Positive electrode active material coated with SI and its coating method
By coating the surface of the high-nickel ternary cathode active material with amorphous SiO2 and doping it with Al, Ti or Zr to form a composite coating layer, the problems of decreased lifespan characteristics and increased resistance at high temperatures are solved, and the stability and charge/discharge efficiency of the battery are improved.
Patent Information
- Application Number
- CN202580020363.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-10-22
- Filing Date
- 2025-10-01
- Publication Date
- 2026-11-10
AI Technical Summary
High-nickel ternary cathode active materials exhibit decreased lifespan characteristics and increased resistance at high temperatures, and also undergo side reactions with the electrolyte, resulting in poor battery performance.
Amorphous SiO2 is coated onto the surface of a high-nickel ternary cathode active material and doped with elements such as Al, Ti, or Zr to form a composite coating layer, thereby improving the stability of the surface and interior.
It improves lifespan characteristics and charge/discharge efficiency, reduces gas generation, and enhances battery safety and structural stability under high-temperature conditions.
Smart Images

Figure CN123076931A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the manufacturing technology of positive electrode active materials for lithium secondary batteries, and particularly to a technique for coating the surface of a ternary positive electrode active material with high nickel (Ni) content with amorphous SiO2 to improve the battery's lifespan characteristics and charge / discharge efficiency. It provides a high-performance positive electrode active material applicable to high-capacity lithium secondary batteries used in electric vehicles, energy storage devices, and other applications. Background Technology
[0002] The higher the Ni content in ternary cathode active materials (Ni, Co, Mn), the greater the energy capacity of the battery. However, this also leads to problems such as decreased lifespan, increased resistance, and gas generation. In existing technologies, methods such as coating the surface of the cathode active material with stabilizing agents or performing heat treatment have been proposed to address these issues. However, these methods have limitations due to the unevenness of surface coating and side reactions, preventing the full realization of satisfactory performance.
[0003] For high-nickel ternary cathode active materials, they are particularly prone to side reactions with the electrolyte, which leads to a decrease in lifespan characteristics at high temperatures. Therefore, new technologies are needed to improve this problem. Summary of the Invention
[0004] The technical problem that an invention aims to solve.
[0005] The purpose of this invention is to provide a high-capacity lithium secondary battery, which improves lifespan characteristics and charge / discharge efficiency by coating the surface of the high-nickel ternary cathode active material with amorphous SiO2, and ensures the long-term stability of the cathode active material.
[0006] Technical solution.
[0007] To achieve the above objectives, one example of the present invention provides a positive electrode active material for secondary batteries comprising the following elements: a) 60 to 99 mol% Ni; b) Si; and c) one or more elements selected from the group consisting of Na, Al, Mg, Zn, Fe, Ba, Ti, Zr, B, and W.
[0008] The Si may exist at a concentration of 0.9 atomic percent or more on the surface of the positive electrode active material and at a depth of 500 nm or more from the surface.
[0009] c) can be Al, Ti, or Zr.
[0010] The elements in b) and c) can form a coating layer of the positive electrode active material.
[0011] The positive electrode active material may further include d) Co; and e) Mn.
[0012] Another embodiment of the present invention provides a method for manufacturing a positive electrode active material for a secondary battery, comprising: a step of generating a hydroxide precursor using a metal salt containing Ni; a step of mixing the hydroxide precursor, lithium, and one or more compounds independently comprising an element selected from the group consisting of Al, Ti, Zr, Mg, Zn, B, Mo, Fe, Co, Ni, Ba, and W to prepare a first mixture; a step of calcining the first mixture at 600 to 700°C for 10 to 14 hours under an O2 atmosphere to obtain a first lithium composite oxide; and a step of adding an element independently comprising an element selected from the group consisting of Al, Ti, Zr, Mg, Zn, B, Mo, Fe, Co, Ni, Ba, and W to the first lithium composite oxide. The steps include: preparing a second mixture using compounds of one or more elements from the group consisting of Al, Ti, Zr, Mg, Zn, B, Mo, Fe, Co, Ni, Ba, and W, as well as compounds containing Si; calcining the second mixture at 650 to 750°C for 10 to 14 hours under an O2 atmosphere to obtain a second lithium composite oxide; dehydrating the second lithium composite oxide after mixing it with water at 20 to 30°C for at least 30 minutes; and drying the second lithium composite oxide after the dehydration step by heat-treating it at 250 to 350°C for at least 8 hours under an O2 atmosphere.
