A low-energy granulation and rapid drying method for preparing particulate magnesium oxide
By using a mixture of coarse and fine magnesium oxide particles and a segmented drying process, the flowability and strength issues of magnesium oxide particles during spray drying were resolved, achieving low-energy and high-efficiency particle preparation, avoiding hollow particles and cracking, and maintaining product purity.
Patent Information
- Application Number
- CN202611319459.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-28
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies for preparing magnesium oxide particles suffer from poor flowability, easy dust generation, and difficulties in conveying and metering. Furthermore, the spray drying process can easily lead to hollow particles, bubbling, or cracking, and the energy consumption is high. It is difficult to improve particle strength and reduce energy consumption without introducing external binders.
A mixture of coarse and fine magnesium oxide is used, with the addition of ammonium salt-type organic dispersants. A segmented drying process is employed, consisting of vacuum flash degassing, low-temperature pulping, pressure spray pre-drying, short-time conditioning, and low-temperature final drying, to control the solid content and hydration process of the pulp, forming hydration junctions within the particles and avoiding particle defects caused by rapid drying.
It achieves the flowability and stability of particles with high solids content, reduces energy consumption, improves particle strength and structural integrity, reduces hollowness and cracking, and does not require external binders, thus maintaining product purity.
Smart Images

Figure REF-OBJ-1787897430692-000007 
Figure REF-OBJ-1787897430692-000008 
Figure REF-OBJ-1787897430692-000009
Abstract
Description
Technical Field
[0001] This invention relates to the technical field of inorganic non-metallic powder processing and spray granulation, and particularly to a low-energy granulation and rapid drying method for preparing granular magnesium oxide. Background Technology
[0002] Magnesium oxide (MgO) is widely used in refractory materials, ceramic materials, and thermally conductive fillers due to its high temperature resistance, good thermal conductivity, and high electrical insulation properties. In traditional applications, direct use of fine magnesium oxide powder presents problems such as poor flowability, easy dust generation, and difficulties in conveying and metering. Therefore, spray granulation is usually used to prepare particles with specific particle size and strength that meet the requirements of the working conditions.
[0003] Aqueous spray granulation is characterized by high production efficiency, uniform particle size, and ease of continuous production. However, MgO readily hydrates upon contact with water to form magnesium hydroxide, which not only increases slurry viscosity and deteriorates stability, but the hydration expansion effect also directly causes particle loosening or cracking. Increasing the solid content of the slurry can reduce water evaporation and lower drying energy consumption, but it further increases slurry viscosity, which is detrimental to slurry transport and atomization stability.
[0004] Existing technologies typically add dispersants, anti-hydration agents, or binders to optimize slurry properties and particle strength; however, some additives introduce impurities or require subsequent high-temperature calcination to remove them. When the spray drying rate is too high, a hard shell preferentially forms on the surface of the droplets, and continuous evaporation of internal moisture will cause the particles to become hollow, bubbly, or cracked; reducing the drying rate will lengthen the production cycle and increase energy consumption.
[0005] Therefore, there is a need to provide a method for preparing granular magnesium oxide that, without introducing exogenous binders or anti-hydration agents that affect product purity, balances high solids content and low viscosity of the slurry, controls magnesium oxide hydration, improves particle strength, reduces hollowness and cracking, and achieves rapid, low-energy drying. Summary of the Invention
[0006] To address the aforementioned problems, the present invention aims to provide a low-energy granulation and rapid drying method for preparing granular magnesium oxide, thereby overcoming the shortcomings of the prior art.
