A biomimetic ion channel membrane and its application in seawater fractional crystallization

By using the light-controlled aperture switching technology of biomimetic ion channel membranes, the problems of equipment investment and land occupation in seawater desalination and salt resource recovery have been solved, realizing the efficient utilization of seawater resources and the recovery of salt resources.

CN123102173APending Publication Date: 2026-11-17TIANJIN SEA WATER DESALINATION & COMPLEX UTILIZATION INST STATE OCEANOGRAPHI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611576246.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-13
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing seawater desalination technologies produce high-salt concentrates while producing freshwater, resulting in a waste of salt resources and an increase in equipment investment and land area. Traditional membrane separation technologies cannot simultaneously meet the needs of freshwater production and salt resource recovery.

Method used

A biomimetic ion channel membrane is used, and the connectivity of confined water clusters is regulated by photoisomerization of spiropyran, so that the effective pore size of the membrane can be reversibly switched between desalination mode and fractional crystallization mode. Multifunctional integration is achieved by utilizing a bilayer heterogeneous structure of an upper negatively charged covalent organic framework layer and a lower photoresponsive covalent organic framework layer.

Benefits of technology

It enables flexible switching between desalination mode and fractional crystallization mode using the same membrane, improving the efficiency of seawater resource utilization and salt resource recovery rate, while reducing equipment investment and land area.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102173A_ABST
    Figure CN123102173A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of membrane separation technology, specifically disclosing a biomimetic ion channel membrane and its application in seawater fractionation and crystallization. The membrane comprises an upper negatively charged COF layer, a lower photoresponsive COF layer, and a polydopamine molecular adhesive layer between the two layers. The lower COF layer is covalently grafted with aminospiropyran photoresponsive units onto the inner wall of the pores via a post-synthetic grafting method. This invention utilizes the reversible photoisomerization of spiropyran under alternating UV / visible light irradiation to achieve precise and reversible switching of the effective pore size of the COF membrane: in the dark or under visible light, spiropyran is in a closed-ring state, with an effective pore size of 0.55~0.60 nm, achieving a high-salt-retention desalination mode; under UV irradiation, spiropyran isomerizes into an open-ring zwitterionic state, expanding the effective pore size to 0.66~0.72 nm, achieving Cl... ‑ Selective permeability and SO4² ‑ A highly efficient fractional crystallization mode. This invention achieves multifunctional integration of a single membrane, satisfying the needs of both freshwater production and salt resource recovery through light-controlled mode switching, with the obtained NaCl purity reaching over 99%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of membrane separation technology, specifically relating to a biomimetic ion channel membrane and its application in seawater fractionation crystallization. Background Technology

[0002] Seawater desalination is a crucial way to alleviate global water shortages. However, existing desalination technologies produce large amounts of high-salinity concentrate along with freshwater. Direct discharge of this concentrate would severely damage the marine ecosystem; while advanced treatment faces technical and economic bottlenecks due to high energy consumption and low efficiency. More importantly, the high-salinity wastewater contains various salts with recovery value, such as sodium chloride and sodium sulfate, but current technologies lack efficient and low-cost separation and recovery methods, resulting in the waste of significant salt resources.

[0003] Traditional membrane separation technologies such as nanofiltration and reverse osmosis have been widely used in seawater desalination. However, the disordered pore structure and uneven pore size distribution of traditional polymer membranes make it impossible to accurately separate chloride and sulfate ions with hydration diameters differing only by a few angstroms, severely limiting the efficiency of high-salinity wastewater separation and crystallization. Covalent organic frameworks, as a novel porous crystalline material, possess advantages such as highly ordered pore structure and precisely controllable pore size, and are considered an ideal material platform for next-generation separation membranes. In recent years, researchers have successfully prepared various covalent organic framework membranes and applied them to the field of ion separation, demonstrating excellent molecular sieving potential.

[0004] However, existing covalent organic framework membranes all have fixed pore sizes, meaning a single membrane can only perform a single separation function. In actual seawater treatment, different operating conditions present vastly different requirements: sometimes it's necessary to retain all salt to produce freshwater, while other times selective separation of specific ions is needed for salt resource recovery. Existing fixed-pore membranes cannot simultaneously meet both needs, necessitating the configuration of two independent treatment systems, significantly increasing equipment investment and floor space requirements. Therefore, how to integrate multiple separation functions onto a single membrane, enabling it to flexibly switch operating modes according to actual needs, is a key technical challenge that urgently needs to be solved in the field of membrane separation.

[0005] To address the aforementioned problems, inspired by the ability of ion channel proteins on biological cell membranes to switch between "on" and "off" states under different stimuli, this invention provides a biomimetic ion channel membrane and its application in seawater fractional crystallization. This invention utilizes the photoisomerization of spiropyran to regulate the connectivity of confined water clusters, achieving reversible switching of the membrane's effective pore size between two states. This allows the same membrane to flexibly switch between desalination and fractional crystallization modes, respectively meeting the needs of freshwater production and salt resource recovery, thus providing a novel technological pathway for the resource utilization of seawater. Summary of the Invention

[0006] The purpose of this invention is to overcome the shortcomings of the prior art and provide a biomimetic ion channel membrane and its application in seawater fractional crystallization.

[0007] To achieve the above objectives, the present invention adopts the following technical solution.

