate, lithium nitrate, lithium chloride, lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, zinc sulfate, zinc nitrate, zinc chloride, zinc bis(fluoromethanesulfonyl)imide, sodium sulfate, sodium nitrate, sodium chloride, sodium hexafluorophosphate, potassium sulfate, potassium nitrate, potassium chloride, and potassium bis(fluoromethanesulfonyl)imide.

[0014] According to the present invention, the mass ratio of the modifier to the monomer is 1:1 to 50, preferably 1:1 to 10.

[0015] According to the present invention, the mass ratio of the initiator to the monomer is 1:1 to 600, preferably 1:300 to 600.

[0016] According to the present invention, the mass ratio of the crosslinking agent to the monomer is 1:1 to 1000, preferably 1:100 to 1000.

[0017] According to the present invention, the mass ratio of the inorganic filler to the monomer is 1:1 to 50, more preferably 1:1 to 20.

[0018] According to the present invention, the mass ratio of the metal salt to the monomer is 1:1 to 20, preferably 1:1 to 5.

[0019] A second aspect of the present invention provides a method for preparing the ionic conductor material, wherein the method is selected from one of click reaction, amine-olefin addition reaction and free radical polymerization reaction, preferably click reaction.

[0020] According to the present invention, the click response includes the following steps:

[0021] (11) Mix the monomer, modifier, initiator, crosslinking agent and metal salt to obtain a mixed solution;

[0022] (12) The ionic conductor material is prepared by clicking reaction of the mixed solution obtained in step (11) under ultraviolet light irradiation.

[0023] According to the present invention, the initiator in step (11) is a photoinitiator.

[0024] According to the present invention, the mixing conditions in step (11) include: a mixing temperature of 20–100°C and a mixing time of 10–30 h. The mixing is carried out under stirring.

[0025] According to the present invention, when the raw materials in step (11) include inorganic fillers, the mixed solution obtained in step (11) is poured onto the inorganic fillers and then subjected to a click reaction under ultraviolet light irradiation.

[0026] According to the present invention, in step (12), the mixed solution can be placed on a polytetrafluoroethylene plate with grooves and then placed under an ultraviolet lamp.

[0027] According to the present invention, the conditions for the click reaction in step (12) are: irradiation with 365nm ultraviolet light for 1 to 30 minutes.

[0028] According to the present invention, the solid obtained after the reaction in step (12) can be dried. The drying is selected from at least one of room temperature drying, vacuum drying, heating drying and freeze drying; preferably, the drying conditions include: a temperature of 30 to 120°C and a time of 1 to 24 hours.

[0029] According to the present invention, the free radical polymerization reaction includes the following steps:

[0030] (21) Mix the monomer, modifier, initiator, crosslinking agent and metal salt to obtain a mixed solution;

[0031] (22) The mixed solution obtained in step (21) is subjected to a polymerization reaction to obtain the ionic conductor material.

[0032] According to the present invention, the initiator in step (21) is a thermal initiator.

[0033] According to the present invention, the mixing conditions in step (21) are: temperature of 20-50°C and time of 10-30 h. The mixing is carried out under stirring.

[0034] According to the present invention, when the raw materials in step (11) include inorganic fillers, the mixed solution obtained in step (11) is poured onto the inorganic fillers and then a polymerization reaction is carried out.

[0035] According to the present invention, in step (22), the mixed solution can be placed on a polytetrafluoroethylene plate with grooves and then subjected to polymerization reaction.

[0036] According to the present invention, in step (22), the polymerization reaction conditions are: heating at 60-80°C for 8-24 hours. A vacuum drying oven is preferably used as the reaction apparatus.

[0037] A third aspect of the present invention provides an ion conductor material prepared by the aforementioned preparation method.

[0038] The fourth aspect of the present invention provides the application of the above-described ion conductor material or the ion conductor material prepared by the above-described method as a separator, solid electrolyte or binder in metal batteries, secondary ion batteries, flexible batteries, capacitors or hybrid energy storage devices.