[0013] The metal salt may further include Co and Mn.
[0014] The step of preparing the first mixture may be the step of preparing the first mixture by mixing the hydroxide precursor, lithium, and a compound containing Zr.
[0015] The Zr-containing compound is ZrO2, and may be 0.1 to 0.5 mol relative to the oxide precursor.
[0016] The step of preparing the second mixture may be to add a compound containing Si, a compound containing Al, a compound containing Ti, and a compound containing Zr to the first lithium composite oxide to prepare the second mixture.
[0017] The compound containing Si is 0.01 to 1.0 mol% SiO2, the compound containing Al is 0.3 to 1.0 mol% Al2O3, the compound containing Ti is 0.3 to 1.0 mol% TiO2, and the compound containing Zr can be 0.05 to 0.2 mol% ZrO2.
[0018] Beneficial effects.
[0019] According to an example of the high-nickel ternary cathode active material doped and coated with SiO2 of the present invention, the interfacial reaction with the electrolyte can be suppressed to improve lifespan characteristics, and the resistance characteristics can be improved to increase charge and discharge efficiency. In addition, the gas generated during charge and discharge can be reduced to improve battery safety, and the structural stability of the cathode active material can be maintained even at high temperatures, thereby preventing long-term performance degradation. Attached Figure Description
[0020] Figure 1 The image is a photograph taken by SEM of the residual Si material on the surface of the positive electrode active material coated with Si.
[0021] Figure 2 This is a schematic diagram roughly showing the location where XPS analysis was performed to confirm the distribution of elements in the Si-coated cathode active material.
[0022] Figure 3a This is a graph showing the results of XPS analysis performed to confirm the presence and concentration of each element in the Si-coated positive electrode active material.
[0023] Figure 3b This is a graph showing the results of XPS analysis performed to confirm the presence and concentration of each element in the Si-coated positive electrode active material.
[0024] Figure 4 This is a graph showing the volume change over time in the positive electrode active material coated with Si. Detailed Implementation
[0025] The specific details for implementing the present invention will now be described in detail with reference to the accompanying drawings. However, in the following description, specific descriptions of well-known functions or configurations will be omitted to avoid unnecessarily obscuring the spirit of the invention.
[0026] The advantages and features of the embodiments disclosed in this specification, as well as the methods for implementing them, will be described with reference to the appendix. Figure 1 As will become clear from the embodiments described below. However, the invention is not limited to the embodiments disclosed below, but can be implemented in many different forms. These embodiments are provided merely to enable those skilled in the art to fully understand the scope of the invention.
[0027] Unless otherwise defined, all terms (including technical and scientific terms) used in this specification may be used in the sense that can be commonly understood by one of ordinary skill in the art to which this invention pertains. Furthermore, terms generally used and defined in dictionaries should not be interpreted ideally or excessively unless explicitly defined otherwise.
[0028] In this specification, singular expressions include plural expressions unless explicitly specified in the context. Similarly, plural expressions include singular expressions unless explicitly specified in the context. Throughout this specification, when a part includes a constituent element, this does not exclude other constituent elements, but rather implies that further constituent elements may be included.
[0029] In this invention, terms such as "comprising" and "including" can indicate the presence of features, steps, actions, elements and / or constituent elements, but these terms do not exclude the addition of one or more other functions, steps, actions, elements, constituent elements and / or combinations thereof.
