A phase change temperature-controlled fire extinguishing microcapsule and its preparation method

By introducing confined phase change composite particles into fire extinguishing microcapsules, the problems of delayed early-stage fire extinguishing agent response and insufficient storage stability are solved by utilizing the solid-liquid phase change endothermic process of phase change materials and the interfacial adsorption effect of inorganic porous carriers, thus achieving timely response and long-term stability of fire extinguishing agents.

CN123101931APending Publication Date: 2026-11-17PEKING UNIVERSITY ZHENGZHOU INSTITUTE OF ADVANCED MATERIALS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611455124.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-18
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing fire extinguishing agents are difficult to intervene and suppress in the early stages of a fire, and it is difficult to balance stability and response sensitivity when stored at normal or medium temperatures. Conventional microencapsulation technology has the risk of response lag or leakage.

Method used

Perfluorohexanone was encapsulated using confined phase change composite particles. By introducing inorganic porous carriers and phase change materials into the microcapsule shell, heat was actively absorbed by utilizing the solid-liquid phase change endothermic process of the phase change material. Combined with interfacial adsorption and pore confinement, the mechanical and barrier properties of the shell were enhanced.

Benefits of technology

It enables timely response in the early stages of a fire and long-term storage stability, reduces the risk of leakage in non-fire conditions, and improves the response reliability and storage stability of the extinguishing agent.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123101931A_ABST
    Figure CN123101931A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of phase change materials technology and provides a phase change temperature-controlled fire extinguishing microcapsule, which has a core-shell structure containing confined phase change composite particles. The core layer is composed of perfluorohexanone and hydrophobic confined phase change composite particles, while the shell layer is composed of a thermosetting resin precursor and amphiphilic confined phase change composite particles. The confined phase change composite particles consist of an inorganic porous carrier and a phase change component loaded in the pores. The advantages of this invention are that the phase change component itself has solid-liquid phase change endothermic properties, absorbing heat when heated, providing a thermal buffer for perfluorohexanone; the inorganic porous carrier improves the loading stability and leakage prevention of the phase change component through interfacial adsorption and pore confinement, inhibits its migration, and enhances the mechanical and barrier properties of the shell layer, thereby reducing perfluorohexanone vaporization leakage under unexpected temperature rises and improving the storage stability and thermal response reliability of the microcapsule.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of phase change materials technology, and in particular to a phase change temperature-controlled fire extinguishing microcapsule and its preparation method. Background Technology

[0002] Perfluorohexanone possesses insulating properties, high volatility, no residue, easy photodegradation, and zero ozone depletion, making it considered a major alternative to halon fire extinguishing agents. Existing conventional fire extinguishing agents, including dry powder, carbon dioxide, and aerosol agents, can only extinguish open flames formed after thermal runaway has occurred. They are insufficient to intervene and inhibit the early stages of the thermal runaway reaction. Furthermore, none of these conventional fire extinguishing agents possess the dual efficacy of extinguishing and cooling, posing a high risk of reignition in fire scenarios.

[0003] Compared to conventional fire extinguishing agents, perfluorohexanone (PFH) can simultaneously achieve both fire extinguishing and cooling effects. Its fire extinguishing efficiency is achieved through a synergistic mechanism of chemical inhibition and physical asphyxiation. Specifically, when the temperature of the protected area rises, some chemical bonds in the PPH molecule break, allowing it to combine with active free radicals generated by the flame, thereby blocking the combustion chain reaction. Simultaneously, its insulating properties prevent it from causing short-circuit damage to electrical equipment. Furthermore, after vaporization, PPH can diffuse and cover the protected area, disrupting combustion conditions by isolating oxygen and thus inhibiting reignition. However, PPH itself has certain physical limitations. Its boiling point at normal pressure is approximately 49.2°C, and its vapor pressure at room temperature is relatively high, exhibiting strong volatility. These limitations restrict its storage stability and long-term protective performance in various application scenarios.

[0004] Encapsulating perfluorohexanone (PFH) within a polymer shell to form microcapsules, enabling the encapsulation and temperature-responsive release of the extinguishing agent, has become one of the main technological pathways for expanding its application scenarios. Among existing extinguishing microcapsule technologies, one approach focuses on designing a two- or more-layer polymer shell encapsulation structure. This involves constructing a composite shell system and densifying it to enhance shell strength and molecular barrier properties, thereby suppressing the vaporization and leakage of PPH at room temperature or intermediate temperatures (49℃~90℃). For example, CN116832387A discloses a double-shell-encapsulated PPH extinguishing microcapsule and its room-temperature preparation method, using PPH as the core material, with the inner shell wall made of β-cyclodextrin and the outer shell wall made of polyurea. However, excessive densification of the shell in this type of scheme can lead to a significant increase in the rupture and release temperature of the microcapsules, causing the extinguishing agent to respond lagably in some real fire scenarios and making it difficult to activate the extinguishing agent in time in the early stages of a fire. On the other hand, although the single-layer thin-walled structure can ensure trigger sensitivity, it will significantly weaken the long-term storage stability and is prone to premature leakage in normal temperature rise scenarios under non-fire conditions.

[0005] Another approach focuses on modifying the shell material, introducing functional fillers such as inorganic minerals and thickeners into the polymer shell to enhance its mechanical and barrier properties. For example, CN118649393A discloses a fire extinguishing microcapsule whose inner shell is coated with a natural polymer and whose outer shell is made of polyisocyanate / phenolic resin. The multi-material composite structure used in the inner shell helps improve the mechanical, barrier, and stability properties of the capsule wall. However, the fillers added in this type of approach are mostly inert phases, which can only delay the leakage of the capsule core through physical barrier effects. They cannot actively absorb heat energy from the heat conduction path or regulate the temperature rise of the capsule core, thus making it difficult to delay the vaporization and pressurization process of the extinguishing agent.

[0006] It is evident that existing technologies are still insufficient to simultaneously meet the comprehensive requirements of long-term storage stability, long-lasting functionality, and precise response and release. Summary of the Invention

[0007] The purpose of this invention is to overcome the shortcomings of the prior art and provide a phase change temperature-controlled fire extinguishing microcapsule and its preparation method. By using confined phase change materials, the mechanical properties and barrier properties of the microcapsule shell are enhanced. At the same time, the inorganic porous carrier is used to adsorb the phase change components at the interface and confine them through the pores. When heated, the phase change components actively absorb heat from the core layer through the solid-liquid phase change endothermic process, which effectively delays the rise in core layer temperature and the subsequent internal pressure accumulation and vaporization process. This significantly reduces the risk of premature leakage of the core layer under non-fire conditions and improves the storage stability and response reliability of the fire extinguishing microcapsule during long-term service.

[0008] The present invention is achieved through the following technical solution: On the one hand, a phase change temperature-controlled fire extinguishing microcapsule is provided, wherein the microcapsule has a core-shell structure containing confined phase change composite particles; The confined phase change composite particles include hydrophobic confined phase change composite particles and amphiphilic confined phase change composite particles. The core layer of the core-shell structure is composed of perfluorohexanone and the hydrophobic confined phase transition composite particles; The shell of the core-shell structure is composed of a thermosetting resin precursor and the amphiphilic confined phase change composite particles. The average particle size of the microcapsules is 5 μm to 500 μm.