[0007] To achieve the above objectives, this invention provides a low-energy granulation and rapid drying method for preparing granular magnesium oxide, comprising the following steps: S1. Mixing coarse-grained magnesium oxide with a D50 of 8-25 μm and fine-grained magnesium oxide with a D50 of 0.3-2.0 μm at a dry basis mass ratio of 65:35-85:15; wherein the hydration conversion rate of the fine-grained magnesium oxide is more than twice that of the coarse-grained magnesium oxide; S2. Dissolving an ammonium salt type organic dispersant in deionized water at 3-10℃, adding it to the mixed powder obtained in S1 for dispersion, to obtain a magnesium oxide slurry with a solid content of 58-65 wt%; controlling the slurry temperature ≤12℃ during the slurry preparation process; S3. Performing vacuum flash evaporation to degas the magnesium oxide slurry, so that the water evaporation accounts for 0.3%-1.0% of the slurry mass before flash evaporation, and the slurry temperature after flash evaporation is more than 3℃ lower than before flash evaporation; S4. After the magnesium oxide mixed powder comes into contact with water, 60 Within min, the slurry after vacuum flash evaporation and degassing is pre-dried by pressure spray to obtain magnesium oxide pre-dried particles with a moisture content of 1.5~3.5 wt%; S5. The magnesium oxide pre-dried particles are conditioned at 40~60℃ in a sealed environment or with low ventilation for 2~12 min to limit hydration of the fine-grained magnesium oxide at the contact points inside the particles, and to control the moisture loss rate during the conditioning stage to not exceed 20%; S6. The conditioned magnesium oxide particles are finally dried at 65~85℃, and the resulting granular magnesium oxide has a moisture content ≤0.5 wt%.
[0008] Furthermore, the hydration activity test method is as follows: Weigh 10.0 g of the magnesium oxide to be tested, add it to 100.0 g of deionized water, stir at 300 r / min for 30 min at 25±0.5℃, and immediately perform solid-liquid separation after stirring. Dry the obtained solid at 105±2℃ to constant weight. Weigh the dried solid for thermogravimetric analysis. Under a nitrogen atmosphere, the temperature is increased from room temperature to 600℃ at a rate of 10℃ / min. The same batch of unhydrated magnesium oxide to be tested is used as a blank sample. The hydration conversion rate is calculated based on the amount of water lost by dehydroxylation of Mg(OH)2 in the range of 250~450℃ after blank correction. The hydration conversion rate refers to the percentage of MgO molars that have been converted to Mg(OH)2 after the hydration test to the initial molar amount of MgO used in the hydration test.
[0009] Furthermore, the coarse-grained magnesium oxide has a BET specific surface area of 0.2~2.0 m². 2 / g, the BET specific surface area of the fine-grained magnesium oxide is 3~15 m² / g. 2 / g.
[0010] Furthermore, the purity of both the coarse-grained magnesium oxide and the fine-grained magnesium oxide is not less than 99.5 wt%, and the D50 ratio between the two is 5~30.
[0011] Furthermore, the ammonium salt type organic dispersant includes one or more of ammonium polyacrylate, ammonium polymethacrylate and ammonium polycarboxylate, and its dosage is 0.03~0.12 wt% of the total dry basis mass of the magnesium oxide mixed powder.
[0012] Furthermore, in S5, the increase in Mg(OH)2 content in the conditioned particles relative to the unconditioned particles is 0.1~0.8 wt% of the dry magnesium oxide mass; the moisture loss rate in the conditioning stage is the percentage of the difference in the mass of free water contained in the particles before and after conditioning relative to the mass of free water contained in the particles before conditioning, under the same dry magnesium oxide mass basis.
[0013] Furthermore, the vacuum flash degassing in S3 is carried out for 1 to 8 minutes under an absolute pressure of 0.8 to 1.2 kPa. The temperature of the slurry after vacuum flash degassing is 3 to 9°C, and the solid content of the slurry is increased by 0.1% to 0.7% compared with that before flash degassing.
[0014] Furthermore, the S4 uses a parallel-flow pressure spray dryer with a feed temperature of 3~9℃, an inlet air temperature of 145~175℃, an outlet air temperature of 72~88℃, and a nozzle pressure of 4~9 MPa.