[0008] 1. A biomimetic ion channel membrane The membrane comprises two covalent organic framework layers, an upper layer and a lower layer, and a polydopamine molecular adhesive layer located between the two layers.

[0009] The upper layer is a non-photoresponsive negatively charged covalent organic framework layer, and its pore walls contain sulfonic acid groups.

[0010] The lower layer is a photoresponsive covalent organic framework layer, on which aminospiropyran photoresponsive units are covalently grafted onto the residual active sites on the inner wall of the covalent organic framework pores using a post-synthetic grafting method.

[0011] The spiropyran unit is isomerized from a closed-ring nonionic state to an open-ring zwitterionic state under ultraviolet light irradiation at wavelengths of 360–400 nm, and the effective pore size of the covalent organic framework membrane is reversibly switched by regulating the connectivity of the confined water clusters; it is restored to a closed-ring nonionic state under visible light irradiation at wavelengths greater than 450 nm or in the dark.

[0012] The membrane can switch between two operating modes by light irradiation: in dark or visible light irradiation, it operates in desalination mode, with an effective pore size of 0.55–0.60 nm, achieving high salt rejection; under ultraviolet light irradiation, it operates in fractional crystallization mode, with an effective pore size of 0.66–0.72 nm, achieving selective permeation of chloride ions and efficient rejection of sulfate ions. The separation mechanism of the membrane is light-controlled size sieving.

[0013] The lower photoresponsive covalent organic framework layer is prepared by the following post-synthetic grafting method: First, a parent covalent organic framework membrane containing residual aldehyde groups is synthesized. By controlling the feed ratio of the trialdehyde monomer 2,4,6-tricarboxymethyl phloroglucinol to the triamino monomer tris(4-aminophenyl)amine, the trialdehyde monomer is in excess by 5-15 mol%, that is, the molar ratio of triamino monomer to trialdehyde monomer is 0.87:1 to 0.95:1. Unreacted aldehyde groups are retained on the inner wall of the covalent organic framework pores as grafting sites. Then, an amino-containing spiropyran derivative, namely aminospiropyran, is synthesized. The aminospiropyran reacts with the residual aldehyde groups on the inner wall of the parent covalent organic framework pores through its amino group to form an imine bond, and the spiropyran unit is covalently grafted to the inner wall of the covalent organic framework pores.

[0014] The upper negatively charged covalent organic framework layer is prepared by polycondensation reaction of sulfonic acid-functionalized diamine monomer 2,5-diaminobenzenesulfonic acid and 1,3,5-tricarboxymethylresorcinol to form a TpPa-SO3H covalent organic framework layer; wherein the molar ratio of 2,5-diaminobenzenesulfonic acid to 1,3,5-tricarboxymethylresorcinol is 1.5:1, that is, the functional groups of amino and aldehyde groups are equivalent; the reaction of 1,3,5-tricarboxymethylresorcinol with amine monomers forms β-ketoenamine bonds, which obtain significantly enhanced hydrolytic stability through intramolecular hydrogen bonding and conjugation effect.

[0015] The parent covalent organic framework of the lower photoresponsive covalent organic framework layer is prepared by polycondensation of tris(4-aminophenyl)amine and 2,4,6-tricarboxymethyl phloroglucinol to form a TAPA-TFP covalent organic framework layer; 2,4,6-tricarboxymethyl phloroglucinol reacts with amine monomers to form β-keto-enamine bonds; after grafting spiropyran, the effective pore size of the membrane is 0.55~0.60 nm in desalination mode and 0.66~0.72 nm in fractional crystallization mode.

[0016] The membrane has an effective pore size of 0.55~0.60 nm in desalination mode, which is smaller than the hydration diameter of chloride ions, thus achieving high retention of sodium chloride. In fractional crystallization mode, the membrane has an effective pore size of 0.66~0.72 nm, which is between the hydration diameter of chloride ions and the hydration diameter of sulfate ions, allowing chloride ions to selectively permeate while sulfate ions are effectively retained. By controlling the grafting density of spiropyran, i.e., 10~50 mol% relative to the covalent organic framework building units, the effective pore size in both modes can be precisely controlled.

[0017] The polydopamine molecular adhesive layer is formed on the surface of the upper covalent organic framework by oxidative self-polymerization of dopamine, with a thickness of 2~10 nm, preferably 3~5 nm. The polydopamine layer enhances the interlayer bonding force by forming multiple interactions such as covalent bonds, hydrogen bonds and π-π stacking with the functional groups of the upper and lower covalent organic frameworks through its catechol groups.

[0018] The porous substrate of the membrane is a solvent-resistant and temperature-resistant cross-linked polyimide porous membrane.

