A supported pd catalyst, a preparation method and application thereof in a reaction of preparing styrene by hydrogenation of phenylacetylene

By preparing the UiO-66 supported Pd catalyst, the problem of poisoning of noble metal catalysts was solved, and a highly active, stable and easily separable hydrogenation reaction of phenylacetylene to styrene was achieved, which reduced production costs and provided a high-value utilization and green degradation pathway for PET.

CN123079415APending Publication Date: 2026-11-13NANKAI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510604193.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-12
Publication Date
2026-11-13

AI Technical Summary

Technical Problem

Existing precious metal catalysts are prone to poisoning in the hydrogenation of phenylacetylene to styrene, leading to decreased catalytic performance and difficulty in separation, resulting in economic losses.

Method used

A Pd catalyst supported on UiO-66 was prepared using PET as a ligand source. Palladium salt was dispersed in the pores of UiO-66 via a solvothermal reaction to form a hierarchical Pd@UiO-66 catalyst. After washing with N,N-dimethylformamide and ethanol and drying, the catalyst was used for the hydrogenation reaction of phenylacetylene.

Benefits of technology

It improves the catalyst's resistance to poisoning and stability, makes it easy to separate, and exhibits high activity and selectivity in the hydrogenation of phenylacetylene to styrene, reducing production costs and providing the possibility of green degradation of PET.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123079415A_ABST
    Figure CN123079415A_ABST
Patent Text Reader

Abstract

This invention discloses a supported Pd catalyst, its preparation method, and its application in the reaction of phenylacetylene to styrene, as well as its anti-poisoning performance. PET, zirconium chloride, and palladium salt are dispersed in a solvent and reacted solvothermically at 100-200℃ for 8-24 hours. The cooled solid is washed and dried to obtain the supported Pd catalyst. The mass ratio of zirconium chloride, PET, and palladium salt is 10-80:10-80:1. This catalyst achieves selective hydrogenation of phenylacetylene without the need for harsh high-temperature and high-pressure conditions, efficiently converting it to styrene. The conversion rate is similar to that of commonly used industrial SiO2 supports, and the unique catalyst structure avoids the problem of poisoning and deactivation common in impregnated catalysts. It exhibits excellent anti-poisoning ability in the presence of triphenylphosphine as a poison. This process not only provides a feasible pathway for PET degradation but also offers a green, sustainable, and low-cost process route for the synthesis of UiO-66. This process not only provides a feasible path for the degradation of PET, but also offers a green, sustainable, and low-cost process route for the synthesis of UiO-66.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of catalytic material preparation and styrene production technology, specifically relating to a supported Pd catalyst, its preparation method, and its application in the hydrogenation reaction of phenylacetylene to styrene. Background Technology

[0002] Pd and Ag are commonly used noble metal catalysts for the hydrogenation of phenylacetylene, and the reaction conditions are quite harsh. Furthermore, noble metal catalysts are prone to poisoning during catalytic reactions, which leads to poor catalytic performance and irreversible poisoning, resulting in significant economic losses. Modifying the catalyst can improve its resistance to poisoning. Summary of the Invention

[0003] The purpose of this invention is to overcome the shortcomings of existing technologies and provide a supported Pd catalyst, its preparation method, and its application in the hydrogenation of phenylacetylene to styrene. This catalyst exhibits high activity, high stability, and easy separation in the hydrogenation of phenylacetylene to styrene, and also possesses excellent resistance to phosphorus poisoning.

[0004] The technical solution to the problem of this invention is as follows:

[0005] The first aspect of the present invention is to provide a method for preparing a supported Pd catalyst, wherein PET, zirconium chloride and palladium salt are dispersed in a solvent and reacted solvothermally at 100-200°C for 8-24 hours, and the solid after cooling is washed and dried to obtain the supported Pd catalyst, wherein the mass ratio of zirconium chloride, PET and palladium salt is 10-80:10-80:1.

[0006] Furthermore, the mass ratio of zirconium chloride, PET, and palladium salt is 30-50:30-50:1. As a preferred embodiment, the mass ratio of zirconium chloride, PET, and palladium salt is between 42:30:1, which can further significantly improve the performance of the prepared material.

[0007] Furthermore, the palladium salt is one or more of palladium acetate, palladium sulfate, palladium chloride, and palladium nitrate.