[0015] Furthermore, S6 employs a vibrating fluidized bed, a low-speed fluidized bed, or a shallow belt dryer for final drying, with a particle heating rate ≤10℃ / min, and utilizes the sensible heat of the outlet gas from the pressure spray dryer to heat the final dried gas.
[0016] Another object of the present invention is to provide a granular magnesium oxide prepared by the method according to any one of claims 1 to 8, comprising a granular skeleton formed of coarse-grained magnesium oxide, fine-grained magnesium oxide distributed in the gaps between the granular skeleton, and a Mg(OH)2-containing hydration bond formed at the contact area of the magnesium oxide particles; wherein the granular magnesium oxide has a D50 of 30 to 80 μm, a moisture content of ≤0.5 wt%, and a Mg(OH)2 content of 0.1 to 1.2 wt%.
[0017] The present invention has the following advantages:
[0018] 1. This invention uses two types of magnesium oxide, coarse and fine, with different hydration activities. The moisture content of the pre-dried particles after pressure spraying is controlled at 1.5~3.5 wt%. Subsequently, the particles are humidified for 2~12 minutes under sealed or low-ventilation conditions at 40~60℃, causing the residual moisture inside the particles to redistribute and preferentially remain in the interparticle gaps and contact areas. This promotes limited and localized hydration of the fine-grained magnesium oxide with higher hydration activity at the contact sites, generating a small amount of Mg(OH)2 in situ and forming Mg(OH)2-containing hydration bonds between adjacent magnesium oxide particles. Thus, this invention transforms magnesium oxide hydration from an unfavorable reaction in the pulping stage into a self-bonding reaction after spray granulation, improving particle strength and reducing particle breakage and pulverization. At the same time, it eliminates the need for curing with external binders or additional high-temperature treatment to achieve granulation strength, shortening the particle strengthening process and effectively reducing the corresponding energy consumption.
[0019] 2. This invention combines coarse and fine-grained magnesium oxide, with coarse-grained magnesium oxide accounting for 65% to 85% of the dry weight of the mixed powder, forming the main packing structure of the granulated particles during spray drying. The smaller-sized fine-grained magnesium oxide can be distributed in some of the voids between the coarse-grained magnesium oxide particles, thereby optimizing the particle size distribution of the mixed powder, which is beneficial to reducing the packing porosity and increasing the powder packing density. At the same time, ammonium salt-type organic dispersants are used to reduce powder agglomeration, and by feeding at a low temperature of 3 to 10°C, slurry temperature not exceeding 12°C, and limiting the contact time between magnesium oxide and water, excessive hydration and slurry thickening during the slurry preparation stage are suppressed. Under the condition of maintaining slurry fluidity and spray stability, the solid content of the slurry can be increased to 58 to 65 wt%, reducing the amount of water used for slurry preparation and the amount of water required for evaporation during spray drying, thereby reducing the drying load and energy consumption from the source.
[0020] 3. This invention employs vacuum flash degassing to allow air bubbles in the slurry to escape and evaporate 0.3% to 1.0% of the water content of the slurry before flash evaporation. Simultaneously, the slurry temperature is reduced by more than 3°C. This step integrates degassing, cooling, and moderate concentration into the same process, which can reduce the formation of internal pores after air bubbles enter the droplets, further inhibit magnesium oxide hydration before spraying through cooling, and reduce the moisture load of subsequent spray drying, thereby improving the density and structural uniformity of the pre-dried particles.
[0021] 4. This invention employs a segmented drying method combining pressure spray pre-drying, short-time conditioning, and low-temperature final drying: spray pre-drying quickly removes most of the moisture, the conditioning process utilizes residual moisture to homogenize the internal moisture of the particles and construct the hydration junction, and the final drying further reduces the moisture content of the particles to below 0.5 wt%. This method avoids premature surface hardening and internal vapor pressure concentration caused by rapid drying in one step, reduces particle hollowness, bubbling, and cracking, and utilizes the sensible heat of the gas exiting the spray dryer to heat the final drying gas, improving thermal energy utilization efficiency, thereby achieving rapid drying, low energy consumption, and particle structural integrity. Attached Figure Description
[0022] Figure 1 The preparation process flow diagram provided by the present invention. Detailed Implementation
[0023] The following embodiments are provided to better understand the present invention and are not limited to the preferred embodiments described. They do not constitute a limitation on the content and scope of protection of the present invention. Any product that is the same as or similar to the present invention, derived by any person under the guidance of the present invention or by combining the features of the present invention with other prior art, falls within the protection scope of the present invention.