[0039] According to the present invention, preferably, the application is an application in lithium batteries.

[0040] Compared with the prior art, the beneficial technical effects of the present invention mainly include:

[0041] (1) The ion conductor material provided by this invention improves the ability of the polymer substrate to dissociate metal salts by grafting small molecule modifiers with strong electron-donating groups, thereby obtaining an ion conductor material with high ionic conductivity and high mechanical strength. When formed into a film, it can be made to have good elasticity.

[0042] (2) The present invention uses small molecule modifiers or inorganic fillers as modifiers, which have good compatibility with polymer substrates and can directly obtain a homogeneous solution through reaction, making the preparation relatively simple.

[0043] (3) Different small molecule modifiers can be grafted according to the different functional groups of the polymer. Groups such as nitro, carboxyl or carbonyl, amino, hydroxyl and ester can be used as strong polar groups to achieve the construction of high-speed ion transport channels and improve ion transport efficiency through dissociation and coordination with metal salts.

[0044] (4) The groups in small molecule modifiers can also induce metal ion salts to dissociate into metal ions, increase the proportion of charge carriers in the system, and facilitate ion transport. Different small molecule modifiers can also change the polymer morphology by grafting or blocking polymer chains, thereby enhancing and toughening the polymer substrate, improving the self-support of the substrate, and providing conditions for the preparation of high ionic conductivity and high elasticity ionic conductors.

[0045] (5) The ion conductor material of the present invention, as a solid electrolyte membrane, possesses the advantages of high elasticity, high ion conductivity, high mechanical strength, and high flame retardancy. The assembled battery exhibits low overpotential, high energy density, and excellent cycle performance. The ion conductor material obtained by the present invention is suitable for preparing lithium-ion batteries as a solid electrolyte and can be applied to metal batteries, secondary ion batteries, flexible batteries, capacitors, or hybrid energy storage devices, etc. Attached Figure Description

[0046] Figure 1 This is a scanning electron microscope image of the surface of the ion conductor material prepared in Example 1;

[0047] Figure 2 , Figure 3 This is a stress-strain curve of the ion conductor material prepared in Example 5;

[0048] Figure 4 This is a linear sweep voltammetry curve of the ion conductor material prepared in Example 1;

[0049] Figure 5 This is a cycle performance diagram of a symmetrical battery assembled from the ion conductor material prepared in Example 1;

[0050] Figure 6 This is a graph showing the cycling performance of a full cell assembled from the ion conductor material prepared in Example 1 at a current density of 0.2C. Detailed Implementation

[0051] The endpoints and any values ​​of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of the various ranges, the endpoint values ​​of the various ranges and individual point values, and individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.

[0052] In this invention, an electrochemical workstation, model CHI760e, is used to test the ionic conductivity. Specifically, the ionic conductor material is placed between two stainless steel pads for measurement, and the electrochemical workstation is connected to perform AC impedance testing at a frequency of 1MHz-0.1Hz.

[0053] In this invention, the structure of the lithium-ion battery is known to those skilled in the art, and symmetrical batteries and full batteries are assembled for electrochemical testing and analysis.

[0054] The symmetrical battery assembly process is as follows: negative electrode shell, lithium sheet, prepared ion conductor material, lithium sheet, and positive electrode shell are placed sequentially, and then placed in a packaging machine and pressurized to 50 MPa. The full battery assembly process is as follows: negative electrode shell, lithium sheet, ion conductor material, positive electrode sheet, and positive electrode shell are placed sequentially, and then placed in a packaging machine and pressurized to 50 MPa. The entire battery assembly process must be carried out in an argon-filled glove box. The CT2001A Blue Battery Testing System is used to test the electrochemical performance of the assembled batteries. Cycle performance is analyzed by constant current charge-discharge testing of the symmetrical battery under stepped current density conditions: voltage range 2.5-4.2V, current density 0.1 mA cm⁻¹. -2 The reversible specific capacity was determined by constant current charge-discharge testing of the full battery under the following conditions: voltage range 2.5-4.2V, current density 0.2C.