[0030] One example of the present invention provides a positive electrode active material for secondary batteries comprising a) 60 to 99 mol% Ni; b) Si; and c) one or more elements selected from the group consisting of Na, Al, Mg, Zn, Fe, Ba, Ti, Zr, B, and W. To improve conductivity, the positive electrode active material may include various forms of ternary transition metal compounds with Ni, preferably Ni, Co, and Mn as essential components. A representative example of such ternary transition metal compounds is a selection of Li(Ni)... 1 / 3 Mn 1 / 3 Co 1 / 3 O2, Li(Ni) 0.5 Mn 0.3 Co 0.2 O2, Li(Ni) 0.2 Co 0.2 Mn 0.6 O2, Li(Ni) 0.6 Co 0.2 Mn 0.2 O2, Li(Ni) 0.3 Co 0.2 Mn 0.5 O2, Li(Ni) 0.3 Co 0.3 Mn 0.4 O2 and Li(Ni) 0.6 Co 0.2 Mn 0.15 Zr 0.05The active material is a single substance or a mixture of two or more substances from the group consisting of O2, preferably a high-nickel active material with a Ni content of 60 to 99 mol%. In this case, for high-nickel cathode active materials with high Ni content, especially those with approximately 80 mol% or more, the capacity increases with increasing Ni content, but disadvantages such as increased resistance, reduced lifetime, and volume expansion due to gas generation may occur. However, the cathode active material according to an example of the present invention eliminates the above-mentioned disadvantages by forming a composite coating layer containing Si elements, and can exhibit excellent lifetime characteristics, reduced gas generation, and reduced resistance.
[0031] To eliminate the aforementioned drawbacks, the positive electrode active material can be coated. In this case, the coating layer may contain Si, preferably a composite coating layer containing Si. The composite coating layer may further contain one or more elements selected from the group consisting of Al, Ti, Zr, Mg, Zn, B, Mo, Fe, Co, Ni, Ba, and W. Compared to a coating layer containing only Si, the composite coating layer exhibits superior performance in terms of lifetime characteristics and resistance reduction.
[0032] In the coating layer and / or composite coating layer, Si can be present on the surface of the positive electrode active material and at a depth of 500 nm or more from the surface. This means that during the formation of the coating layer, the coating layer is not simply distributed on the outer surface of the positive electrode active material, but rather the material forming the coating layer diffuses to a certain depth to form a thick coating layer. In particular, in the coating layer or composite coating layer, Si can be present at a concentration of 5.0 atomic% or more at the surface, 2.0 atomic% or more at a depth of 250 nm from the surface, and 1.5 atomic% or more at a depth of 500 nm from the surface.
[0033] In this case, if the coating layer is a composite coating layer, c) can be Al, Ti and Zr. At this point, Al can exist at a concentration of 2.0, 2.5, or 2.7 atoms or more on the surface, at a concentration of 1.5, 2.0, or 2.3 atoms or more at 250 nm from the surface, and at a concentration of 2.0 or 3.0 atoms or more at 500 nm from the surface. Ti can exist at a concentration of 1.5, 1.7, or 2.0 atoms or more on the surface, at a concentration of 0.8, 0.9, or 1.0 atoms or more at 250 nm from the surface, and at a concentration of 0.6, 0.7, or 0.8 atoms or more at 500 nm from the surface. Zr can exist at a concentration of 0.4 or 0.5 atoms or more on the surface, at a concentration of 0.6, 0.7, or 0.8 atoms or more at 250 nm from the surface, and at a concentration of 0.4, 0.5, or 0.6 atoms or more at 500 nm from the surface.
[0034] The elements in b) and c) can form a coating layer of the positive electrode active material, preferably a composite coating layer.
[0035] Another embodiment of the present invention provides a manufacturing method comprising: a step of generating a hydroxide precursor using a metal salt containing Ni; a step of mixing the hydroxide precursor, lithium, and one or more compounds independently comprising an element selected from the group consisting of Al, Ti, Zr, Mg, Zn, B, Mo, Fe, Co, Ni, Ba, and W to prepare a first mixture; a step of calcining the first mixture at 500 to 800°C, preferably 600 to 700°C, under an O2 atmosphere for at least 8 hours, 9 hours, or 10 hours, preferably 10 to 14 hours, to obtain a first lithium composite oxide; and a step of adding one or more compounds independently comprising an element selected from the group consisting of Al, Ti, Zr, Mg, Zn, B, Mo, Fe, Co, Ni, Ba, and W to the first lithium composite oxide. The process involves the following steps: preparing a second mixture from two or more compounds, preferably three or more compounds, and a compound containing Si; calcining the second mixture under an O2 atmosphere at 500 to 900°C, 600 to 800°C, preferably 650 to 750°C, for at least 9 hours, 10 hours, or preferably 10 to 14 hours to obtain a second lithium composite oxide; mixing the second lithium composite oxide with water at 10 to 40°C, preferably 20 to 30°C, for at least 10 minutes, 20 minutes, or preferably 30 minutes, or less than 1 hour, followed by dehydration; and drying the second lithium composite oxide after the dehydration step under an O2 atmosphere at 200 to 400°C, preferably 250 to 350°C, for at least 6 hours, 7 hours, preferably 8 hours, or less than 10 hours.