[0009] Through the above technical solution, confined phase change composite particles are encapsulated in microcapsules. When heat is transferred to the microcapsules, the phase change material reduces the heat transferred to the core layer through solid-liquid phase change endothermic reaction, thereby slowing down the temperature rise rate of the core material and the accumulation of vaporization internal pressure. The surface of the hydrophobic confined phase change composite particles is moderately hydrophobically treated, so that after the addition of a dispersed oil phase containing perfluorohexanone, it tends to remain inside the oil droplets rather than enter the continuous aqueous phase, thus ensuring the effective retention and uniform dispersion of the phase change temperature control unit in the core layer. The outer surface of the amphiphilic confined phase change composite particles has a moderate hydrophilic / lipophilic balance, while retaining reactive groups such as hydroxyl and amino groups, so that it preferentially adsorbs at the oil-water interface after emulsification, and is then embedded in the shell layer during polyurea interface polymerization or melamine / phenolic resin deposition, achieving stable anchoring and structural reinforcement of the composite particles in the shell layer.

[0010] Furthermore, both the hydrophobic confined phase change composite particles and the amphiphilic confined phase change composite particles comprise organic phase change materials and inorganic porous carriers, and the mass ratio of organic phase change materials to inorganic porous carriers is 1~3:9~2.

[0011] Through the above technical solution, phase change materials (PCMs) are loaded into the pores of a surface-modified inorganic porous carrier to form confined PCM composite particles. The surface modification treatment can adjust the wettability of the pore surface. In the confined PCM composite particles, the inorganic carrier, with its rigid framework structure and high specific surface area, applies capillary confinement and interfacial adsorption to the loaded PCMs, making it less prone to macroscopic flow and precipitation of the PCMs during solid-liquid phase transitions. After introducing the confined PCM composite particles into the core-shell structure of microcapsules, the inorganic carrier can simultaneously perform dual functions: firstly, as a physical reinforcing component, it improves the compressive strength and molecular barrier density of the polymer shell; secondly, as a thermal buffer unit, it actively absorbs heat when the ambient temperature rises, utilizing the latent heat absorption capacity of the PCMs. The synergistic effect of these two functions enables the microcapsules to achieve active temperature rise suppression while maintaining the integrity of the shell structure.

[0012] Furthermore, the organic phase change material is selected from any one of fatty alcohols, fatty acids, and polyethylene glycol; wherein the fatty alcohol is C 14 ~C 24 Saturated fatty alcohols, with fatty acid C 12 ~C 24 The number average molecular weight of the saturated fatty acid and polyethylene glycol is 1000~20000; the phase change temperature range of the organic phase change material is 45~90℃; and the latent heat of phase change of the organic phase change material is not less than 150J / g.

[0013] Through the above technical solutions, the aforementioned substances are all long-chain organic compounds with polar end groups (hydroxyl or carboxyl groups). These polar groups can form hydrogen bonds with the silanol and aluminol groups on the surface of the inorganic porous carrier, thereby achieving good wettability and interfacial bonding during impregnation, ensuring that the phase change material does not easily undergo phase separation after loading. The phase change temperature range is set at 45~90℃, precisely covering the critical temperature rise range of perfluorohexanone (boiling point approximately 49.2℃) above room temperature storage and below fire triggering. When the ambient temperature slowly rises to this range, the phase change material first undergoes a solid-liquid phase change to absorb heat, rather than directly vaporizing and pressurizing the perfluorohexanone. The requirement of a latent heat of phase change of not less than 150J / g ensures that each unit mass of phase change material possesses sufficient heat absorption capacity.

[0014] Furthermore, the hydrophobic confined phase change composite particles are prepared by surface modification of an inorganic porous carrier with a hydrophobic modifier; wherein the hydrophobic modifier is selected from one or more of hexamethyldisilazane, methyltrimethoxysilane, methyltriethoxysilane, and C3-C8 alkyltrialkoxysilane. And / or, the amphiphilic confined phase change composite particles are prepared by surface modification of an inorganic porous carrier with aminosilane and C3-C8 alkyltrialkoxysilane; wherein the molar ratio of aminosilane to C3-C8 alkyltrialkoxysilane is 1:3 to 3:1. And / or, the inorganic porous carrier is selected from any one of vermiculite, mesoporous silica, silica aerogel or halloysite.

[0015] Through the above technical solution, the organic phase change material is loaded into the pores of a modified inorganic porous carrier. The surface modification treatment employs at least one of hexamethyldisilazane, methyltrimethoxysilane, methyltriethoxysilane, C3-C8 alkyltrialkoxysilane, and aminosilane to adjust the wettability of the inorganic porous carrier's pore surface. The inorganic porous carrier is an electrically insulating silicate or silica-based porous material with abundant nano / submicron pore structures, including interlayer domains, mesoporous channels, hollow cavities, or three-dimensional network pores. During vacuum impregnation, the pores draw in the molten phase change material through capillary force and fix it inside the carrier. After loading, the pore space exerts a confinement effect on the phase change material, restricting its molecular chain movement and macroscopic flow, making it less prone to leakage, seepage, or phase separation during repeated solid-liquid phase change cycles, thereby maintaining the structural integrity of the composite particles and the long-term stability of the latent heat of phase change. Furthermore, the rigid framework structure of the carrier itself provides physical support within the microcapsule shell without adversely affecting the fire-extinguishing release performance of perfluorohexanone. Simultaneously, the carrier's electrical insulation properties ensure the safety of the microcapsules in electrical equipment fire protection scenarios, preventing short-circuit risks caused by the carrier's conductivity.

[0016] Furthermore, the raw materials for preparing the microcapsules, based on 100 parts by weight of perfluorohexanone, include: Thermosetting shell precursor: 5-50 parts; Emulsifier: 0.5~10 parts; Hydrophobic confined phase change composite particles: 1~10 parts; Hydrophilic confined phase change composite particles: 1~10 parts; Crosslinking agent: 0~20 parts; Fluorinated ether cosolvent: 0~100 parts; Deionized water: 200-600 parts; Through the above technical solutions, perfluorohexanone, as a low-boiling-point solvent, requires the use of fluorinated ether co-solvents to adjust the polarity and viscosity of the oil phase, ensuring uniform dissolution of polymer monomers in the oil phase and reducing the oil-water interfacial tension; the amount of emulsifier above the critical micelle concentration provides sufficient interfacial coverage to maintain the kinetic stability of emulsion droplets during the polymerization reaction; the ratio of polymer monomers to crosslinking agents determines the shell crosslinking density and mechanical strength, if it is too low, the shell strength will be insufficient, and if it is too high, the shell brittleness will increase; the inorganic confined phase change composite particles, while ensuring the thermal buffering function, do not affect the emulsion stability and shell continuity in terms of solid phase content.

[0017] A method for preparing the above-mentioned phase change temperature-controlled fire extinguishing microcapsule is also provided, comprising the following steps: Step S1: Add perfluorohexanone, fluoroether co-solvent and hydrophobic confined phase change composite particles into a sealed container, stir and mix evenly to form an oil phase suspension, and keep it in the dark and warm for later use. Step S2: Add the emulsifier and amphiphilic confined phase change composite particles to deionized water, heat to 20~40℃, and stir until the emulsifier is completely dissolved to obtain an aqueous dispersion. Step S3: The oil phase suspension obtained in step S1 is slowly added dropwise to the aqueous phase dispersion obtained in step S2 and shear emulsified to form an oil-in-water emulsion; Step S4: Add thermosetting resin precursor and crosslinking agent to the oil-in-water emulsion obtained in step S3, so that the thermosetting resin precursor undergoes a polymerization reaction at the oil-water interface to form a shell layer, and at the same time, the confined phase change composite particles are embedded in the shell layer and the core layer; after curing, washing and low-temperature drying, the phase change temperature-controlled fire extinguishing microcapsules are obtained.