[0019] 2. Method for preparing the above-mentioned biomimetic ion channel membrane Includes the following steps: Step 1: Synthesis of aminospiropyran photoresponsive molecules Phenylhydrazine and 3-methyl-2-butanone were added to the reaction system at a molar ratio of 1:1. Using glacial acetic acid as solvent, the reaction was refluxed at 80-100℃ for 4-6 h. After the reaction was completed, the solvent was removed by vacuum distillation. The residue was extracted with diethyl ether, washed with saturated sodium chloride solution, washed with saturated sodium bicarbonate solution, dried with anhydrous sodium sulfate, and then distilled under vacuum to obtain 2,3,3-trimethyl-3H-indole. 2,3,3-trimethyl-3H-indole was dissolved in anhydrous ethanol, and excess iodomethane was added, wherein the molar ratio of 2,3,3-trimethyl-3H-indole to iodomethane was 1:1.1~1.3. The mixture was refluxed at 60~70℃ for 12~18 h, and after cooling, the precipitated solid was filtered, washed with cold ethanol, and dried under vacuum to obtain 1,2,3,3-tetramethyl-3H-indoleonium iodide. 1,2,3,3-Tetramethyl-3H-indoline iodide was dissolved in deionized water, and 10 wt% NaOH aqueous solution was slowly added dropwise until the pH reached 9-10. The mixture was stirred at room temperature for 0.5-1 h, extracted with diethyl ether, and the organic phases were combined, washed with saturated sodium chloride solution, dried over anhydrous sodium sulfate, and the solvent was removed by vacuum distillation to obtain 2-methylene-1,3,3-trimethylindoline, i.e., the Fischer base. Salicylic aldehyde was slowly added dropwise to a mixed acid of fuming nitric acid and concentrated sulfuric acid in a volume ratio of 2:3 under an ice bath at 0~5℃, while controlling the temperature to not exceed 5℃. After the addition was completed, the mixture was raised to room temperature and reacted for 2~3 hours. The reaction solution was then poured into ice water, and the precipitated yellow precipitate was filtered out. After washing with cold water, the precipitate was recrystallized from ethanol to obtain 5-nitrosalicylic aldehyde. Fischer base and 5-nitrosalicylaldehyde were dissolved in anhydrous ethanol at a molar ratio of 1:1.02 and condensed by reflux at 80-85°C for 6-8 h. The solvent was removed by vacuum distillation, and the product was purified by column chromatography with a mixture of petroleum ether and ethyl acetate in a volume ratio of 5:1 as the eluent to obtain nitrospiropyran. Nitrospiropyran was dissolved in ethanol, and 10 wt% Pd / C catalyst was added. The mass ratio of nitrospiropyran to Pd / C was 10:1. The mixture was stirred at room temperature for 12-16 h under a hydrogen atmosphere of 1 atm, or reacted with SnCl2·2H2O in concentrated hydrochloric acid at 40-50 °C for 4-6 h. The solvent was removed by filtration and vacuum distillation, and the mixture was purified by column chromatography with a 20:1 volume ratio of dichloromethane and methanol as the eluent to obtain aminospiropyran.

[0020] Step 2: Preparation of the upper negatively charged covalent organic framework layer After thermal crosslinking of the crosslinked polyimide porous substrate at 330℃ for 2 h, it was cut into the required size, ultrasonically cleaned with deionized water and ethanol for 15 min each, and then dried with nitrogen for later use. 2,5-Diaminobenzenesulfonic acid and 1,3,5-tricarboxymethyl phloroglucinol were added in a molar ratio of 1.5:1, i.e., the amino and aldehyde functional groups were in equal amounts, and dissolved in a mixed solvent of mesitylene, dioxane and acetic acid in a volume ratio of 5:5:1. The mixture was then sonicated for 10 minutes to ensure complete dissolution. The pretreated substrate was vertically suspended in the reactor, so that the substrate was completely immersed in the reaction solution. The reactor was sealed and the reaction was carried out at 120°C for 72 h in a solvothermal manner. After the reaction was completed, the membrane was naturally cooled to room temperature, removed, and washed three times each with DMF, methanol, and deionized water for 10 min each time. It was then vacuum dried at 60 °C for 12 h to form a TpPa-SO3H covalent organic framework layer on the substrate surface with a thickness of 180~220 nm.

[0021] Step 3: Introduction of the polydopamine molecular adhesive layer Dopamine hydrochloride was dissolved in Tris-HCl buffer with a concentration of 10 mmol / L and pH 8.5 to prepare a dopamine solution with a concentration of 1.0 g / L. The TpPa-SO3H composite membrane obtained in step 2 was completely immersed in the above dopamine solution and allowed to react at room temperature and under aerobic conditions for 4 h. During the reaction, the solution was gently stirred to promote uniform deposition. Remove the membrane and rinse the surface three times with deionized water to remove unpolymerized dopamine monomers, forming a polydopamine thin layer with a thickness of 3-5 nm.

[0022] Step 4: Preparation of the parent covalent organic framework layer Tris(4-aminophenyl)amine and 2,4,6-tricarboxymethyl phloroglucinol were added at a molar ratio of 0.90:1, i.e., 10 mol% excess of trialdehyde monomer. The mixture was dissolved in a mixed solvent of mesitylene, dioxane and acetic acid in a volume ratio of 5:5:1 and sonicated for 10 min to aid dissolution. The TpPa-SO3H obtained in step 3 was vertically immersed in the above solution along with polydopamine and the substrate composite film. The reaction vessel was sealed and subjected to a solvothermal reaction at 80°C for 24 h. After the reaction was completed and the membrane was naturally cooled, it was removed and washed three times each with DMF and methanol, and twice with deionized water. It was then vacuum dried at 60°C for 8 h to form a TAPA-TFP covalent organic framework layer containing residual aldehyde groups on the surface of the polydopamine layer. The thickness of this layer was 120~180 nm.