[0036] The metal salt may further include Co and Mn metal salts to form a metal salt for use as a ternary cathode active material. At this time, the hydroxide precursor can be in the following proportions: 60 to 99 mol%, 65 to 99 mol%, 70 to 99 mol%, 75 to 99 mol%, 80 to 99 mol%, 85 to 99 mol%, 90 to 99 mol%, 95 to 99 mol%, 60 to 95 mol%, 65 to 95 mol%, 70 to 95 mol%, 75 to 95 mol%, 80 to 95 mol%, 85 to 95 mol%, 90 to 95 mol%, 60 to 93 mol%, 65 to 93 mol%, 70 to 93 mol%, 75 to 93 mol%, 80 to 93 mol%, 85 to 93 mol%, 90 to 93 mol%, 60 to 90 mol%, 65 to 90 mol%, 70 to 90 mol%, 75 to 90 mol%, 80 to 90 mol%, 85 to 90 mol%. The composition may contain Ni in the following proportions: 85 to 95 mol%, preferably 85.0 to 90.4 mol%, and may contain Co in the following proportions: 8.0 to 15.0 mol%, 8.5 to 15.0 mol%, 9.0 to 15.0 mol%, 8.0 to 14.0 mol%, 8.5 to 14.0 mol%, preferably 8.0 to 14.0 mol%, or 8.4 to 13.4 mol%. The composition may contain Co in the following proportions: 0.5 to 2.0 mol%, 0.8 to 2.0 mol%, 1.0 to 2.0 mol%, 0.5 to 1.5 mol%, 0.8 to 1.5 mol%, 1.0 to 1.5 mol%, 0.5 to 1.3 mol%, 0.8 to 1.3 mol%, 1.0 to 1.3 mol%, preferably 1.0 to 1.5 mol%, or 1.0 to 1.2 mol%. The step of preparing the first mixture can be a step of mixing the hydroxide precursor, lithium, and one or more compounds that independently contain elements selected from the group consisting of Al, Ti, Zr, Mg, Zn, B, Mo, Fe, Co, Ni, Ba, and W to prepare the first mixture. The elements selected from the group consisting of Al, Ti, Zr, Mg, Zn, B, Mo, Fe, Co, Ni, Ba, and W can be elements used for doping the positive electrode active material, preferably compounds containing Zr. In this case, the Zr-containing compound can be ZrO2, and the ZrO2 content relative to the oxide precursor can be 0.1 to 0.5 mol%, 0.2 to 0.4 mol%, preferably 0.3 mol%. If the content of the dopant element exceeds 0.5 mol%, an initial capacity decrease and an increase in resistance may occur in the electrochemical characteristics.
[0037] In the step of preparing the second mixture, a compound independently containing one or more elements selected from the group consisting of Al, Ti, Zr, Mg, Zn, B, Mo, Fe, Co, Ni, Ba, and W is used for coating the positive electrode active material. In this case, one or more elements selected from the group consisting of Al, Ti, Zr, Mg, Zn, B, Mo, Fe, Co, Ni, Ba, and W can form a composite coating layer together with Si. Specifically, a single Si coating layer may not exhibit superior performance compared to a composite coating layer in terms of resistivity, while a composite coating layer containing one or more, two or more, or preferably three or more elements selected from the group consisting of Al, Ti, Zr, Mg, Zn, B, Mo, Fe, Co, Ni, Ba, and W can exhibit superior electrochemical properties compared to a single coating layer in terms of initial capacity, C-rate, resistivity, and high-temperature cycle retention. The compound used to form the composite