[0018] Through the above technical solution, this invention is based on a preparation strategy of modification, loading, and post-coating. First, molten phase change material is forcibly pressed into the depths of the pores of a modified inorganic porous carrier under negative pressure through vacuum impregnation, achieving a high filling rate loading of the phase change material. This step is the material basis for endowing the final microcapsules with thermal buffering function. Then, the loaded composite particles are co-dispersed with perfluorohexanone in the oil phase through an emulsification process to form emulsion droplets containing functional particles. In the interfacial polymerization reaction, the polymer monomers undergo condensation at the oil-water interface, gradually forming a continuous shell. At the same time, the polar groups (hydroxyl or carboxyl groups) carried on the surface of the composite particles undergo chemical bonding (forming urethane covalent bonds with polyisocyanate systems) or strong physical interactions (forming multiple hydrogen bonds with phenolic / melamine systems) with the polymer monomers or crosslinking agents, so that the composite particles are anchored in situ in the polymer network during the shell formation process, rather than simple physical doping. This synchronous anchoring mechanism effectively avoids the debonding of particles from the shell during subsequent use, ensuring the long-term stability of the structure.

[0019] Furthermore, the emulsifier is selected from one or more of sodium dodecyl sulfate, sodium dodecyl sulfonate, Tween-80, gum arabic, and PVA.

[0020] And / or, in step S3, the emulsification speed is 200 rpm to 5000 rpm, and the emulsification time is 2 min to 30 min; And / or, in step S4, the polymerization reaction temperature is 20℃~45℃, and the reaction time is 1h~5h.

[0021] The above technical solutions utilize emulsifiers of both anionic and nonionic types. Anionic emulsifiers include sodium dodecyl sulfate and sodium dodecyl sulfonate, which maintain the emulsion's anti-agglomeration stability during polymerization by adsorbing onto the oil-water interface and imparting a negative charge to the droplet surface, thus employing electrostatic repulsion. Nonionic emulsifiers include Tween-80, gum arabic, and PVA, which stabilize the emulsion through the steric hindrance effect of long-chain molecules at the interface. PVA and gum arabic also have thickening effects, increasing the viscosity of the continuous aqueous phase and effectively inhibiting the settling rate of inorganic composite particles with a density greater than water during emulsion settling. The combined use of these two types of emulsifiers creates a synergistic effect between electrostatic and steric hindrance stability, significantly expanding the pH and temperature range for emulsion stability.

[0022] Furthermore, in step S1, the preparation process of the hydrophobic confined phase change composite particles is as follows: Step 1: The inorganic porous carrier is surface modified with a hydrophobic modifier to obtain a modified inorganic porous carrier, wherein the amount of hydrophobic modifier added is 1% to 15% of the mass of the inorganic porous carrier; Step 2: Place the hydrophobic modified inorganic porous carrier obtained in Step 1 in a forced-air drying oven and dry it at 100℃~120℃ for 1h~2h. Step 3: Heat the organic phase change material to a temperature 10°C to 20°C above its phase change point to melt it, and stir it under heat preservation conditions until it is completely melted to obtain a homogeneous and clear liquid phase system; Step 4: Place the dried hydrophobic modified inorganic porous carrier obtained in Step 2 into a vacuum reaction apparatus and preheat the vacuum reaction apparatus to 10°C~20°C higher than the phase change temperature of the phase change material. Then add molten organic phase change material to it and vacuum impregnate it for 1h~2h under heat preservation conditions. Cool the impregnated mixture to room temperature to allow the phase change material to solidify inside the modified inorganic porous carrier, thus obtaining hydrophobic confined phase change composite particles.

[0023] The above technical solution involves first heating the phase change material to 10°C-20°C above its phase change point, minimizing its viscosity and completely melting it into a homogeneous liquid phase to ensure its fluidity during subsequent impregnation. Simultaneously, the inorganic porous carrier is dried at 100°C-120°C for 1-2 hours to thoroughly remove physically adsorbed water molecules and residual air from the pores. The presence of moisture hinders the entry of the phase change material into the nanopores due to surface tension, while residual air is extracted under vacuum conditions, creating a negative pressure driving force. The dried carrier is placed in a vacuum reaction apparatus and preheated to 10°C-20°C above its phase change temperature. This prevents the molten phase change material from solidifying upon cooling and blocking the pore inlets, and also ensures the carrier itself is in thermal equilibrium, facilitating the uniform spreading of the liquid phase change material. Impregnation under vacuum conditions for 1-2 hours further expels residual gas from the pores due to the negative pressure, while the molten phase change material is drawn into the depths of the pores under the dual driving force of pressure difference and capillary force. Finally, the cooling process to room temperature allows the phase change material to slowly crystallize and solidify within a confined space, forming stable, shaped composite particles.

[0024] Further, in step S1, the preparation process of the amphiphilic confined phase change composite particles is as follows: Step 1: The inorganic porous carrier is surface modified by an amphiphilic polymer, that is, aminosilane and C3-C8 alkyltrialkoxysilane are prepared into a composite modifier in a molar ratio of 1:3 to 3:1, and the inorganic porous carrier is surface modified by the composite modifier to obtain an amphiphilic inorganic porous carrier. Step 2: Place the modified inorganic porous carrier obtained in Step 1 in a forced-air drying oven and dry it at 100℃~120℃ for 1h~2h. Step 3: Heat the organic phase change material to a temperature 10°C to 20°C above its phase change point to melt it, and stir it under heat preservation conditions until it is completely melted to obtain a homogeneous and clear liquid phase system; Step 4: Place the dried modified inorganic porous carrier obtained in Step 2 into a vacuum reaction apparatus and preheat the vacuum reaction apparatus to 10°C~20°C higher than the phase change temperature of the phase change material. Then add molten organic phase change material to it and vacuum impregnate it for 1h~2h under heat preservation conditions. Cool the impregnated mixture to room temperature to allow the phase change material to solidify inside the modified inorganic porous carrier, thus obtaining amphiphilic confined phase change composite particles.

[0025] The above technical solution utilizes a pre-loading, post-coating preparation strategy for confined phase change composite particles. First, molten phase change material is impregnated under negative pressure through vacuum impregnation into the pores of a surface-modified inorganic porous carrier, forming highly filled confined phase change composite particles upon cooling, providing thermal buffering for the microcapsules. Subsequently, the hydrophobic confined phase change composite particles are dispersed in an oil phase containing perfluorohexanone to form an oil-phase suspension; the amphiphilic confined phase change composite particles are dispersed in an aqueous phase and emulsified to form an oil-in-water emulsion. During interfacial polymerization, in-situ polycondensation, or resin deposition, amphiphilic confined phase change composite particles, with their suitable hydrophilic / lipophilic balance and the reactive groups such as hydroxyl and amino groups retained on their surface, adsorb onto the oil-water interface and undergo chemical bonding (e.g., reacting with polyisocyanates to form urethane or urea bonds) or physical interactions (e.g., forming multiple hydrogen bonds with phenolic / melamine resin systems) with polymer monomers or crosslinking agents. This allows them to be in-situ anchored within the polymer network during shell formation. Meanwhile, hydrophobic confined phase change composite particles remain stably within the oil droplets, effectively preserving the phase change temperature control unit within the core layer. This simultaneous anchoring mechanism creates a chemical or strong physical bond between the composite particles and the shell, effectively preventing interfacial debonding during subsequent use and ensuring the long-term stability of the microcapsule structure.

[0026] Furthermore, the thermosetting resin precursor is selected from at least one of polyisocyanate compounds, phenolic resin prepolymers, and melamine-formaldehyde resin prepolymers.