[0023] Step 5: Post-synthetic grafting of spiropyran Aminospiropyran was dissolved in DMF to prepare a grafting solution with a concentration of 5 mmol / L; The TAPA-TFP covalent organic framework membrane containing residual aldehyde groups obtained in step four was immersed in the above aminospiropyran solution and reacted at 50°C for 24 h. The aminospiropyran formed an imine bond by reacting its amino group with the residual aldehyde group on the inner wall of the covalent organic framework pores, thus covalently grafting the spiropyran unit onto the inner wall of the covalent organic framework pores. After the reaction was completed, the membrane was removed and washed three times each with DMF, methanol and deionized water for 10 min each time to remove unreacted free aminospiropyran. It was then vacuum dried at 60 °C for 12 h to obtain the biomimetic ion channel membrane, denoted as TpPa-SO3H / PDA / TAPA-TFP-SP / substrate.

[0024] 3. Application of the above-mentioned biomimetic ion channel membrane in seawater fractional crystallization Includes the following steps: S1: Mode Selection and Light Control Separation Stage The membrane was placed in a nanofiltration device, and the feed liquid was simulated seawater mainly containing NaCl and Na2SO4; Under dark or visible light irradiation, i.e. desalination mode, simulated seawater is passed through the membrane with an operating pressure of 5~30 bar as the driving force to achieve high salt retention and produce low salinity permeable water; When the ultraviolet light is switched to a wavelength of 360~400 nm, i.e., the fractional crystallization mode, the ultraviolet light irradiation intensity is 5~50 mW / cm², and the effective pore size of the membrane is expanded from 0.55~0.60 nm to 0.66~0.72 nm. At the same time, simulated seawater is passed through the membrane by pressure as the driving force. The upper TpPa-SO3H layer pre-retains large-sized impurities, colloidal substances, and suspended particles through size sieving. In the lower TAPA-TFP-SP layer, spiropyran isomerizes into an open-ring zwitterionic state under ultraviolet light irradiation. By controlling the connectivity of confined water clusters, the effective pore size is switched to a fractional crystallization mode, achieving Cl... - Selective permeability and SO4² - Highly efficient interception; Collect Cl-rich - The permeable liquid.

[0025] S2: Separative Crystallization Stage The Cl-rich material collected in step S1 - The permeate was evaporated and crystallized at 50-90℃ to obtain high-purity NaCl crystals; The retentate is rich in SO4²⁻ - It can be processed separately or recycled as a by-product raw material.

[0026] S3: Pattern Recovery and Looping Spiropyran was irradiated with visible light with a wavelength greater than 450 nm to restore it from an open-ring zwitterionic state to a closed-ring nonionic state, and the membrane returned to desalination mode. Steps S1 and S2 were repeated.

[0027] Compared with the prior art, the present invention has the following beneficial effects: First, it features light-controlled reversible dual-mode switching. This invention covalently grafts spiropyran photoresponsive units onto the inner wall of the pores of a covalent organic framework, utilizing the reversible isomerization of spiropyran under ultraviolet or visible light irradiation to achieve precise and reversible switching of the membrane's effective pore size. Unlike traditional fixed-pore-size membranes that can only perform a single separation function, this invention allows the same membrane to switch between desalination and fractional crystallization modes, achieving multi-functional integration of a single membrane.

[0028] Second, the bilayer heterogeneous structure provides synergistic benefits. This invention employs a bilayer heterogeneous structure consisting of an upper negatively charged TpPa-SO3H layer and a lower photoresponsive TAPA-TFP-SP layer. The upper layer provides pre-sieving, retaining large-sized impurities, colloidal substances, and suspended particles, while protecting the lower layer for fine sieving and separation. A synergistic sieving channel with a decreasing pore size gradient is formed between the two layers. The upper layer pre-retains large-sized impurities and multivalent ions through size sieving and charge repulsion, while the lower layer achieves precise sieving of monovalent and divalent ions through photocontrolled pore size switching. The synergistic effect of the two layers significantly improves separation efficiency and selectivity.

[0029] Third, polydopamine molecular adhesive enhances interlayer bonding. This invention introduces a polydopamine molecular adhesive layer between two covalent organic framework layers. Through the catechol groups forming covalent bonds, hydrogen bonds, and π-π stacking with the functional groups of the upper and lower covalent organic frameworks, multiple interactions are formed, significantly enhancing the interlayer bonding and structural stability of the membrane, effectively solving the technical problem of easy peeling between layers of multilayer covalent organic framework membranes.

[0030] Fourth, a complete solution for seawater fractional crystallization. This invention provides a complete seawater fractional crystallization process, from light-controlled separation to evaporation crystallization and pattern recovery, achieving the integration of seawater desalination and salt resource recovery, and has significant economic and environmental benefits. Attached Figure Description

[0031] Figure 1 The UV-Vis absorption spectrum of the biomimetic film after irradiation with UV and visible light; Figure 2 SEM cross-sectional image of the thin film. Detailed Implementation

[0032] Example 1: Synthesis of aminospiropyran photoresponsive molecules Synthesis of S1: 2,3,3-trimethyl-3H-indole 10.8 g (100 mmol) of phenylhydrazine and 8.6 g (100 mmol) of 3-methyl-2-butanone were dissolved in 50 mL of glacial acetic acid, and the mixture was heated under reflux for 4 h. After the reaction was completed, the mixture was cooled to room temperature, and the solvent was removed by vacuum distillation. The residue was extracted three times with 50 mL of diethyl ether each time. The organic phases were combined and washed successively with saturated sodium bicarbonate solution and saturated sodium chloride solution. The mixture was dried over anhydrous sodium sulfate overnight, filtered, and the solvent was removed by vacuum distillation to give 2,3,3-trimethyl-3H-indole.