coating layer can be a compound containing Si, a compound containing Al, a compound containing Ti, or a compound containing Zr.At this time, the compound containing Si can be SiO2, and can be 0.01 to 1.0 mol%, 0.01 to 0.9 mol%, 0.01 to 0.8 mol%, 0.01 to 0.7 mol%, 0.01 to 0.6 mol%, 0.01 to 0.5 mol%, 0.01 to 0.45 mol%, 0.01 to 0.4 mol%, 0.01 to 0.35 mol%, 0.01 to 0.3 mol%, 0.01 to 0.25 mol%, 0.01 to 0.2 mol%, 0.01 to 0.15 mol%, 0.01 to 0.1 mol%, 0.05 to 1.0 mol%, 0.05 to 0.9 mol%, 0.05 to 0.8 mol%, 0.05 to 0.7 mol%, 0.05 to 0.6 mol%, 0.05 to 0.5 mol%. mol%, 0.05 to 0.45 mol%, 0.05 to 0.4 mol%, 0.05 to 0.35 mol%, 0.05 to 0.3 mol%, 0.05 to 0.25 mol%, 0.05 to 0.2 mol%, 0.05 to 0.15 mol%, 0.05 to 0.1 mol%, 0.1 to 1.0 mol%, 0.1 to 0.9 mol%, 0.1 to 0.8 mol%, 0.1 to 0.7 mol%, 0.1 to 0.6 mol%, 0.1 to 0.5 mol%, 0.1 to 0.45 mol%, 0.1 to 0.4 mol%, 0.1 to 0.35 mol%, 0.1 to 0.3 mol%, 0.1 to 0.25 mol%, 0.1 to 0.2 mol%, 0.1 to 0.15 mol%, 0.15 to 1.0 mol%. mol%, 0.15 to 0.9 mol%, 0.15 to 0.8 mol%, 0.15 to 0.7 mol%, 0.15 to 0.6 mol%, 0.15 to 0.5 mol%, 0.15 to 0.45 mol%, 0.15 to 0.4 mol%, 0.15 to 0.35 mol%, 0.15 to 0.3 mol%, 0.15 to 0.25 mol%, 0.15 to 0.2 mol%, 0.15 to 0.15 mol%, 0.15 to 0.1 mol%, preferably 0.05 to 0.5 mol%, 0.1 to 0.5 mol%, 0.1 to 0.35 mol%.The compound containing Al can be Al₂O₃, and can be 0.1 to 1.0 mol%, 0.1 to 0.9 mol%, 0.1 to 0.8 mol%, 0.1 to 0.7 mol%, 0.1 to 0.6 mol%, 0.2 to 1.0 mol%, 0.2 to 0.9 mol%, 0.2 to 0.8 mol%, 0.2 to 0.7 mol%, 0.2 to 0.6 mol%, 0.3 to 1.0 mol%, 0.3 to 0.9 mol%, 0.3 to 0.8 mol%, 0.3 to 0.7 mol%, 0.3 to 0.6 mol%, 0.4 to 1.0 mol%, 0.4 to 0.9 mol%, 0.4 to 0.8 mol%, 0.4 to 0.7 mol%, 0.4 to 0.6 mol%, 0.5 to 1.0 mol%, 0.5 to 0.9 mol%, 0.5 to 0.8 mol%. 0.5 to 0.7 mol%, 0.5 to 0.6 mol%, preferably 0.5 to 0.7 mol%, 0.6 mol%. The Ti-containing compound can be TiO2, and can be 0.1 to 1.0 mol%, 0.1 to 0.9 mol%, 0.1 to 0.8 mol%, 0.1 to 0.7 mol%, 0.1 to 0.6 mol%, 0.2 to 1.0 mol%, 0.2 to 0.9 mol%, 0.2 to 0.8 mol%, 0.2 to 0.7 mol%, 0.2 to 0.6 mol%, 0.3 to 1.0 mol%, 0.3 to 0.9 mol%, 0.3 to 0.8 mol%, 0.3 to 0.7 mol%, 0.3 to 0.6 mol%, 0.4 to 1.0 mol%, 0.4 to 0.9 mol%, 0.4 to 0.8 mol%, 0.4 to 0.7 mol%, 0.4 to 0.6 mol%, 0.5 to 1.0 mol%, 0.5 to 0.9 mol%, 0.5 to 0.8 mol%. 0.5 to 0.7 mol%, 0.5 to 0.6 mol%, preferably 0.5 to 0.7 mol%, 0.6 mol%.The compound containing Zr can be ZrO2, and can be 0.01 to 0.2 mol%, 0.02 to 0.2 mol%, 0.03 to 0.2 mol%, 0.04 to 0.2 mol%, 0.05 to 0.2 mol%, 0.06 to 0.2 mol%, 0.07 to 0.2 mol%, 0.08 to 0.2 mol%, 0.09 to 0.2 mol%, 0.1 to 0.2 mol%, 0.01 to 0.15 mol%, 0.02 to 0.15 mol%, 0.03 to 0.15 mol%, 0.04 to 0.15 mol%, 0.05 to 0.15 mol%, 0.06 to 0.15 mol%, 0.07 to 0.15 mol%, 0.08 to 0.15 mol%, 0.09 to 0.15 mol%, 0.1 to 0.15 mol%. mol%, 0.01 to 0.1 mol%, 0.02 to 0.1 mol%, 0.03 to 0.1 mol%, 0.04 to 0.1 mol%, 0.05 to 0.1 mol%, 0.06 to 0.1 mol%, 0.07 to 0.1 mol%, 0.08 to 0.1 mol%, 0.09 to 0.1 mol%, 0.1 to 0.1 mol%. However, the examples of the compounds and concentrations are not limited thereto.