[0008] Furthermore, the solvent is composed of solvent A and solvent B, wherein solvent A is one or more of acetone, ethanol, and isopropanol; and solvent B is one or more of formic acid, acetic acid, propionic acid, and N,N-dimethylformamide.

[0009] Further, the volume ratio of solvent A to solvent B is 1:0.5-5, preferably 1:1-3. In a preferred embodiment, acetone is used as solvent A and formic acid is used as solvent B in the mixed solvent, with a volume ratio of acetone to formic acid of 1:1.

[0010] Furthermore, the temperature of the solvothermal reaction is 140-180℃, and the reaction time is 10-18h.

[0011] Furthermore, the washing process involves sequentially washing with N,N-dimethylformamide and ethanol.

[0012] Furthermore, the drying temperature is 20-100℃, and the drying time is 6-12h, preferably 9-12h at 20-40℃.

[0013] A second aspect of the present invention is to provide a catalyst prepared by the above-described preparation method, which is a palladium salt coated with UiO-66, wherein palladium is distributed in the channels of the UiO-66 and has a hierarchical microporous structure.

[0014] A third aspect of the present invention is to provide the application of the above-described catalyst in the hydrogenation reaction of phenylacetylene to styrene. The catalyst is mixed with phenylacetylene and a solvent, and hydrogen gas is introduced at atmospheric pressure, and the reaction is carried out at 20-100°C for 1-5 hours.

[0015] UiO-66, a typical MOF material, is self-assembled from metal ions and organic ligands through coordination bonds. It possesses high specific surface area, tunable pore structure, and good chemical stability, making it a highly sought-after material in catalysis. Pd, a commonly used active component in hydrogenation catalysts, exhibits high catalytic activity and selectivity, performing well in numerous hydrogenation reactions. However, the production cost of MOFs is typically high. Terephthalic acid is the organic ligand for MOF synthesis, and it can also be obtained from the decomposition of PET. This makes industrial production of MOFs possible and solves the problem of slow degradation of PET in the natural environment, which typically takes hundreds of years to completely decompose, and the fact that traditional PET degradation often requires excessive solvents and easily causes environmental pollution. Furthermore, its unique structure offers the possibility of improving the catalyst's resistance to poisoning.

[0016] Advantages and beneficial effects of the present invention:

[0017] 1. This invention uses PET as a ligand source to prepare a UiO-66 supported Pd catalyst. The incorporation of Pd during the synthesis of the porous material significantly improves the performance and long-term operational stability of the catalytic hydrogenation of phenylacetylene to styrene. Furthermore, it exhibits excellent resistance to poisoning, and the synthesized catalyst is easily separated from the reaction solution after the reaction.

[0018] 2. This invention not only provides a new approach for the high-value utilization of PET, but also makes the green degradation of PET possible. UiO-66 also endows the catalyst with unique structure and properties. The selective hydrogenation of p-phenylacetylene to prepare styrene expands the new catalyst system and is expected to realize the low-cost industrialization of MOF materials.

[0019] 3. The preparation method of the catalyst of this invention is easy to control, requires simple equipment, and has the potential for large-scale production. The catalyst is easy to regenerate and still has good catalytic effect after recycling. Attached Figure Description

[0020] Figure 1 The XRD spectra of UiO-66, Pd / UiO-66, and Pd@UiO-66 are shown.

[0021] Figure 2 Thermogravimetric analysis (TGA) diagrams for UiO-66, Pd / UiO-66, and Pd@UiO-66 are shown.

[0022] Figure 3 The N2 adsorption-desorption curves are for UiO-66, Pd / UiO-66, and Pd@UiO-66.

[0023] Figure 4 The graph shows the change in conversion rate of styrene to be prepared by hydrogenation of phenylacetylene from UiO-66, Pd / UiO-66, Pd@UiO-66 and Pd / SiO2 over time.

[0024] Figure 5 The selectivity of styrene prepared by hydrogenation of phenylacetylene from UiO-66, Pd / UiO-66, Pd@UiO-66 and Pd / SiO2 as a function of time.

[0025] Figures 6.1-6.3 The graph shows the conversion and selectivity of UiO-66, Pd / UiO-66, Pd@UiO-66 and Pd / SiO2 in the hydrogenation of phenylacetylene to styrene using triphenylphosphine as a poison.