[0033] S2: Synthesis of 1,2,3,3-tetramethyl-3H-indolium iodide 3.2 g (20 mmol) of 2,3,3-trimethyl-3H-indole was dissolved in 50 mL of anhydrous ethanol, and 3.1 g (22 mmol) of iodomethane was added. The mixture was heated under nitrogen protection and refluxed for 12 h. After the reaction was completed, the mixture was cooled to room temperature, and a pale yellow solid precipitated. The solid was filtered, washed three times with 10 mL of cold ethanol, and dried under vacuum for 12 h to obtain 1,2,3,3-tetramethyl-3H-indole iodide.

[0034] S3: Synthesis of Fischer base, 2-methylene-1,3,3-trimethylindoline. Dissolve 5.0 g (16.6 mmol) of the above quaternary ammonium salt in 30 mL of deionized water. Slowly add 10% NaOH solution dropwise under ice-water bath cooling until the pH reaches 10, and stir for 1 h. Extract three times with diethyl ether, 30 mL each time. Combine the organic phases, wash with saturated sodium chloride solution, dry to anhydrous sodium sulfate, and remove the solvent under reduced pressure to obtain 2-methylene-1,3,3-trimethylindoline.

[0035] Synthesis of S4: 5-Nitrosalicylaldehyde Under ice-water bath conditions ranging from 0 to 5 °C, 12.2 g (100 mmol) of salicylaldehyde was slowly added dropwise to a mixture of 20 mL of fuming nitric acid and 30 mL of concentrated sulfuric acid, controlling the dropping rate to keep the reaction temperature below 5 °C. After the addition was complete, the ice bath was removed, and the mixture was slowly brought to room temperature to continue the reaction for 2 h. The reaction solution was then slowly poured into 200 mL of ice water, resulting in the precipitation of a yellow precipitate. After standing for 30 min, the precipitate was filtered and washed with cold water until the filtrate was neutral. The crude product was recrystallized from ethanol to obtain 5-nitrosalicylic acid.

[0036] S5: Synthesis of Nitrospiropyran. 2.9 g (14.7 mmol) of 2-methylene-1,3,3-trimethylindoline and 2.5 g (15.0 mmol) of 5-nitrosalicylic acid were dissolved in 50 mL of anhydrous ethanol, and the mixture was heated under reflux for 6 h. After the reaction was complete, the mixture was cooled to room temperature, and the solvent was removed under reduced pressure. The residue was purified by column chromatography using 200-300 mesh silica gel as the stationary phase and a 5:1 (v / v) mixture of petroleum ether and ethyl acetate as the eluent. The orange fraction was collected, combined, and the solvent was removed under reduced pressure to obtain a yellow solid, nitrospiropyran.

[0037] ¹H NMR (400 MHz, CDCl3): δ 8.15 (d, J = 2.5 Hz, 1H), 8.05 (dd, J =9.0, 2.5 Hz, 1H), 7.20–6.80 (m, 4H), 6.68 (d, J = 10.5 Hz, 1H), 6.65 (d, J =9.0 Hz, 1H), 5.85 (d, J = 10.5 Hz, 1H), 2.75 (s, 3H), 1.25 (s, 3H), 1.15 (s, 3H).

[0038] S6: Synthesis of aminospiropyran 3.2 g (10 mmol) of nitrospiropyran was dissolved in 50 mL of ethanol, and 0.3 g of 10% Pd / C was added. The mixture was stirred at room temperature for 12 h under a hydrogen atmosphere (1 atm). After the reaction was complete, Pd / C was removed by filtration, and the solvent was removed by vacuum distillation. The residue was purified by column chromatography using 200-300 mesh silica gel as the stationary phase and a 20:1 (v / v) mixture of dichloromethane and methanol as the eluent. The product fractions were collected, combined, and the solvent was removed by vacuum distillation to obtain a yellow solid aminospiropyran.

[0039] ¹H NMR (400 MHz, CDCl3): δ 7.20–6.80 (m, 4H), 6.75 (d, J = 2.5 Hz,1H), 6.68 (d, J = 10.5 Hz, 1H), 6.65 (dd, J = 8.5, 2.5 Hz, 1H), 6.55 (d, J= 8.5 Hz, 1H), 5.85 (d, J = 10.5 Hz, 1H), 3.65 (br s, 2H, -NH2), 2.75 (s, 3H), 1.25 (s, 3H), 1.15 (s, 3H).

[0040] Example 2: Preparation of biomimetic ion channel membrane S1: Preparation of cross-linked polyimide porous substrate The polyimide porous membrane was cut to the required size and placed in a tube furnace. Under nitrogen protection, the temperature was increased to 330 °C at a rate of 5 °C / min and held for 2 h to induce thermal cross-linking, thereby improving its stability in organic solvents such as DMF. After heat treatment, the membrane was naturally cooled to room temperature and then ultrasonically cleaned with deionized water and ethanol for 15 min each. Finally, it was dried with nitrogen for later use.