[0024] For experiments not specifically described in the examples, the procedures or conditions should be followed according to the conventional experimental procedures described in the literature in this field. Reagents or instruments whose manufacturers are not specified are all commercially available conventional reagent products.
[0025] In this invention, solid content refers to the percentage of the total mass of the slurry containing the sum of the effective solids of magnesium oxide and dispersant; moisture content refers to the percentage of the mass loss of the sample when dried to constant weight at 105±2℃ relative to the mass of the sample before drying; samples used to determine the hydration increment are dried to constant weight at 105±2℃ before thermogravimetric analysis to eliminate the influence of free water. The moisture loss rate during the conditioning stage, as referred to in this invention, is the percentage of the difference in the mass of free water contained in the particles before and after conditioning, relative to the mass of free water contained in the particles before conditioning, under the same dry magnesium oxide mass basis, calculated according to formula (1):
[0026] (1)
[0027] In the formula, Rw represents the moisture loss rate during the conditioning stage; M0 represents the mass of free water contained in the particles before conditioning, based on the specified dry magnesium oxide mass; and M1 represents the mass of free water contained in the particles after conditioning, based on the same dry magnesium oxide mass. The free water mass of the particles before and after conditioning is calculated based on the moisture content measured after drying the particles to constant weight at 105±2℃.
[0028] The contact time between magnesium oxide and water, as referred to in this invention, begins when the first batch of magnesium oxide mixed powder is added to the aqueous dispersion medium and ends when the slurry begins to atomize from the pressure nozzle. Low-volume humidification refers to humidification performed while maintaining a humid and hot atmosphere within the device; in the following embodiments, the ventilation rate is controlled to be no higher than 0.2 times / min of the effective volume of the humidification device, and the relative humidity of the circulating gas is no less than 80%.
[0029] Magnesium oxide hydration activity determination: 10 g each of coarse-grained magnesium oxide and fine-grained magnesium oxide were weighed and added to 100.0 g of deionized water at 25±0.5℃. The mixture was stirred at 300 r / min for 30 min. Solid-liquid separation was performed immediately, and the solid was dried to constant weight at 105±2℃. The dried sample was weighed for thermogravimetric analysis. The temperature was increased from room temperature to 600℃ at 10℃ / min under a nitrogen atmosphere. The unhydrated magnesium oxide of the same batch was used as a blank sample. The mass of dehydroxylated water corresponding to Mg(OH)2 was calculated by taking the weight loss after blank correction in the range of 250-450℃. The magnesium oxide hydration conversion rate X was calculated according to formula (2):
[0030] (2)
[0031] in, The mass of water produced by the dehydroxylation of Mg(OH)2 in the sample. The initial mass of magnesium oxide used in the hydration test.
[0032] Humidity conditioning hydration increment measurement
[0033] Representative particle samples were taken before and after conditioned humidity, and sealed immediately. The samples were dried at 105±2℃ to constant weight and then tested by TG-DSC-MS. The weight loss caused by thermal decomposition of the dispersant was deducted from the pre-dried particles of the same batch as the baseline. The hydration increment Δw of conditioned humidity was calculated according to formula (3):
[0034] (3)
[0035] Where L1 and L0 are the mass losses attributable to water in the 250~450℃ range for samples before and after humidification, respectively, and m MgO This represents the dry basis mass of magnesium oxide in the sample. If necessary, micro-Raman spectroscopy should be used to test the primary particle contact area of the particle cross-section at 3650 cm⁻¹. -1 The stretching vibration peak of the hydroxyl group in the nearby Mg(OH)2 further confirmed the hydration junction.