[0055] In this invention, the room temperature in each example is 25°C.

[0056] In this invention, the sources of materials for each example are as follows:

[0057] Vinyl silicone oil: purchased from Jipeng Silicone Materials Co., Ltd., analytical grade AR;

[0058] Butyl mercaptopropionate: purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., analytical grade AR, weight average molecular weight Mw~162.25;

[0059] Mercaptopropionic acid: purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., analytical grade AR, molecular weight 292.24;

[0060] Lithium-doped hydroxyapatite was prepared by the following method: 0.331 g of anhydrous calcium chloride was dissolved in 40 mL of water, and 4.8 g of sodium oleate was dissolved in 50 mL of water. After each dissolution, the solutions were stirred for 1 h. The pH was adjusted to 10, and 50 mL of a solution containing 0.56 g of sodium dihydrogen phosphate was added. The solutions were stirred for 30 min, and then 0.133 g of lithium nitrate was added. After stirring for 1 h, a precursor solution was obtained. The precursor solution was placed in a microwave hydrothermal reactor and kept at 200 °C for 4 h. The reaction product was cooled to room temperature, washed with water and alcohol, and then dispersed in water. After washing with water and filtration, the product was dried at 60 °C for 12 h to obtain lithium-doped hydroxyapatite.

[0061] Example 1

[0062] This example demonstrates the preparation of ionic conductor materials using a click reaction method.

[0063] 0.8 g of butyl mercaptopropionate was dissolved in 3 g of vinyl silicone oil (weight average molecular weight 10000). 0.005 g of 2,2-dimethoxy-2-phenylacetophenone was added, and the mixture was stirred for 12 h. Then, 0.9 g of lithium bis(trifluoromethanesulfonyl)imide was added, and the mixture was stirred for 12 h. 0.03 g of 2,2'-(1,2-ethylenedioxy)bis(ethanesulfonyl)thiol was added, and the mixture was stirred for 2 h. The mixture was then cast onto 0.18 g of lithium-doped hydroxyapatite fiber membrane, and then irradiated under a UV lamp at 365 nm for 5 min. After that, it was dried at 80 °C in a vacuum environment for 12 h to obtain the ion conductor material.

[0064] Scanning electron microscopy (SEM) analysis of the surface of the ion-conducting material revealed a smooth surface structure, such as... Figure 1 As shown.

[0065] The electrochemical performance test data of the ion conductor materials are shown in Table 1.

[0066] Example 2

[0067] This example demonstrates the preparation of ionic conductor materials using a click reaction method.

[0068] 0.3g of butyl mercaptopropionate was dissolved in 3g of vinyl silicone oil (weight average molecular weight 8000), 0.01g of 2-hydroxy-methylphenylpropane-1-one was added, and the mixture was stirred for 12h. Then, 3g of lithium hexafluorophosphate was added and stirred for 12h. After adding 0.01g of 4,4′-dimercaptodiphenyl ether and stirring for 2h, the mixed solution was cast onto 0.36g of lithium-doped hydroxyapatite fiber membrane, and then irradiated under a UV lamp at 365nm for 15min. Subsequently, it was dried at 30℃ in a vacuum environment for 24h to obtain the ion conductor material.

[0069] The electrochemical performance test data of the ion conductor materials are shown in Table 1.

[0070] Example 3

[0071] This example demonstrates the preparation of ionic conductor materials using a click reaction method.

[0072] 0.8 g of butyl mercaptopropionate was dissolved in 3 g of vinyl silicone oil (weight average molecular weight 20000). 0.007 g of 2,4,6-trimethylbenzoyl diphenylphosphine oxide was added and stirred for 12 h. Then, 0.9 g of lithium difluorosulfonylimide was added and stirred for 12 h. 0.003 g of pentaerythritol tetrakis(3-mercaptopropionate) was added and stirred for 2 h. The mixed solution was then cast onto 0.6 g of lithium-doped hydroxyapatite fiber membrane and irradiated under a UV lamp at 365 nm for 25 min. Subsequently, it was dried at 80 °C in a vacuum environment for 20 h to obtain the ion conductor material.