[0041] S2: Preparation of the upper TpPa-SO3H covalent organic framework layer 0.5 mmol of 2,5-diaminobenzenesulfonic acid (Pa-SO3H) and 0.33 mmol of 1,3,5-tricarboxymethyl phloroglucinol (Tp) were dissolved in 15 mL of a mixed solvent of mesitylene, dioxane, and acetic acid in a volume ratio of 5:5:1. The solution was sonicated for 10 min to ensure complete dissolution. The solution was then transferred to a hydrothermal reactor containing a cross-linked polyimide substrate, sealed, and placed in an oven for solvothermal reaction at 120 °C for 72 h. After the reaction, the membrane was allowed to cool naturally to room temperature. The membrane was then removed and washed three times sequentially with DMF, methanol, and deionized water, immersing for 15 min each time, to remove unreacted monomers and residual solvent, yielding a TpPa-SO3H composite membrane.

[0042] S3: Preparation of polydopamine molecular adhesive layer Prepare 100 mL of Tris-HCl buffer solution with a pH of 8.5 and a concentration of 10 mmol / L. Dissolve 0.5 g of dopamine hydrochloride in the buffer solution to prepare a dopamine solution with a concentration of 2.5 g / L. Immerse the TpPa-SO3H composite membrane obtained in S2 with the substrate in the above solution and react at room temperature under aerobic conditions for 4 h. After the reaction, remove the membrane and wash it repeatedly with deionized water three times, soaking for 10 min each time, to remove unpolymerized dopamine monomers, obtaining the TpPa-SO3H composite membrane with PDA and the substrate. The thickness of the PDA layer was approximately 4 nm according to SEM cross-sectional measurements.

[0043] S4: Preparation of the parent covalent organic framework layer 0.95 mmol of tris(4-aminophenyl)amine (TAPA) and 1.05 mmol of 2,4,6-tricarboxymethyl phloroglucinol (TFP) were dissolved in 10 mL of a mixed solvent of mesitylene, dioxane, and acetic acid in a volume ratio of 5:5:1. The mixture was ultrasonically treated for 10 min to ensure uniform dispersion. The TpPa-SO3H composite membrane obtained in S3, along with the PDA and substrate, was immersed in the above solution and transferred to a hydrothermal reactor. After sealing, the reactor was placed in an oven and subjected to a solvothermal reaction at 80 °C for 24 h. After the reaction, the membrane was allowed to cool naturally to room temperature. The membrane was then removed and washed three times sequentially with DMF, methanol, and deionized water, immersing for 15 min each time, to remove unreacted monomers and residual solvent, yielding a TAPA-TFP covalent organic framework layer containing residual aldehyde groups.

[0044] S5: Post-synthetic grafting of spiropyran 34 mg (0.12 mmol) of the aminospiropyran synthesized in Example 1 was dissolved in 24 mL of DMF and sonicated for 5 min to ensure complete dissolution. The covalent organic framework membrane containing residual aldehyde groups obtained in S4 was immersed in the above solution and reacted at 50 °C for 24 h. After the reaction, the membrane was removed and washed three times in sequence with DMF, methanol, and deionized water, soaking for 15 min each time to remove unreacted aminospiropyran. It was then vacuum dried at 60 °C for 12 h to obtain the biomimetic ion channel membrane, denoted as TpPa-SO3H / PDA / TAPA-TFP-SP / substrate.

[0045] Example 3: Characterization of biomimetic ion channel membranes Photoisomerization characterization: The changes in the absorption spectrum of the film before and after irradiation with 365 nm UV light were monitored using a UV-Vis spectrophotometer. The film sample was fixed in a quartz cuvette, with air as the blank background, and the scanning wavelength range was 300 to 700 nm. Figure 1 As shown, the SP state has no obvious absorption peak at approximately 550 nm; after irradiation with ultraviolet light for 30 min, the MC state exhibits a characteristic absorption peak at approximately 550 nm, proving that spiropyran has successfully isomerized into a zwitterionic state. Subsequently, irradiation with visible light greater than 450 nm for 30 min causes the absorption peak at 550 nm to disappear, proving that the isomerization process is reversible.

[0046] Effective pore size characterization: using ions with different hydration diameters, including Li + Na + K + Cl - SO4² -The effective pore size of the membrane was calculated using the rejection curves of various ions. Specifically, the membrane was placed in a nanofiltration testing device with an effective area of ​​3.14 cm² and an operating pressure of 15 bar. Tests were conducted using feed solutions containing a single salt at a concentration of 10 mmol / L. Rejection rate-hydration diameter curves were plotted based on the rejection rates of each ion. The hydration diameter corresponding to a rejection rate of 50% was considered the effective pore size of the membrane. Test results showed that the effective pore size of the TAPA-TFP-SP layer was 0.55 to 0.60 nm in the SP state (desalination mode) and 0.66 to 0.72 nm after isomerization to the MC state (fractional crystallization mode) under UV irradiation. The effective pore size in both modes could be precisely controlled by adjusting the grafting density (10% to 50% molar percentage).