[0027] Through the above technical solutions, when polyisocyanates and water-soluble amine compounds are used as wall material precursors, they undergo interfacial condensation polymerization at the oil-water interface to generate a polyurea shell. This reaction can proceed rapidly at room temperature to medium temperature, and the resulting polyurea shell exhibits high mechanical strength and thermal stability. During this process, the reactive groups such as hydroxyl and amino groups retained on the surface of the amphiphilic confined phase change composite particles at the oil-water interface can react with trace amounts of isocyanate groups to form urethane bonds or urea bonds, thereby anchoring the composite particles in the polyurea shell in a covalent manner. When phenolic resin prepolymers or melamine-formaldehyde resin prepolymers are used as wall material precursors, they undergo in-situ condensation polymerization and deposition on the surface of oil droplets under acid catalysis to form a thermosetting resin shell. At this time, multiple hydrogen bonds are formed between the polar groups such as hydroxyl and amino groups on the surface of the composite particles and the polar groups such as hydroxymethyl and imino groups in the resin, achieving a strong physical embedding. Both of the above-mentioned shell formation paths can achieve in-situ anchoring and thermal buffering of confined phase change composite particles within the framework of the present invention, and do not depend on the specific chemical composition of the wall material, thus exhibiting good process adaptability and wide industrial applicability.

[0028] Beneficial effects This invention forms confined phase change composite particles by loading phase change material (PCM) into the nanopores of a modified inorganic porous carrier, and then embedding these particles in the polymer shell of a microcapsule and / or dispersing them in the core layer. When the ambient temperature rises to the PCM temperature range, the PCM absorbs latent heat through a solid-liquid phase change process, reducing the effective heat transferred to the perfluorohexanone core material and slowing down the temperature rise rate and internal pressure accumulation process of the core material.

[0029] The inorganic porous carrier used in this invention possesses a rigid framework structure and a high specific surface area. When embedded in a polymer shell, it serves two purposes: firstly, as a physical reinforcing component, it enhances the shell's compressive strength and fracture resistance; secondly, the layered or porous structure of the inorganic carrier extends the diffusion path of gas molecules, strengthening the shell's molecular barrier properties against perfluorohexanone. Simultaneously, the low thermal conductivity of the inorganic carrier itself forms an additional thermal resistance layer in the heat conduction path, further reducing the net heat flux into the core layer.

[0030] The phase change materials selected in this invention all have polar end groups. On the one hand, they form hydrogen bonds with the silanol and aluminol on the surface of the inorganic porous carrier, ensuring that the phase change material is not prone to phase separation after loading. On the other hand, during the interfacial polymerization reaction, the polar groups on the surface of the composite particles can chemically bond or strongly physically interact with the polymer monomers or crosslinking agents, so that the composite particles are anchored in situ in the polymer network during the shell forming process. Attached Figure Description

[0031] Figure 1This is a schematic diagram of the core-shell structure of the phase change temperature-controlled fire extinguishing microcapsule of the present invention.

[0032] Figure 2 An optical microscope image of the phase change temperature-controlled fire extinguishing microcapsule prepared in Example 1 of this invention.

[0033] Figure 3 Scanning electron microscope (SEM) image of the phase change temperature-controlled fire extinguishing microcapsule prepared in Example 1 of the present invention.

[0034] Figure 4 Thermogravimetric analysis (TGA) curve of the phase change temperature-controlled fire extinguishing microcapsule prepared in Example 1 of the present invention.

[0035] Figure 5 Differential scanning calorimetry (DSC) curve of the phase change temperature-controlled fire extinguishing microcapsule prepared in Example 1 of the present invention.

[0036] Figure 6 Scanning electron microscope (SEM) image of the phase change temperature-controlled fire extinguishing microcapsule prepared in Example 2 of the present invention.

[0037] Figure 1 In the diagram, 1-confined phase transition composite particles; 2-shell; 3-core. Detailed Implementation

[0038] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to specific embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.

[0039] Based on the embodiments of this invention, all other embodiments obtained by those skilled in the art without inventive effort are within the scope of protection of this invention. Experimental methods in the following embodiments that do not specify specific conditions are generally performed under conventional conditions or as recommended by the manufacturer. Unless otherwise stated, all percentages, ratios, proportions, or parts are by weight.

[0040] Unless otherwise specified, the reagents and raw materials used in the embodiments and comparative examples of this invention are commercially available.

[0041] The phase change material is selected from any one of fatty alcohols, fatty acids, and polyethylene glycol; the fatty alcohol is C 14 ~C 24 Saturated fatty alcohols, wherein the fatty acid is C 12 ~C 24 The polyethylene glycol contains saturated fatty acids and has a number-average molecular weight of 1,000 to 20,000. The phase change temperature range of the phase change material is 45 to 90°C, and the latent heat of phase change of the phase change material is not less than 150 J / g.

[0042] The inorganic porous carrier is selected from at least one of the following components: vermiculite with an interlayer structure; mesoporous silica with a mesoporous channel structure; silica aerogel with a porous structure; halloysite with a hollow lumen structure. Surface modification treatment is performed using at least one of methylsilane, hexamethyldisilazane, C3-C8 alkylsilane, and aminosilane to adjust the surface wettability of the inorganic porous carrier's pores.

[0043] The fluoroether cosolvent is selected from methyl nonafluorobutyl ether; The thermosetting resin precursor is selected from at least one of polyisocyanates, phenolic resin prepolymers, and melamine-formaldehyde resin prepolymers; The crosslinking agent is selected from one or more of water-soluble amine compounds, isocyanates, and aldehydes.

[0044] The emulsifier is selected from one or more of sodium dodecyl sulfate, sodium dodecyl sulfonate, Tween-80, gum arabic, and PVA.

[0045] Example 1 A method for preparing the above-mentioned phase change temperature-controlled fire extinguishing microcapsule includes the following steps: S1. Preparation of confined phase change composite particles; (1) Preparation of hydrophobic confined phase change composite particles; Halloysite was dried at 120°C for 2 hours.

[0046] Weigh out octyltriethoxysilane and halloysite at a mass ratio of 1:10. Add octyltriethoxysilane to a mixed solution of ethanol / water at a volume ratio of 9:1. Adjust the pH to 4.5-5.0 with glacial acetic acid and pre-hydrolyze at room temperature for 30 min.

[0047] Then, dried halloysite was added, and the reaction was carried out at 60°C and 400 rpm for 4 hours. After the reaction was completed, the mixture was filtered, washed three times with anhydrous ethanol, and dried at 110°C for 2 hours to obtain hydrophobically modified halloysite.

[0048] The raw materials were weighed at a mass ratio of 6:4 for octadecyl alcohol and hydrophobically modified halloysite. The octadecyl alcohol was placed in a constant-temperature container and heated to 70°C to melt it. The mixture was kept at this temperature and stirred until completely melted into a homogeneous, clear liquid, which was then kept at this temperature for later use. The hydrophobically modified halloysite was placed in a forced-air drying oven and dried at 110°C for 1.5 hours to completely remove adsorbed water and residual air from the pores of the carrier. The dried hydrophobically modified halloysite was added to a vacuum reaction apparatus and preheated to 70°C. Molten octadecyl alcohol was then added, and the mixture was vacuum impregnated for 2.5 hours under maintaining the temperature, allowing the liquid octadecyl alcohol to enter the hollow cavity of the halloysite under negative pressure, capillary action, and pore adsorption. The impregnated mixture was cooled to room temperature, allowing the octadecyl alcohol to solidify inside the halloysite, yielding hydrophobically confined phase change composite particles.

[0049] (2) Preparation of amphiphilic confined phase change composite particles Halloysite was dried at 120°C for 2 hours.

[0050] A composite modifier is formed by mixing 3-aminopropyltriethoxysilane and octyltriethoxysilane at a molar ratio of 2:1, wherein the total mass of the composite modifier is 10% of the mass of halloysite.

[0051] The composite modifier was added to a mixed solution of ethanol / water at a volume ratio of 9:1, the pH was adjusted to 4.5-5.0 with glacial acetic acid, and pre-hydrolyzed at room temperature for 30 min. Then halloysite was added, and the reaction was carried out at 60℃ and 400 rpm for 4 h.