[0073] The electrochemical performance test data of the ion conductor materials are shown in Table 1.

[0074] Example 4

[0075] This example demonstrates the preparation of ionic conductor materials using a click reaction method.

[0076] 0.15 g of butyl mercaptopropionate was dissolved in 3 g of vinyl silicone oil (weight average molecular weight 10000). 0.005 g of 2,2-dimethoxy-2-phenylacetophenone was added, and the mixture was stirred for 12 h. Then, 0.9 g of lithium bis(trifluoromethanesulfonyl)imide was added, and the mixture was stirred for 12 h. 0.03 g of 2,2'-(1,2-ethylenedioxy)bis(ethanesulfonyl)thiol was added, and the mixture was stirred for 2 h. The mixture was then cast onto 0.18 g of lithium-doped hydroxyapatite fiber membrane, and then irradiated under a UV lamp at 365 nm for 5 min. After that, it was dried at 80 °C in a vacuum environment for 12 h to obtain the ion conductor material.

[0077] The electrochemical performance test data of the ion conductor materials are shown in Table 1.

[0078] Example 5

[0079] The only difference between this example and Example 1 is that it does not contain lithium-doped hydroxyapatite. That is, the raw materials (which do not contain lithium-doped hydroxyapatite, and the other raw materials are the same as in Example 1) are mixed to obtain a mixed solution, which is then poured into a polytetrafluoroethylene mold, irradiated under a UV lamp at 365nm for 5 minutes, and then dried at 80°C in a vacuum environment for 12 hours to obtain an ion conductor material.

[0080] The electrochemical performance test data of the ion conductor materials are shown in Table 1.

[0081] Example 6

[0082] The only difference between this example and Example 5 is that polyethylene glycol diacrylate (weight average molecular weight of 5000) is used instead of the vinyl silicone oil in Example 5.

[0083] The electrochemical performance test data of the ion conductor materials are shown in Table 1.

[0084] Example 7

[0085] The only difference between this example and Example 5 is that mercaptopropionic acid is used instead of butyl mercaptopropionate in Example 5.

[0086] The electrochemical performance test data of the ion conductor materials are shown in Table 1.

[0087] Example 8

[0088] This example demonstrates the preparation of ionic conductor materials using free radical polymerization.

[0089] 0.8 g of butyl mercaptopropionate was dissolved in 3 g of vinyl silicone oil (weight average molecular weight of 10000), 0.005 g of azobisisoheptanenitrile was added, and the mixture was stirred for 12 h. Then, 0.9 g of lithium bis(trifluoromethanesulfonyl)imide was added and stirred for 12 h. After that, 0.03 g of 2,2'-(1,2-ethylenedioxy)bis(ethanethiol) was added and stirred for 2 h. The mixed solution was then poured into a polytetrafluoroethylene mold and reacted at 80 °C under vacuum for 12 h to obtain an ion conductor material.

[0090] The electrochemical performance test data of the ion conductor materials are shown in Table 1.

[0091] Table 1

[0092]

[0093] The specific embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combining the various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.

Claims

1. An ionic conductor material, wherein, The ion conductor material is prepared using the following raw materials: monomer, modifier, initiator, crosslinking agent, and metal salt; The monomer includes at least one of polyethylene glycol diacrylate, polynorbornene, polyacrylate, polybutadiene, polyisoprene, polychloroprene, styrene-butadiene rubber, and vinyl silicone oil, preferably vinyl silicone oil; The modifier includes at least one of mercaptopropionic acid, 3-mercaptopropionitrile, 2-mercaptoethylamine, sodium 3-mercapto-1-propanesulfonate, 2-mercapto-3-pentanone, 8-mercapto-1-octanol, 4-mercaptobenzyl alcohol, sodium vinyl sulfonate, propylene glycol monoacrylate, 3-vinylaniline, N-vinylacetamide, and butyl mercaptopropionate, preferably butyl mercaptopropionate.