[0047] Film morphology characterization: Field emission scanning electron microscopy (FESEM) was used to observe the cross-section of the film. The sample underwent liquid nitrogen embrittlement followed by gold sputtering with an accelerating voltage of 5 kV. Figure 2 The SEM cross-sectional images show that the overall thickness of the three layers is about 350 nm, and the three layers are tightly bonded together with no obvious defects or interlayer delamination.

[0048] Example 4: Dual-mode separation performance test of biomimetic ion channel membrane The TpPa-SO3H / PDA / TAPA-TFP-SP / basement membrane prepared in Example 2 was placed in a nanofiltration test apparatus with an effective area of ​​3.14 cm² and an operating pressure of 15 bar. The feed solution was simulated seawater with a composition of 0.45 mol / L NaCl, 0.05 mol / L Na2SO4, and a total salt concentration of approximately 0.5 mol / L.

[0049] Desalination mode test: Nanofiltration was performed in the dark (without light) using pressure as the driving force. After the system had been running stably for 30 minutes, the permeate sample was collected, and the concentration of each ion in the permeate was detected by ion chromatography. The NaCl rejection rate was found to be 99.2%, and the Na2SO4 rejection rate was 99.5%.

[0050] Separate crystallization mode test: First, the membrane was irradiated with 365 nm ultraviolet light from the lower layer (TAPA-TFP-SP side) for 30 min at an intensity of 20 mW / cm². Then, nanofiltration was performed using pressure as the driving force. After the system had been running stably for 30 min, the permeate sample was collected, and the concentration of each ion in the permeate was measured. The Cl concentration was measured. - The retention rate drops to 20%, i.e., Cl - 80% transmittance, SO4² - The retention rate remained at 98%, Cl - / SO4² - The separation factor is approximately 80.

[0051] Example 5: Cyclic stability test of biomimetic ion channel membrane The membrane prepared in Example 2 was alternately irradiated with ultraviolet light and visible light. After each irradiation, the separation performance under both modes was tested according to the method in Example 4. The specific cycling conditions were: ultraviolet light irradiation for 30 min, light intensity 20 mW / cm², wavelength 365 nm; visible light irradiation for 30 min, light intensity 50 mW / cm², wavelength greater than 450 nm.

[0052] After 100 photo-switching cycles, in desalination mode, the NaCl retention rate increased from 99.2% to 98.8%, and the Na2SO4 retention rate increased from 99.5% to 99.0%; in fractional crystallization mode, Cl... - The retention rate changed from 20% to 22%, SO4² - The rejection rate remained at 97%. Changes in all properties were less than 5%, demonstrating the membrane's excellent photostability and cycle durability.

[0053] Application example: Simulating the fractional crystallization of seawater Feed solution preparation: The simulated seawater composition is 0.45 mol / L NaCl, 0.05 mol / L Na2SO4, and a total salt concentration of approximately 0.5 mol / L.

[0054] Experimental setup: A nanofiltration device was used, with TpPa-SO3H / PDA / TAPA-TFP-SP / basement membrane as the separation membrane, with an effective area of ​​10 cm².

[0055] Experimental Procedure: Irradiate the membrane with 365 nm ultraviolet light from the bottom for 30 min at an intensity of 20 mW / cm², then switch to fractional crystallization mode. Perform nanofiltration separation at an operating pressure of 15 bar and collect the permeate. Evaporate the collected permeate at 70 °C for 4 h to crystallize. Collect the crystallized product and perform XRD and ion chromatography analysis.

[0056] Results: In the fractional crystallization mode, Cl - The transmittance is 80%, SO4² - The retention rate was 98%, and the Cl in the permeate was [missing information]. - With SO4² - The molar ratio was increased from 9:1 in the feed to approximately 360:1. The XRD pattern of the crystals obtained by evaporation and crystallization was in perfect agreement with the NaCl standard card. Ion chromatography analysis showed that the purity of NaCl in the crystals reached 99.2%, and SO4²⁻ - The residual amount is less than 0.3 wt%.

[0057] In summary, this invention utilizes a gradient heterogeneous structure—an upper layer with negatively charged pre-sieving, a middle layer with PDA molecular adhesive, and a lower layer with photoresponsive fine sieving—to couple the reversible photoisomerization of spiropyran under UV / Vis light with the regulation of the connectivity of confined water clusters within the COF channels. This achieves precise and reversible switching of the effective pore size of the membrane, thus integrating desalination and fractional crystallization functions onto a single membrane. The middle polydopamine molecular adhesive layer enhances the bonding force between the upper and lower COF layers through hydrogen bonding and multiple interactions, forming a gradient sieving channel with decreasing pore size and synergistic charge repulsion and photoresponsiveness. This solves the problem of easy peeling between multilayer COF membranes and achieves synergistic effects between upper pre-sieving protection and lower photocontrolled fine sieving. Therefore, this invention achieves integrated seawater desalination and salt resource recovery with a single membrane, providing an innovative membrane material design and complete process route for fractional crystallization of high-salinity seawater.