[0038] Hereinafter, the positive electrode active material and its manufacturing method according to embodiments of the present invention will be described in detail with reference to the accompanying drawings.
[0039] Example 1.
[0040] (a) Precursor preparation process Hydroxide precursors containing transition metals, namely nickel (Ni), cobalt (Co), and manganese (Mn), are generated using nickel (Ni), cobalt (Co), and manganese (Mn) metal salts, respectively, in amounts of 85.0 to 90.4 mol%, 8.4 to 13.4 mol%, and 1.0 to 1.2 mol%.
[0041] (b) First heat treatment process The hydroxide precursor obtained in process (a) is mixed with lithium and ZrO2 at 0.3 mol% relative to the precursor to prepare a first mixture. The first mixture is calcined at 600 to 700 °C for 10 to 14 hours under an O2 atmosphere to obtain a first lithium composite oxide.
[0042] (c) Second heat treatment process Add 0.1 mol% ZrO2, 0.6 mol% Al2O3, 0.6 mol% TiO2 and 0.10 mol% SiO2 to the first lithium composite oxide obtained in process (b) to prepare a second mixture. Then, calcine the second mixture at 650 to 750°C for 10 to 14 hours under an O2 atmosphere to obtain the second lithium composite oxide.
[0043] (d) Washing and dehydration processes The second lithium composite oxide obtained in process (c) is mixed with water at 20 to 30°C for more than 30 minutes, and then dehydrated and dried.
[0044] (e) Drying process After the process (d), the positive electrode active material is obtained by drying through heat treatment at 250 to 350°C for more than 8 hours in an O2 atmosphere.
[0045] Example 2.
[0046] The process is carried out in the same manner as in Example 1, but the process (c) is carried out as follows.
[0047] (c) Second heat treatment process Add 0.1 mol% ZrO2, 0.6 mol% Al2O3, 0.6 mol% TiO2, and 0.25 mol% SiO2 to the first lithium composite oxide obtained in process (b) to prepare a second mixture. Then, calcine the second mixture at 650 to 750°C for 10 to 14 hours under an O2 atmosphere to obtain the second lithium composite oxide.
[0048] Example 3.
[0049] The process is carried out in the same manner as in Example 1, but the process (c) is carried out as follows.
[0050] (c) Second heat treatment process Add 0.1 mol% ZrO2, 0.6 mol% Al2O3, 0.6 mol% TiO2, and 0.35 mol% SiO2 to the first lithium composite oxide obtained in process (b) to prepare a second mixture. Then, calcine the second mixture at 650 to 750°C for 10 to 14 hours under an O2 atmosphere to obtain the second lithium composite oxide.
[0051] Comparative Example 1.
[0052] The process is carried out in the same manner as in Example 1, but in process (c), SiO2 is not added to the first lithium composite oxide to obtain the second lithium composite oxide.
[0053] Comparative Example 2.
[0054] The process is carried out in the same manner as in Example 1, but in process (c), only SiO2 is added instead of compounds containing Ti, Al, or Zr to obtain the second lithium composite oxide.
[0055] Comparative Example 3.
[0056] The process was carried out in the same manner as in Example 1, except that 0.50 mol% SiO2 was added in process (c) to obtain the second lithium composite oxide.