2. The ion conductor material according to claim 1, characterized in that, The raw materials for ion conductor materials also include inorganic fillers; the inorganic fillers are selected from at least one of hydroxyapatite, lithium-doped hydroxyapatite, tin disulfide, barium titanate, and fumed silica, preferably lithium-doped hydroxyapatite.

3. The ion conductor material according to claim 1, characterized in that, The initiator is selected from at least one of photoinitiators and thermal initiators; Preferably, the photoinitiator comprises at least one selected from 2-hydroxy-methylphenylpropane-1-one, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]-1-propanone, and 2,2-dimethoxy-2-phenylacetophenone; And / or, the thermal initiator includes at least one of azobisisobutyronitrile, azobisisoheptanenitrile, cumene hydroperoxide, tert-butyl hydroperoxide, benzoyl peroxide, and dicyclohexyl peroxide.

4. The ion conductor material according to claim 1, characterized in that, The crosslinking agent is selected from at least one of pentaerythritol tetrakis(3-mercaptopropionic acid), 4,4′-dimercaptodiphenyl ether, and 2,2′-(1,2-ethylenedioxy)diethyl mercaptan; And / or, the metal salt comprises at least one of lithium sulfate, lithium nitrate, lithium chloride, lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, zinc sulfate, zinc nitrate, zinc chloride, zinc bis(fluoromethanesulfonyl)imide, sodium sulfate, sodium nitrate, sodium chloride, sodium hexafluorophosphate, potassium sulfate, potassium nitrate, potassium chloride, and potassium bis(fluoromethanesulfonyl)imide.

5. The ion conductor material according to claim 1, characterized in that, The mass ratio of the modifier to the monomer is 1:1 to 50, preferably 1:1 to 10; And / or, the mass ratio of the initiator to the monomer is 1:1 to 600, preferably 1:300 to 600; And / or, the mass ratio of the crosslinking agent to the monomer is 1:1 to 1000, preferably 1:100 to 1000; And / or, the mass ratio of the inorganic filler to the monomer is 1:1 to 50, preferably 1:1 to 20; And / or, the mass ratio of the metal salt to the monomer is 1:1 to 20, preferably 1:1 to 5.

6. A method for preparing the ion conductor material according to any one of claims 1 to 5, wherein, The method is selected from one of click reaction, amine-olefin addition reaction and free radical polymerization reaction, with click reaction being preferred.

7. The method according to claim 6, characterized in that, The click response includes the following steps: (11) Mix the monomer, modifier, initiator, crosslinking agent and metal salt to obtain a mixed solution; (12) The ionic conductor material is prepared by clicking reaction of the mixed solution obtained in step (11) under ultraviolet light irradiation.

8. The method according to claim 7, characterized in that, The initiator mentioned in step (11) is a photoinitiator.

9. The method according to claim 7, characterized in that, The conditions for the click reaction in step (12) are: irradiation with ultraviolet light for 1 to 30 minutes; and / or, the ultraviolet light is 365 nm.

10. The method according to claim 6, characterized in that, The free radical polymerization reaction includes the following steps: (21) Mix the monomer, modifier, initiator, crosslinking agent and metal salt to obtain a mixed solution; (22) The mixed solution obtained in step (21) is subjected to a polymerization reaction to obtain the ionic conductor material.

11. The method according to claim 10, characterized in that, The initiator mentioned in step (21) is a thermal initiator.

12. The method according to claim 10, characterized in that, The conditions for the polymerization reaction in step (22) are: heating at 60-80°C for 8-24 hours.

13. An ion conductor material prepared by any one of claims 6 to 12.

14. The use of the ion conductor material according to any one of claims 1 to 5 or the ion conductor material prepared by any one of claims 6 to 12 as a separator, solid electrolyte or binder in metal batteries, secondary ion batteries, flexible batteries, capacitors or hybrid energy storage devices.

15. The application according to claim 14, characterized in that, The application is in lithium batteries.

Citation Information

Patent Citations

  • In-situ polymer electrolyte, preparation method and battery

    CN118572184A