[0052] After the reaction was completed, the mixture was filtered, washed three times with anhydrous ethanol, and dried at 110°C for 2 hours to obtain amphiphilic modified halloysite with both amino and alkyl groups on its surface.

[0053] Vacuum impregnation was performed with octadecyl alcohol and amphiphilic modified halloysite at a mass ratio of 40:60, under the same vacuum impregnation conditions as the above-mentioned hydrophobic confined phase change composite particles, to obtain amphiphilic confined phase change composite particles.

[0054] S2. Preparation of phase change temperature-controlled shell fire extinguishing microcapsules The raw material ratio, based on 100 parts by weight of perfluorohexanone, includes 100 parts of perfluorohexanone; 100 parts of methyl nonafluorobutyl ether; 20 parts of isophorone diisocyanate; 5 parts of diethylenetriamine; 6 parts of hydrophobic confined phase change composite particles; 2 parts of amphiphilic confined phase change composite particles; 3 parts of sodium dodecyl sulfate; and 500 parts of deionized water.

[0055] Preparation of oil phase suspension: At room temperature, add perfluorohexanone, methyl nonafluorobutyl ether, and hydrophobic confined phase change composite particles into a sealed container, stir at 400 rpm for 30 min, mix until a homogeneous and transparent oil phase solution is obtained, and keep it in the dark and warm for later use.

[0056] Preparation of aqueous dispersion: Sodium dodecyl sulfate and amphiphilic confined phase change composite particles are added to deionized water, heated to 35°C, and stirred until the emulsifier is completely dissolved to obtain an aqueous dispersion.

[0057] Emulsification and molding: The oil phase suspension is slowly added dropwise to the aqueous phase dispersion. After the addition is complete, the mixture is sheared and emulsified at 600 rpm for 30 minutes to form an oil-in-water emulsion.

[0058] Shell formation reaction: The obtained emulsion was transferred to a temperature-controlled jacketed reactor. Isophorone diisocyanate was added at room temperature and with low stirring at 400 rpm for 15 min. Then, diethylenetriamine was added dropwise, and the reaction was maintained at this temperature with stirring for 30 min after the addition was complete. Subsequently, the system was heated to 30°C and the reaction was maintained at this temperature with stirring for 3 h to promote complete polymerization. During the reaction, the confined phase change composite particles were embedded in the shell and core layers.

[0059] Post-processing: After the reaction was completed, the product was allowed to stand and precipitate, and then filtered and washed with deionized water four times to remove impurities remaining on the surface of the microcapsules; then dried at 35℃ for 12 hours to obtain the phase change temperature-controlled fire extinguishing microcapsule product.

[0060] The detection conditions were as follows: the morphology and particle size distribution of the microcapsules were observed using an optical microscope and a scanning electron microscope.

[0061] Thermogravimetric analysis (TGA) was used to heat the microcapsules from room temperature to 600°C at a heating rate of 10°C / min under a nitrogen atmosphere to determine the thermogravimetric behavior. The encapsulation rate was calculated based on the weight loss steps of the core material perfluorohexanone, and the shell rupture release temperature was determined to characterize the microcapsules with significant weight loss initiation temperature.

[0062] The phase transition temperature and latent heat of phase transition of the microcapsules were determined by heating them from 25°C to 90°C at a heating rate of 5°C / min under a nitrogen atmosphere using differential scanning calorimetry (DSC).

[0063] Long-term stability test: After storing the microcapsule samples in an 80℃ constant temperature oven for 100 hours, the samples were weighed and the thermal weight loss rate was calculated.

[0064] After testing, such as Figure 1 As shown, the phase change temperature-controlled fire extinguishing microcapsules of the present invention exhibit a regular core-shell spherical structure with an average particle size of approximately 200 μm. The core layer 3 is perfluorohexanone, the shell layer 2 is a thermosetting resin precursor, and the confined phase change composite particles 1 are distributed in the shell layer 2 and / or the core layer 3.

[0065] like Figure 2 As shown in the optical microscope images, the overall morphology and particle size distribution of the microcapsules prepared in Example 1 are clearly displayed. Numerous well-defined spherical particles are visible in the images, exhibiting good dispersibility without obvious agglomeration or breakage.

[0066] Combination Figure 3 As shown in the scanning electron microscope (SEM) images, the surface morphology and shell structure of the microcapsules of Example 1 are displayed at a higher magnification. The images reveal that the microcapsule surfaces are relatively smooth and dense, with continuous and intact shells, free of obvious cracks or pores. Some microcapsules exhibit slight surface indentations, which are attributed to volume shrinkage during shell solidification, but no signs of shell rupture or core material leakage were observed. No free halloysite / octadecyl alcohol composite particles were found exposed on the shell surface, indicating that the composite particles are effectively embedded within the shell or core.

[0067] Combination Figure 4 As shown, the TGA curve records the thermogravimetric behavior of the microcapsules of Example 1 during the heating process from room temperature to 600°C under a nitrogen atmosphere. The curve can be clearly distinguished into two main weight loss steps: The first weight loss step (100~200℃): corresponds to the vaporization and overflow of the perfluorohexanone core material. The weight loss ratio at this step is approximately 60%, based on which the coverage rate is calculated to be 60%. The initial temperature drop point at this step is 112℃, which is further defined as the shell rupture and release temperature, representing the characteristic temperature at which the shell begins to fail under thermal action and the core material begins to release.

[0068] The second weight loss stage (300~450℃): corresponds to the thermal decomposition of the polyurea shell, with a weight loss ratio of approximately 23%.

[0069] The intermediate section (200~300℃) exhibits a slow weight loss of 17%, attributed to the thermal weight loss of the octadecyl alcohol phase change material within the halloysite nanotubes. After being loaded into the halloysite nanotubes, the thermal decomposition behavior of octadecyl alcohol is influenced by the pore confinement effect, resulting in a wider temperature loss range rather than a sharp weight loss step. Therefore, TGA testing shows that the core material contains 60% perfluorohexanone, with a 60% coating rate; the rupture release temperature is 112℃. This further demonstrates that this embodiment not only exceeds the boiling point of perfluorohexanone and the phase change temperature of the phase change material, avoiding premature leakage under normal / medium temperature conditions, but also falls below the rupture temperature of traditional double-layered dense shells, ensuring timely response in fire scenarios. This curve verifies that the introduction of inorganic confined phase change composite particles did not significantly increase the rupture release temperature of the shell, achieving enhanced thermal buffering without sacrificing response sensitivity.

[0070] like Figure 5As shown, the DSC curves recorded the heat flow changes of the microcapsules of Example 1 during the heating process from 25°C to 90°C. A distinct upward endothermic peak appeared at 48°C, corresponding to the solid-liquid phase transition endothermic process of octadecyl alcohol loaded within halloysite nanotubes. The latent heat of phase transition was 18.2 J / g, and the phase transition temperature was 48°C. Compared with the theoretical phase transition temperature of 55°C and the theoretical latent heat of phase transition of 240 J / g of pure octadecyl alcohol, the octadecyl alcohol loaded within halloysite nanotubes exhibited two significant changes: The phase transition temperature decreased by 7°C, from 55°C to 48°C, which is attributed to the nanoscale spatial confinement effect of the halloysite hollow cavity diameter of 10–190 nm on the octadecyl alcohol molecules. Within the nanoscale confined space, the degrees of freedom of movement and crystal orientation of the octadecyl alcohol molecules are restricted by the pore walls, leading to changes in crystallization kinetics, manifested as a decrease in phase transition temperature and a broadening of the phase transition peak.