[0057] Experimental Example 1. Confirmation of SiO2 on the Surface of the Positive Electrode Active Material To confirm whether SiO2 remains on the surface of the positive electrode active material according to an example of the present invention, in the positive electrode active material manufacturing method of Example 1, the SiO2 content (0.5 mol%, 0.25 mol%, and 0.1 mol%) and calcination temperature (675°C, 685°C, 695°C, and 700°C) of process (c) were varied to manufacture the positive electrode active material, and the surface of the manufactured positive electrode active material was scanned with a scanning electron microscope (SEM) at a beam of 15 keV for 180 seconds to confirm whether SiO2 remains. The results are as follows: Figure 1 As shown, it was confirmed that SiO2 remained on the surface of the manufactured positive electrode active material.
[0058] Experimental Example 2. Confirmation of Si Content in Each Layer of the Positive Electrode Active Material In the positive electrode active material manufactured according to Example 1, to confirm whether the Si element only remains on the outer surface of the positive electrode active material, X-ray photoelectron spectroscopy (XPS) was performed at Ion beam etch 2 keV for 250 seconds. Figure 2 As shown, the Si content of the positive electrode active material before and after the addition of SiO2 was confirmed at (A) the surface, (B) 250 nm and (C) 500 nm depth.
[0059] Table 1
[0060] The results are shown in Table 1. Figure 3a and Figure 3b As shown, not only on the surface of the positive electrode active material, but also at positions of 250 nm and 500 nm above the surface, a minimum Si element distribution of approximately 1.5 atomic percent is observed. This confirms that while Si is highly distributed on the surface, a certain amount of Si element is also diffused inside.
[0061] Experimental Example 3: Determination of Si content in positive electrode active material.
[0062] The Si content in the final positive electrode active material was determined by surface SEM and XPS analysis at the input amounts in each step, according to the methods of Examples 1 to 3 and Comparative Examples 1 to 3.
[0063] XPS analysis was performed at 2 keV for 250 seconds using an Ion beam etch at 500 nm from the surface. Surface SEM analysis was performed by scanning the surface at 15 keV for 180 seconds using a beam etch.
[0064] Table 2
[0065] As shown in Table 2, in Examples 1 to 3, the Si content of the final positive electrode active material increased as the mol% of Si increased, when Si compounds were added together with Al, Ti and Zr compounds.
[0066] Conversely, as in Comparative Example 2, when Si compound was added alone without being added together with Al, Ti, and Zr compounds, no Si was detected in the generated positive electrode active material.
[0067] Experimental Example 4: Evaluation of the electrochemical characteristics of lithium secondary batteries.
[0068] To evaluate the electrochemical characteristics of lithium secondary batteries using the positive electrode active materials manufactured according to the methods of Examples 1 to 3 and Comparative Examples 1 to 3, experiments were conducted as follows.
[0069] (1) Initial volume determination For lithium secondary batteries (half-cells) using positive electrode active materials manufactured according to the methods of Examples 1 to 3 and Comparative Examples 1 to 3, the initial charge capacity and initial discharge capacity were determined using an electrochemical analysis apparatus (Toyo, Toscat-3100) by applying a charge / discharge experiment at 25°C, a voltage range of 2.0V to 4.6V, and a discharge rate of 0.1C to 5.0C.
[0070] (2) High-temperature life test The lifetime characteristics of lithium secondary batteries (half-cells) using positive electrode active materials manufactured according to the methods of Examples 1 to 3 and Comparative Examples 1 to 3 were determined by repeated charge / discharge cycles 50 times at temperatures above 40°C, voltage ranges from 2.0V to 4.6V, and discharge rates from 0.1C to 1.0C using an electrochemical analysis apparatus (Toyo, Toscat-3100).
[0071] Table 3
[0072] As shown in Table 3, comparing Examples 1 to 3 with Comparative Example 2, the measured values of EIS (Electrochemical Impedance Spectroscopy) were significantly reduced when a composite coating was formed with Al, Ti, and Zr elements, compared to the case where only Si was used to form the coating layer.
[0073] Furthermore, comparing Examples 1 to 3 with Comparative Example 1, the high temperature cycle retention is superior when the coating layer contains Si elements, compared to the case where the composite coating layer does not contain Si elements.