[0026] Figure 7 A graph showing the change in stability of styrene prepared by hydrogenation of Pd@UiO-66 phenylacetylene.

[0027] Figures 8.1-8.6 Transmission electron microscopy (TEM) images and elemental distribution maps of Pd@UiO-66.

[0028] Figures 9.1-9.6 The images show the transmission electron microscope (TEM) image and elemental distribution of Pd / UiO-66. Detailed Implementation

[0029] To more clearly illustrate the present invention, the following description, in conjunction with preferred embodiments, further clarifies the invention. Those skilled in the art should understand that the specific descriptions below are illustrative rather than restrictive, and should not be construed as limiting the scope of protection of the present invention. All equivalent changes or modifications made in accordance with the spirit and essence of the present invention should be covered within the scope of protection of the present invention.

[0030] Except for the self-made reagents used in the preparation examples below, all other reagents used in the following examples are commercially available reagents.

[0031] In the following examples, Pd@UiO-66 represents a catalyst prepared by means of Pd supported inside the pores of UiO-66 and Pd / UiO-66 represents a catalyst prepared by means of Pd supported on the surface of UiO-66, which are prepared by means of ...

[0032] Example 1: UiO-66:

[0033] Weigh 210 mg of zirconium chloride and 150 mg of PET and disperse them in a mixed solution containing 6 mL of acetone and 6 mL of formic acid. Transfer the mixture to a hydrothermal reactor and heat it in a constant temperature oven at 160 °C for 12 hours. After cooling, collect the solid and wash it sequentially with N,N-dimethylformamide and ethanol. Dry it in an oven at 30 °C and collect the resulting white solid powder, which is designated as UiO-66.

[0034] Example 2: Pd@UiO-66:

[0035] Weigh 210 mg zirconium chloride, 150 mg PET and 340 μL of 5 mg / mL PdCl2 solution and disperse them in a mixed solution containing 6 mL acetone and 6 mL formic acid. Transfer the mixture to a hydrothermal reactor and heat it in a constant temperature oven at 160 °C for 12 hours. After cooling, collect the solid and wash it with N,N-dimethylformamide and ethanol. After drying, collect the solid and label it as Pd@UiO-66.

[0036] Example 3: Pd / UiO-66:

[0037] Take the UiO-66 obtained in Example 1 above, place it in a round-bottom flask, and then disperse it in 20 mL of distilled water. After the dispersion is uniform, add 1 mL of 5 mg / mL PdCl2 solution. Stir at room temperature for 6 h, then remove water by rotary evaporation at 50 °C. The solid collected after drying is denoted as Pd / UiO-66.

[0038] Example 4: Pd / SiO2:

[0039] First, 1.00 g of activated SiO2 solid was accurately weighed using an analytical balance and transferred to a round-bottom flask. After ultrasonic treatment, it was uniformly dispersed in 20 mL of distilled water. Then, 1 mL of 5 mg / mL PdCl2 solution was added using a pipette, and the mixture was stirred at 600 rpm for 6 hours. The impregnated solution was then transferred to a rotary evaporator and concentrated by rotary evaporation at 50°C in a water bath until a semi-dry powder was obtained. Finally, it was dried in an 80°C oven for 12 hours.

[0040] Figure 1The X-ray diffraction patterns of UiO-66, Pd / UiO-66, and Pd@UiO-66 are shown. X-ray diffraction characterization and comparison with simulation cards confirm the successful synthesis of the catalyst.

[0041] Figure 2 Thermogravimetric analysis (TGA) plots of UiO-66, Pd / UiO-66, and Pd@UiO-66 are shown. UiO-66 exhibits excellent thermal stability at temperatures below 400 °C. The weight loss observed in the 30–150 °C range is attributed to the removal of adsorbed water molecules from the material surface and pores, while the weight loss in the 150–400 °C range is related to the removal of DMF molecules from the pores. When the temperature exceeds 400 °C, the weight loss indicates that the ligands are gradually decomposed or lost from the framework.