[0071] The apparent latent heat of phase change decreased from 240 J / g in the pure state to 18.2 J / g in the composite particles. This value represents the latent heat of phase change of the entire microcapsule sample, which is sufficient to play a thermal buffering role in practical applications, ensuring that its core thermal buffering function remains unaffected.

[0072] Long-term stability test results show that after storage at 80℃ for 100 hours, the thermal weight loss of the microcapsules is less than 10%, and the core material retention rate is good.

[0073] Example 2 A method for preparing a phase change temperature-controlled fire extinguishing microcapsule includes the following steps: S1. Preparation of confined phase change composite particles; (1) Preparation of hydrophobic confined phase change composite particles; The vermiculite powder was dried at 120℃ for 2 hours.

[0074] Vermiculite was hydrophobically modified using methyltriethoxysilane, wherein the amount of methyltriethoxysilane used was 12% of the mass of vermiculite.

[0075] After modification, palmitic acid was melted at 80°C and mixed with hydrophobically modified vermiculite at a mass ratio of 60:40. The mixture was then vacuum impregnated at 80°C for 1 hour to obtain hydrophobically confined phase change composite particles.

[0076] (2) Preparation of amphiphilic confined phase change composite particles A composite modifier was prepared by using 3-aminopropyltriethoxysilane and octyltriethoxysilane in a molar ratio of 3:1, and the total mass of the composite modifier was 12% of the mass of vermiculite.

[0077] After composite modification, the mixture was vacuum impregnated with palmitic acid at a mass ratio of 2:8 to amphiphilic modified vermiculite to obtain amphiphilic confined phase change composite particles.

[0078] S2. Preparation of melamine-formaldehyde resin prepolymer; Add 37% formaldehyde solution and deionized water to a sealed container, and adjust the pH to 8.5-9.0 with 10% NaOH solution. Add melamine, stir, and slowly heat to 70-75℃. Maintain the temperature until the system changes from turbid to clear and transparent to obtain the melamine-formaldehyde resin prepolymer solution.

[0079] S3. Preparation of phase change temperature-controlled shell fire extinguishing microcapsules; The raw material ratio is as follows: perfluorohexanone 100 parts by weight; melamine-formaldehyde resin prepolymer (33 parts by weight of melamine); hydrophobic confined phase change composite particles 4 parts; amphiphilic confined phase change composite particles 3 parts; sodium dodecyl sulfonate (emulsifier) ​​4 parts; deionized water 120 parts.

[0080] Preparation of oil phase suspension: At room temperature, add perfluorohexanone and hydrophobic confined phase change composite particles into a sealed container, stir at 400 rpm for 30 min, mix to form a homogeneous oil phase suspension, and keep it in the dark and warm for later use.

[0081] Preparation of aqueous dispersion: Sodium dodecyl sulfonate and amphiphilic confined phase change composite particles are added to deionized water, heated to 35°C, and stirred until the emulsifier is completely dissolved to obtain an aqueous dispersion.

[0082] Emulsification and molding: The oil phase suspension is slowly added dropwise to the aqueous phase dispersion. After the addition is complete, the mixture is sheared and emulsified at 800 rpm for 30 minutes to form an oil-in-water emulsion.

[0083] Shell formation reaction: The melamine-formaldehyde resin prepolymer solution was slowly added to the emulsified emulsion and mixed thoroughly under medium-speed stirring at 400 rpm. The pH of the system was slowly adjusted to 4.0-5.0 with acetic acid solution, and the reaction was carried out under continuous stirring at 30℃ for 3 hours, allowing the resin to deposit and cross-link on the surface of the core material droplets. During the reaction, the confined phase change composite particles were embedded in the shell and core layers.

[0084] Post-processing: After the reaction was completed, the product was cooled to room temperature and then filtered and washed with deionized water four times to remove impurities remaining on the surface of the microcapsules. Subsequently, it was dried at room temperature to obtain the phase change temperature-controlled fire extinguishing microcapsule product.

[0085] The testing conditions are the same as in Example 1; After testing, combined Figure 6As shown, the surface morphology of the microcapsules prepared in this embodiment is illustrated. Similar to Example 1, the microcapsules exhibit a regular spherical shape with a continuous and dense shell. However, due to the different shell system, melamine resin is more brittle than polyurea, and some microcapsules have fine wrinkles or cracks on their surface. No obvious surface exposure or aggregation of the vermiculite / palmitic acid composite particles was observed in the melamine resin shell, indicating that they were effectively embedded within the shell.

[0086] TGA testing showed an encapsulation rate of 54%. The burst release temperature was 149℃. DSC testing showed an endothermic phase transition peak at 56℃, with a latent heat of phase transition of 15.3 J / g.

[0087] Example 3 A method for preparing a phase change temperature-controlled fire extinguishing microcapsule includes the following steps: S1. Preparation of confined phase change composite particles (1) Preparation of hydrophobic confined phase change composite particles; Halloysite was dried at 120°C for 2 hours.

[0088] Hydrophobic surface modification was performed using propyltriethoxysilane, with the mass of propyltriethoxysilane being 10% of the mass of halloysite.

[0089] After modification, PEG6000 was heated to 70°C to completely melt it, and then mixed with hydrophobically modified halloysite at a mass ratio of 4:6. The mixture was then impregnated at 70°C under vacuum for 2 hours to obtain hydrophobically confined phase change composite particles.

[0090] (2) Preparation of amphiphilic confined phase change composite particles Halloysite was amphiphilically modified with 3-aminopropyltriethoxysilane and propyltriethoxysilane at a molar ratio of 1:2. Subsequently, vacuum impregnation was performed with PEG6000 at a mass ratio of 4:6 to the amphiphilically modified halloysite to obtain amphiphilic confined phase change composite particles.

[0091] S2. Preparation of phase change temperature-controlled shell fire extinguishing microcapsules Raw material ratio (based on 100 parts by weight of perfluorohexanone): 100 parts perfluorohexanone; 100 parts methyl nonafluorobutyl ether; 27 parts resorcinol; 36 parts formaldehyde solution (37 wt%); 3 parts hydrophobic confined phase change composite particles; 4 parts amphiphilic confined phase change composite particles; 2 parts sodium dodecyl sulfate; 200 parts deionized water. Nitrogen gas is introduced throughout the process to prevent oxidation of the system.

[0092] Preparation of oil phase suspension: At room temperature, perfluorohexanone, methyl nonafluorobutyl ether and hydrophobic confined phase change composite particles are added to a sealed container and stirred at 400 rpm for 30 min to mix into a homogeneous oil phase suspension. The mixture is then kept in the dark and warm for later use.

[0093] Preparation of aqueous dispersion: Sodium dodecyl sulfate and amphiphilic confined phase change composite particles are added to deionized water, heated to 35°C, and stirred until the emulsifier is completely dissolved to obtain an aqueous dispersion.

[0094] Emulsification and molding: The oil phase suspension is slowly added dropwise to the aqueous phase dispersion. After the addition is completed, the mixture is sheared and emulsified at 1000 rpm for 30 minutes to form an oil-in-water emulsion.

[0095] In-situ polymerization: Formaldehyde solution is added to the emulsion, the pH is adjusted to 8-9 with NaOH solution, the temperature is raised to 35℃, and the reaction is carried out for 2 hours under mechanical stirring at 400 rpm, causing resorcinol and formaldehyde to undergo condensation crosslinking on the surface of the core material droplets to form a phenolic resin shell. During the reaction, inorganic confined phase change composite particles are embedded inside the phenolic resin shell.

[0096] Post-processing: After the reaction was completed, the product was naturally cooled to room temperature and then filtered and washed with deionized water four times. Subsequently, it was dried at 35°C for 12 hours to obtain the phase change temperature-controlled fire extinguishing microcapsule product.