[0074] Experimental Example 5: Evaluation of the volume expansion rate (gas characteristics) of lithium secondary batteries.
[0075] To determine whether and how much gas is generated in a lithium secondary battery, the volume expansion rate of the lithium secondary battery was measured.
[0076] Using a single-cell battery as the subject, after charging / discharging at 25 ℃ and a voltage range of 2.75V-4.2V, the battery was charged at 4.3V and then placed in a 70 ℃ oven. The battery volume change rate was measured twice using a digital density specific meter for each of the following measurements after 14 or 28 days.
[0077] Table 4
[0078] The results are shown in Table 4 and Figure 4 As shown, compared with Comparative Examples 1 and 2, Examples 1 and 2 also had a smaller volume, and the volume expansion rate between 14 and 28 days was also significantly reduced.
[0079] Industrial availability.
[0080] The SiO2 (composite coating of Al / Ti / Zr) high-nickel cathode active material and its manufacturing method of the present invention can be directly integrated into conventional cathode material processes consisting of co-precipitation, calcination, water washing, and low-temperature heat treatment, thus making it suitable for mass production. It can be widely used in electric vehicle batteries, energy storage devices (ESS), power tools, and high-performance mobile IT equipment requiring high energy density and high-temperature cycle stability, thus exhibiting high industrial applicability.
Claims
1. A positive electrode active material for secondary batteries, comprising the following elements: a) 60 to 99 mol% Ni; b) Si; and c) Select one or more elements from the group consisting of Na, Al, Mg, Zn, Fe, Ba, Ti, Zr, B, and W.
2. The positive electrode active material for secondary batteries according to claim 1, wherein, The Si is present at a concentration of 0.9 atomic percent or more on the surface of the positive electrode active material and at a depth of 500 nm or more from the surface.
3. The positive electrode active material for secondary batteries according to claim 1, wherein, c) refers to Al, Ti, and Zr.
4. The positive electrode active material for secondary batteries according to claim 1, wherein, The elements in b) and c) form the coating layer of the positive electrode active material.
5. The positive electrode active material for secondary batteries according to claim 1, wherein, The positive electrode active material further includes d) Co; and e) Mn.
6. A method for manufacturing a positive electrode active material for a secondary battery, comprising: The step of generating hydroxide precursors using Ni-containing metal salts; The step of preparing the first mixture involves mixing the hydroxide precursor, lithium, and one or more compounds that independently contain elements selected from the group consisting of Al, Ti, Zr, Mg, Zn, B, Mo, Fe, Co, Ni, Ba, and W. The first mixture is calcined at 600 to 700°C for 10 to 14 hours under an O2 atmosphere to obtain the first lithium composite oxide. The step of adding one or more compounds containing elements selected from the group consisting of Al, Ti, Zr, Mg, Zn, B, Mo, Fe, Co, Ni, Ba and W, as well as a compound containing Si, to the first lithium composite oxide to prepare the second mixture; The step of calcining the second mixture at 650 to 750°C for 10 to 14 hours under an O2 atmosphere to obtain the second lithium composite oxide; The second lithium composite oxide is mixed with water at 20 to 30°C for more than 30 minutes, and then dehydrated. as well as The second lithium composite oxide, after the dehydration step, is dried by heat treatment at 250 to 350°C for more than 8 hours in an O2 atmosphere.
7. The manufacturing method according to claim 6, wherein, The metal salt further includes Co and Mn.
8. The manufacturing method according to claim 6, wherein, The step of preparing the first mixture is to mix the hydroxide precursor, lithium, and a Zr-containing compound to prepare the first mixture.
9. The manufacturing method according to claim 8, wherein, The Zr-containing compound is ZrO2, and is present in an amount of 0.1 to 0.5 mol relative to the oxide precursor.
10. The manufacturing method according to claim 6, wherein, The step of preparing the second mixture is to add a compound containing Si, a compound containing Al, a compound containing Ti, and a compound containing Zr to the first lithium composite oxide to prepare the second mixture.
11. The manufacturing method according to claim 10, wherein, The compound containing Si is 0.01 to 1.0 mol% SiO2. The compound containing Al is 0.3 to 1.0 mol% Al₂O₃. The compound containing Ti is 0.3 to 1.0 mol% TiO2. The compound containing Zr is 0.05 to 0.2 mol% ZrO2.