[0042] Figure 3 The N2 adsorption isotherms for UiO-66, Pd / UiO-66, and Pd@UiO-66 are shown. Compared to UiO-66, the introduction of palladium salts significantly reduces the surface area of ​​the materials. The reduction in surface area of ​​Pd@UiO-66 is due to the presence of Pd in ​​the pores of UiO-66, and the fact that Pd is encapsulated within UiO-66 during synthesis, leading to a decrease in surface area after the introduction of palladium salts. In Pd / UiO-66, the presence of Pd blocks or occupies the pores or surface of the material. This results in a larger specific surface area and exposes more active sites for contact with the feedstock, thus leading to better conversion and selectivity.

[0043] Application Examples

[0044] The prepared catalyst was reacted with phenylacetylene and ethanol solvent in a three-necked flask equipped with a condenser under continuous stirring at 30°C. Hydrogen gas was introduced at atmospheric pressure, and the reaction was carried out for 3 hours. Figure 4 The graph shows the change in conversion rate of styrene to be prepared by hydrogenation of phenylacetylene from UiO-66, Pd / UiO-66, Pd@UiO-66 and Pd / SiO2 over time. Figure 5 The selectivity for the hydrogenation of phenylacetylene to styrene using UiO-66, Pd / UiO-66, Pd@UiO-66, and Pd / SiO2 varies with time. The Pd loading is 0.5%. Figure 4 and Figure 5 It can be seen that, under the same reaction conditions, the conversion rate and selectivity of Pd@UiO-66 are similar to those of Pd / UiO-66 and Pd / SiO2.

[0045] Figures 6.1-6.3The graphs show the conversion and selectivity of UiO-66, Pd / UiO-66, Pd@UiO-66, and Pd / SiO2 in the hydrogenation of phenylacetylene to styrene using triphenylphosphine as a poison. It can be seen that Pd@UiO-66 shows the smallest change in conversion and selectivity of phenylacetylene hydrogenation after the addition of the poison, which proves that Pd@UiO-66 has the best resistance to poisoning.

[0046] from Figure 7 It can be seen that after 5 cycles of reaction, the conversion rate and selectivity of Pd@UiO-66 for the hydrogenation of phenylacetylene to styrene did not change significantly, indicating that the catalyst did not deactivate significantly.

[0047] Figures 8.1-8.6 The images show the transmission electron microscope (TEM) image and elemental distribution diagram of Pd@UiO-66. The elemental distribution diagram shows that C, O, Zr, and Pd elements are uniformly distributed in the catalyst.

[0048] Figures 9.1-9.6 The images show the transmission electron microscope (TEM) image and elemental distribution map of Pd / UiO-66. The elemental distribution map shows that C, O, Zr, and Pd are uniformly distributed in the catalyst.

[0049] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A method for preparing a Pd-supported catalyst, characterized in that, PET, zirconium chloride and palladium salt are dispersed in a solvent and reacted at 100-200℃ for 8-24 hours. After cooling, the solid is washed and dried to obtain a supported Pd catalyst. The mass ratio of zirconium chloride, PET and palladium salt is 10-80:10-80:

1.

2. The preparation method according to claim 1, characterized in that, The mass ratio of zirconium chloride, PET, and palladium salt is 30-50:30-50:

1.

3. The preparation method according to claim 1, characterized in that, The palladium salt is one or more of palladium acetate, palladium sulfate, palladium chloride, and palladium nitrate.

4. The preparation method according to claim 1, characterized in that, The solvent is composed of solvent A and solvent B, wherein solvent A is one or more of acetone, ethanol, and isopropanol; and solvent B is one or more of formic acid, acetic acid, propionic acid, and N,N-dimethylformamide.

5. The preparation method according to claim 4, characterized in that, The volume ratio of solvent A to solvent B is 1:0.5-5.

6. The preparation method according to claim 1, characterized in that, The solvothermal reaction is carried out at a temperature of 140-180℃ for 10-18 hours.

7. The preparation method according to claim 1, characterized in that, The drying temperature is 20-100℃, and the drying time is 6-12h.

8. A catalyst prepared by the preparation method according to any one of claims 1-7.

9. The use of the catalyst according to claim 8 in the hydrogenation reaction of phenylacetylene to styrene.

10. The application according to claim 9, characterized in that, The catalyst is mixed with phenylacetylene and solvent, and hydrogen gas is introduced at atmospheric pressure. The reaction is carried out at 20-100℃ for 1-5 hours.