[0036] Example 1
[0037] S1: Coarse-grained magnesium oxide with a purity of 99.72% and fine-grained magnesium oxide with a purity of 99.74% are selected. The coarse-grained magnesium oxide has a D50 of 15.0 μm and a BET specific surface area of 0.80 m². 2 / g, hydration conversion rate 1.4%; fine-grained magnesium oxide with a D50 of 0.90 μm and a BET specific surface area of 7.6 m². 2 / g, hydration conversion rate 4.5%. 7.50 kg of coarse-grained magnesium oxide and 2.50 kg of fine-grained magnesium oxide were weighed at a dry basis mass ratio of 75:25, and dry-mixed for 10 min to obtain magnesium oxide mixed powder.
[0038] S2: Dissolve 8.0 g of ammonium polyacrylate effective solids in deionized water at 6℃. The amount of ammonium polyacrylate is 0.08% of the dry weight of magnesium oxide. The amount of deionized water added should be based on the solid content of the resulting slurry reaching 62%. Add the magnesium oxide mixed powder in batches to the dispersion within 8 min, first stirring and wetting at 600 r / min, then dispersing at 1000 r / min for 12 min. Use jacket cooling to ensure that the maximum temperature of the slurry during the pulping process does not exceed 9.5℃.
[0039] S3: The slurry is fed into a vacuum flash tank with a weighing module and flashed and degassed for 4 minutes under an absolute pressure of 0.90 kPa, so that the amount of water evaporated accounts for 0.60% of the mass of the slurry before flashing, and the slurry temperature drops from 9.5℃ to 5.8℃.
[0040] S4: Spray atomization begins 38 minutes after the magnesium oxide mixed powder first comes into contact with water; a parallel flow pressure spray dryer is used with a feed temperature of 5.8℃, an inlet air temperature of 160℃, an outlet air temperature of 80℃, and a nozzle pressure of 6.5 MPa. The feed flow rate is adjusted to make the moisture content of the pre-dried particles 2.5%.
[0041] S5: Immediately send the pre-dried granules into a 50℃ closed slow turning device and turn them at 5 r / min for 6 min to redistribute the residual moisture inside the granules and promote the limited hydration of fine-grained magnesium oxide; the moisture loss rate during the conditioning stage is controlled to be below 10%.
[0042] S6: The moisture-conditioned particles are fed into a vibrating fluidized bed and finally dried at 75°C for 20 min, with a particle heating rate of 8°C / min; the final drying gas is heated by the sensible heat of the gas exiting the spray dryer through a gas-to-gas heat exchanger to obtain the granular magnesium oxide of Example 1.
[0043] Example 2
[0044] The preparation method in this embodiment is the same as that in Example 1, except that the following conditions are used:
[0045] The D50 of coarse and fine-grained magnesium oxide were 8.5 μm and 1.7 μm, respectively, and their BET specific surface areas were 1.8 m² and 1.8 μm, respectively. 2 / g and 4.0 m 2 / g, with hydration conversion rates of 1.9% and 4.1% respectively, and a dry basis mass ratio of 65:35; ammonium polymethyl methacrylate was used as the dispersant, with an effective solids content of 0.12% of the dry basis mass of magnesium oxide, an initial deionized water temperature of 3℃, a slurry solid content of 58.0%, a maximum slurry preparation temperature of 7.0℃, and a time from the first contact of the powder with water to the start of atomization of 50 min; the absolute pressure of vacuum flash evaporation was 0.80 kPa, the flash evaporation time was 6 min, the water evaporation rate was 1.0% of the slurry mass before flash evaporation, and the slurry temperature decreased from 7.0℃ to 3.5℃; the spray feed temperature was 3.5℃, the inlet air temperature was 145℃, the outlet air temperature was 72℃, the nozzle pressure was 4.0 MPa, and the moisture content of the pre-dried particles was 3.5%; the pre-dried particles were conditioned at 40℃ with low ventilation for 12 days. For min, the relative humidity of the circulating gas is maintained above 80%, and the moisture loss rate during the conditioning stage is controlled below 20%; then, a shallow belt dryer is used for final drying at 65℃ for 40 min, with a particle heating rate of 5℃ / min.