Claims

1. A biomimetic ion channel membrane, characterized in that: The membrane comprises two covalent organic framework layers, an upper layer and a lower layer, and a polydopamine molecular adhesive layer located between the two layers; The upper layer is a non-photoresponsive negatively charged COF layer, and its inner wall contains sulfonic acid groups. The lower layer is a photoresponsive COF layer, which is covalently grafted with aminospiropyran photoresponsive units on the residual active sites on the inner wall of the COF channels by a post-synthesis grafting method. The spiropyran unit is isomerized from a closed-ring nonionic state to an open-ring zwitterionic state under ultraviolet light irradiation, and the effective pore size of the COF membrane is reversibly switched by regulating the connectivity of the confined water clusters; it reverts to the closed-ring nonionic state under visible light or in the dark. The membrane operates in desalination mode under dark or visible light conditions, with an effective pore size of 0.55–0.60 nm; and in fractional crystallization mode under ultraviolet light, with an effective pore size of 0.66–0.72 nm.

2. The membrane according to claim 1, characterized in that, The lower photoresponsive COF layer is prepared by the following post-synthesis grafting method: (a) a parent COF membrane containing residual aldehyde groups is first synthesized by controlling the feed ratio of the trialdehyde monomer 2,4,6-tricarboxymethyl phloroglucinol to the triamino monomer tri(4-aminophenyl)amine, so that the trialdehyde monomer is in excess by 5–15 mol%; (b) an amino-containing spiropyran derivative is synthesized; (c) the spiropyran derivative is reacted with the residual aldehyde groups on the inner wall of the parent COF pores to form an imine bond.

3. The membrane according to claim 1, characterized in that, The upper negatively charged COF layer is prepared by polycondensation reaction of 2,5-diaminobenzenesulfonic acid and 1,3,5-tricarboxymethylresorcinol to form a TpPa-SO3H COF layer; 1,3,5-tricarboxymethylresorcinol reacts with amine monomers to form β-keto-enamine bonds.

4. The membrane according to claim 1, characterized in that, The parent COF of the lower photoresponsive COF layer is prepared by polycondensation reaction of tris(4-aminophenyl)amine and 2,4,6-tricarboxymethyl phloroglucinol to form the TAPA-TFP COF layer; 2,4,6-tricarboxymethyl phloroglucinol reacts with amine monomers to form β-keto-enamine bonds.

5. The membrane according to claim 1, characterized in that, By controlling the grafting density of spiropyran to 10–50 mol%, the effective pore size under both modes can be precisely controlled.

6. The membrane according to claim 1, characterized in that, The polydopamine molecular adhesive layer is formed on the surface of the upper COF layer by oxidative self-polymerization of dopamine, and has a thickness of 2–10 nm.

7. The membrane according to claim 1, characterized in that, The porous substrate of the membrane is a cross-linked polyimide porous membrane.

8. A method for preparing a biomimetic ion channel membrane as described in any one of claims 1-7, characterized in that, Includes the following steps: (1) Synthesis of aminospiropyran: Phenylhydrazine was condensed with 3-methyl-2-butanone to obtain 2,3,3-trimethyl-3H-indole; quaternized with iodomethane and treated with dilute alkali to obtain 2-methylene-1,3,3-trimethylindoline; salicylaldehyde was nitrated to obtain 5-nitrosalicylaldehyde; the two were condensed to obtain nitrospiropyran; and reduced to obtain aminospiropyran. (2) Preparation of TpPa-SO3H upper COF layer on cross-linked polyimide substrate: The substrate is immersed in a solution containing Pa-SO3H and Tp, with a molar ratio of Pa-SO3H to Tp of 1.5:1, and the reaction is carried out at 60–120℃ for 12–72 hours by solvothermal reaction. (3) Introducing the PDA layer: Immerse the obtained membrane in a Tris-HCl buffer solution containing dopamine and react aerobically at room temperature for 2–6 hours; (4) Preparation of TAPA-TFP parent COF layer containing residual aldehyde group: Dissolve TAPA and TFP in mesitylene / dioxane / acetic acid at a feed ratio of 5-15 mol% excess TFP, immerse the resulting membrane in the solution, and react with solvent at 60-90℃ for 12-24 hours. (5) Post-synthesis grafting: Immerse the obtained membrane in a solution containing SP-NH2 and react at room temperature to 60°C for 12–48 hours, then wash and dry.

9. An application of the biomimetic ion channel membrane as described in any one of claims 1-7 in seawater fractional crystallization, characterized in that, Includes the following steps: S1: Mode selection and light control separation: The membrane is placed in a nanofiltration device, and the feed solution is simulated seawater containing NaCl and Na2SO4; it operates in desalination mode under dark or visible light, with pressure driving the feed solution through the membrane; switching to ultraviolet light irradiation for fractional crystallization mode, the effective pore size of the membrane is expanded from 0.55–0.60 nm to 0.66–0.72 nm, the upper COF layer retains large-sized impurities, and the lower spiropyran isomerizes to the MC state, realizing Cl... - Selective permeability and SO4² - Highly efficient retention and collection of Cl-rich cells - The permeate; S2: Separative crystallization, the permeate is evaporated and crystallized to obtain NaCl crystals; S3: Mode recovery, the membrane is restored to desalination mode by visible light irradiation, and S1 and S2 are repeated; The ultraviolet light irradiation intensity is 5–50 mW / cm², the operating pressure is 5–30 bar, and the evaporation crystallization temperature is 50–90℃.