[0097] The testing conditions are the same as in Example 1; Testing revealed that the microcapsules exhibited a regular core-shell spherical structure. TGA testing showed an encapsulation rate of 90%. The rupture release temperature was 147℃. DSC testing showed an endothermic phase transition peak at 56℃, with a latent heat of phase transition of 17.9 J / g.

[0098] Comparative Example 1 Except for the absence of confined phase change composite particles, the other raw material ratios and preparation steps are exactly the same as in Example 1.

[0099] Raw material ratio (based on 100 parts by weight of perfluorohexanone): 100 parts perfluorohexanone; 100 parts methyl nonafluorobutyl ether; 20 parts IPDI; 5 parts diethylenetriamine; 3 parts sodium dodecyl sulfate; 500 parts deionized water.

[0100] The testing conditions are the same as in Example 1; Testing revealed an encapsulation rate of 55% and a burst release temperature of 108°C. DSC analysis showed no endothermic peak during phase change (latent heat of phase change was 0). After storage at 80°C for 100 hours, the thermal weight loss was approximately 45%, significantly higher than that of Example 1 (<10%). These results indicate that while the microcapsules without the addition of inorganic confined phase change composite particles exhibit similar encapsulation rates and burst release temperatures, the lack of thermal buffering from the phase change material leads to severe vaporization and leakage of the perfluorohexanone core material during long-term high-temperature storage, resulting in insufficient long-term storage stability.

[0101] Comparative Example 2 The preparation of the confined phase change composite particles was the same as in Example 1. In the raw material ratio, the amount of confined phase change composite particles added was adjusted to 25 parts (accounting for 25% of the mass of perfluorohexanone), and the remaining raw material ratios and preparation steps were the same as in Example 1.

[0102] The testing conditions are the same as in Example 1; Testing revealed that during emulsification, excessive solid filler increased the density and viscosity of the oil phase, significantly reducing emulsion stability and leading to noticeable particle sedimentation and stratification after standing. The resulting microcapsule product contained numerous exposed composite particles on the shell surface, exhibiting poor shell continuity and shell defects in some microcapsules. The encapsulation rate decreased to approximately 35%. The rupture release temperature was 32°C, significantly lower than in Example 1, indicating insufficient shell integrity. DSC testing showed a latent heat of phase change of 45.6 J / g. After storage at 80°C for 8 hours, the core layer completely leaked. These results indicate that excessive confined phase change composite particles disrupted the molding integrity of the polymer shell, causing microscopic defects and accelerating core leakage.

[0103] Comparative Example 3 The preparation of the inorganic confined phase change composite particles was the same as in Example 1. In the raw material ratio, the amount of confined phase change composite particles added was adjusted to 1 part (accounting for 1% of the mass of perfluorohexanone), and the remaining raw material ratios and preparation steps were the same as in Example 1.

[0104] The testing conditions are the same as in Example 1; The coating rate was tested to be 58%. The burst release temperature was 110℃. DSC testing showed that the latent heat of phase change was only 2.3 J / g, indicating extremely limited heat absorption capacity. After storage at 80℃ for 100 h, the thermal weight loss was approximately 22%, a negligible improvement compared to Comparative Example 1 (25%). The results indicate that excessively low amounts of composite particles cannot provide sufficient heat absorption capacity, making it difficult to produce a measurable temperature rise suppression effect, and the improvement in long-term storage stability is not significant.

[0105] Comparative Example 4 The raw materials were weighed according to a mass ratio of octadecyl alcohol to halloysite of 4:6 (the mass ratio of phase change material to carrier is approximately 4:6, exceeding the upper limit of the phase change material proportion corresponding to claims 1-3:9-2). The vacuum impregnation method was used for preparation as in Example 1.

[0106] The testing conditions are the same as in Example 1; Testing revealed that during the impregnation process, due to excessive addition of phase change material exceeding the effective loading capacity of the halloysite hollow cavity, some octadecyl alcohol failed to be adsorbed by the carrier pores and remained on the outer surface of the particles. After cooling, precipitated octadecyl alcohol crystals were clearly visible on the particle surface. When the resulting composite particles were used for microcapsule preparation, the free octadecyl alcohol interfered with the stability of the oil-water interface during emulsification, resulting in incomplete microcapsule encapsulation.

[0107] Comparative Example 5 The raw materials were weighed according to a mass ratio of octadecyl alcohol to halloysite of 0.5:9.5. The vacuum impregnation method was used for preparation as in Example 1.

[0108] The testing conditions are the same as in Example 1; Testing revealed an extremely low loading of phase change material in the composite particles. DSC analysis showed that the latent heat of phase change in the composite particles was only 7.5 J / g. When the obtained composite particles were used for microcapsule preparation (with the same addition amount as in Example 1), the final microcapsules exhibited a latent heat of phase change of only 0.9 J / g, indicating a negligible thermal buffering function. After storage at 80°C for 100 hours, the thermal weight loss was approximately 24%, which is essentially equivalent to that of Comparative Example 1.

[0109] In summary, comparing Example 1 and Comparative Example 1, both have similar coverage rates and rupture release temperatures. However, Example 1 exhibits significantly better thermal weight loss after high-temperature storage at 80°C / 100h compared to Comparative Example 1. This difference is attributed to the endothermic phase change of the inorganic confined phase change composite particles in Example 1: when the ambient temperature rises above 48°C, octadecyl alcohol undergoes a solid-liquid phase change, absorbing heat and reducing the effective heat transferred to the perfluorohexanone core material, thus slowing down the temperature rise rate and vaporization leakage process of the core material. In contrast, Comparative Example 1 lacks the thermal buffering effect of the phase change material, and the perfluorohexanone core material directly vaporizes at high temperatures and diffuses and leaks through the shell.

[0110] By comparing the amount of composite particles added in Example 1, Comparative Example 2, and Comparative Example 3, it can be seen that when the amount added in Comparative Example 3 is 1 part, the latent heat of phase change is only 2.3 J / g, and the heat absorption capacity is insufficient to produce a significant temperature rise suppression effect; when the amount added in Example 1 is 8 parts, the latent heat of phase change reaches 18.2 J / g, and the thermal weight loss is significantly reduced to <10%; when the amount added is further increased to 25 parts in Comparative Example 2, the excessive solid filler destroys the integrity of the shell molding, the coverage rate drops sharply to 35%, the rupture release temperature drops to 95°C, and the shell defects accelerate the core material leakage, with the thermal weight loss rising to about 30%.

[0111] Comparing the mass ratios of PCM to the carrier in Examples 1, 4, and 5, it can be seen that when the PCM ratio is too high, the phase change material exceeds the effective loading capacity of the carrier, and the free phase change material interferes with the emulsion stability and damages the shell quality. When the PCM ratio is too low, the latent heat of phase change of the composite particles is extremely limited, and it cannot perform its heat buffering function. The mass ratio in Example 1 ensures that the phase change material reaches a suitable filling density inside the carrier, which guarantees sufficient heat absorption capacity and avoids phase separation and process defects caused by exceeding the carrier's loading capacity.

[0112] Examples 1, 2, and 3 all successfully prepared fire extinguishing microcapsules with phase change temperature control function, with encapsulation rates of 60%, 54%, and 90%, respectively, and rupture release temperatures of 112℃, 149℃, and 147℃. The results of the three examples demonstrate that the present invention is not dependent on specific wall material chemical compositions and exhibits good adaptability to three mainstream shell systems: polyurea, melamine resin, and phenolic resin, possessing broad industrial applicability. Among them, the phenolic resin system in Example 3 achieved the highest encapsulation rate of 90%, which is attributed to the relatively mild reaction conditions and good shell-forming properties during the in-situ polymerization of phenolic resin.

[0113] The DSC test results of Example 1 showed that the phase transition temperature of octadecyl alcohol loaded in halloysite nanotubes was 48°C, which was 7°C lower than the theoretical phase transition temperature of pure octadecyl alcohol (55°C). This is because the hollow cavity of halloysite creates a nanoscale spatial confinement effect on the octadecyl alcohol molecules. Within the nanoscale confined space, the degree of freedom of movement and crystal orientation of the phase change material molecules are restricted by the pore walls, leading to changes in crystallization kinetics, which manifests as a decrease in the phase transition temperature. Nevertheless, the latent heat of phase transition of 18.2 J / g, which is the heat absorption function of the phase change material, is still retained, and its core heat buffering function remains unaffected.

[0114] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art can still modify the technical solutions described in the foregoing embodiments or make equivalent substitutions for some of the technical features. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A phase change temperature-controlled fire extinguishing microcapsule, characterized in that, The microcapsule has a core-shell structure containing confined phase change composite particles; The confined phase change composite particles include hydrophobic confined phase change composite particles and amphiphilic confined phase change composite particles. The core layer of the core-shell structure is composed of perfluorohexanone and the hydrophobic confined phase transition composite particles; The shell of the core-shell structure is composed of a thermosetting resin precursor and the amphiphilic confined phase change composite particles. The average particle size of the microcapsules is 5 μm to 500 μm.

2. The phase change temperature-controlled fire extinguishing microcapsule according to claim 1, characterized in that, Both the hydrophobic confined phase change composite particles and the amphiphilic confined phase change composite particles comprise organic phase change materials and inorganic porous carriers, with the mass ratio of organic phase change materials to inorganic porous carriers being 1~3:9~2.

3. The phase change temperature-controlled fire extinguishing microcapsule according to claim 2, characterized in that, The organic phase change material is selected from any one of fatty alcohols, fatty acids, and polyethylene glycol; The fatty alcohol is C 14 The fatty alcohol is C 24 The fatty alcohol is C 12 The fatty alcohol is C 24 The fatty alcohol is C 4. The phase change temperature-controlled fire extinguishing microcapsule according to claim 2, characterized in that, The hydrophobic confined phase change composite particles are prepared by surface modification of an inorganic porous carrier with a hydrophobic modifier; wherein the hydrophobic modifier is selected from one or more of hexamethyldisilazane, methyltrimethoxysilane, methyltriethoxysilane, and C3-C8 alkyltrialkoxysilane. And / or, the amphiphilic confined phase change composite particles are prepared by surface modification of an inorganic porous carrier with aminosilane and C3-C8 alkyltrialkoxysilane; wherein the molar ratio of aminosilane to C3-C8 alkyltrialkoxysilane is 1:3 to 3:

1. And / or, the inorganic porous carrier is selected from any one of vermiculite, mesoporous silica, silica aerogel or halloysite.

5. The phase change temperature-controlled fire extinguishing microcapsule according to claim 2, characterized in that, The raw materials for preparing the microcapsules, based on 100 parts by weight of perfluorohexanone, include: Thermosetting resin precursor: 5-50 parts; Emulsifier: 0.5~10 parts; Hydrophobic confined phase change composite particles: 1~10 parts; Amphiphilic confined phase transition composite particles: 1~10 parts; Crosslinking agent: 0~20 parts; Fluorinated ether cosolvent: 0~100 parts; Deionized water: 200-600 parts.

6. A method for preparing the phase change temperature-controlled fire extinguishing microcapsule according to claim 5, characterized in that, Includes the following steps: Step S1: Add perfluorohexanone, fluoroether co-solvent and hydrophobic confined phase change composite particles into a sealed container, stir and mix evenly to form an oil phase suspension, and keep it in the dark and warm for later use. Step S2: Add the emulsifier and amphiphilic confined phase change composite particles to deionized water, heat to 20~40℃, and stir until the emulsifier is completely dissolved to obtain an aqueous dispersion. Step S3: The oil phase suspension obtained in step S1 is slowly added dropwise to the aqueous phase dispersion obtained in step S2 and shear emulsified to form an oil-in-water emulsion; Step S4: Add a thermosetting resin precursor and a crosslinking agent to the oil-in-water emulsion obtained in step S3, so that the thermosetting resin precursor undergoes a polymerization reaction at the oil-water interface to form a shell layer, and at the same time, the confined phase change composite particles are embedded in the shell layer and the core layer; after curing, washing and low-temperature drying, the phase change temperature-controlled fire extinguishing microcapsules are obtained.

7. The method for preparing phase change temperature-controlled fire extinguishing microcapsules according to claim 6, characterized in that, The emulsifier is selected from one or more of sodium dodecyl sulfate, sodium dodecyl sulfonate, Tween-80, gum arabic, and PVA. And / or, in step S3, the emulsification speed is 200 rpm to 5000 rpm, and the emulsification time is 2 min to 30 min; And / or, in step S4, the polymerization reaction temperature is 20℃~45℃, and the reaction time is 1h~5h.

8. The method for preparing phase change temperature-controlled fire extinguishing microcapsules according to claim 6, characterized in that, In step S1, the preparation process of the hydrophobic confined phase change composite particles is as follows: Step 1: The inorganic porous carrier is surface modified with a hydrophobic modifier to obtain a modified inorganic porous carrier, wherein the amount of hydrophobic modifier added is 1% to 15% of the mass of the inorganic porous carrier; Step 2: Place the hydrophobic modified inorganic porous carrier obtained in Step 1 in a forced-air drying oven and dry it at 100℃~120℃ for 1h~2h. Step 3: Heat the organic phase change material to a temperature 10°C to 20°C above its phase change point to melt it, and stir it under heat preservation conditions until it is completely melted to obtain a homogeneous and clear liquid phase system; Step 4: Place the dried hydrophobic modified inorganic porous carrier obtained in Step 2 into a vacuum reaction apparatus and preheat the vacuum reaction apparatus to 10°C~20°C higher than the phase change temperature of the phase change material. Then add molten organic phase change material to it and vacuum impregnate it for 1h~2h under heat preservation conditions. Cool the impregnated mixture to room temperature to allow the phase change material to solidify inside the modified inorganic porous carrier, thus obtaining hydrophobic confined phase change composite particles.

9. The method for preparing phase change temperature-controlled fire extinguishing microcapsules according to claim 6, characterized in that, In step S1, the preparation process of the amphiphilic confined phase change composite particles is as follows: Step 1: The inorganic porous carrier is surface modified with amphiphilic silane, that is, aminosilane and C3~C8 alkyltrialkoxysilane are prepared into a composite modifier in a molar ratio of 1:3 to 3:1, and the inorganic porous carrier is surface modified with the composite modifier to obtain an amphiphilic inorganic porous carrier. Step 2: Place the modified inorganic porous carrier obtained in Step 1 in a forced-air drying oven and dry it at 100℃~120℃ for 1h~2h. Step 3: Heat the organic phase change material to a temperature 10°C to 20°C above its phase change point to melt it, and stir it under heat preservation conditions until it is completely melted to obtain a homogeneous and clear liquid phase system; Step 4: Place the dried modified inorganic porous carrier obtained in Step 2 into a vacuum reaction apparatus and preheat the vacuum reaction apparatus to 10°C~20°C higher than the phase change temperature of the phase change material. Then add molten organic phase change material to it and vacuum impregnate it for 1h~2h under heat preservation conditions. Cool the impregnated mixture to room temperature to allow the phase change material to solidify inside the modified inorganic porous carrier, thus obtaining amphiphilic confined phase change composite particles.

10. The method for preparing phase change temperature-controlled fire extinguishing microcapsules according to claim 5, characterized in that, The thermosetting shell-forming precursor is selected from at least one of polyisocyanate, phenolic resin prepolymer, and melamine-formaldehyde resin prepolymer.