[0046] Example 3
[0047] The preparation method in this embodiment is the same as that in Example 1, except that the following conditions are used:
[0048] The D50 of coarse and fine-grained magnesium oxide were 24.0 μm and 0.80 μm, respectively, and their BET specific surface areas were 0.35 m² and 0.80 μm, respectively. 2 / g and 6.5 m 2 / g, with hydration conversion rates of 0.8% and 2.6% respectively, and a dry basis mass ratio of 85:15; ammonium polyacrylate was used as the dispersant, with an effective solids content of 0.03% of the dry basis mass of magnesium oxide, an initial deionized water temperature of 10℃, a slurry solid content of 65.0%, a maximum slurry preparation temperature of 12℃, and a time from the first contact of the powder with water to the start of atomization of 30 min; vacuum flash evaporation absolute pressure of 1.15 kPa, flash evaporation time of 1.5 min, water evaporation of 0.30% of the slurry mass before flash evaporation, and slurry temperature reduced from 12℃ to 9℃; spray feed temperature of 9℃, inlet air temperature of 175℃, outlet air temperature of 88℃, nozzle pressure of 9.0 MPa, and pre-dried particle moisture content of 1.5%; pre-dried particles were conditioned at 60℃ in a sealed environment for 2 min, with moisture loss controlled below 5% during the conditioning stage; subsequently, they were finally dried in a low-speed fluidized bed at 85℃ for 12 minutes. The particle heating rate is 10℃ / min.
[0049] Example 4
[0050] The D50 is 18.0 μm and the BET specific surface area is 0.70 m². 2 37.5 kg of coarse-grained magnesium oxide with a hydration conversion rate of 1.1% and a D50 of 1.2 μm and a BET specific surface area of 8.2 m² was obtained. 2 A mixture of 12.5 kg of fine-grained magnesium oxide (with a hydration conversion rate of 3.7%) and 1 g of magnesium oxide. The purity of both types of magnesium oxide is not less than 99.5%.
[0051] The effective solids of polycarboxylic acid ammonium, equivalent to 0.06% of the dry weight of magnesium oxide, were dissolved in deionized water at 5°C and added to the mixed powder to obtain a slurry with a solid content of 63.0%. The maximum slurry preparation temperature was 10°C, and the time from the first contact of the powder with water to the start of atomization was 45 min.
[0052] The slurry was vacuum flashed for 5 min under an absolute pressure of 0.90 kPa, and the water evaporation was 0.70% of the slurry mass before flashing, and the slurry temperature decreased by 4℃. Subsequently, it was pre-dried by co-current pressure spray at an inlet air temperature of 160℃, an outlet air temperature of 82℃, and a nozzle pressure of 7.0 MPa to obtain pre-dried particles with a moisture content of 2.2%.
[0053] The pre-dried particles were conditioned at 52°C with low ventilation for 7 min, and the moisture loss rate during the conditioning stage was controlled to be below 12%. Subsequently, they were finally dried in a vibrating fluidized bed at 78°C for 18 min, with a particle heating rate of 8°C / min. The final drying gas was heated by the sensible heat of the spray drying outlet gas to obtain the granular magnesium oxide of Example 4.
[0054] Comparative Example 1
[0055] The pulping, vacuum flash evaporation, and spray pre-drying were carried out according to Example 1; S5 was omitted, and the pre-dried particles with a moisture content of 2.5% were directly dried under the conditions of S6 in Example 1, i.e., no humidification was performed. The remaining conditions were the same as in Example 1.
[0056] Comparative Example 2
[0057] Pre-dried granules were prepared according to Example 1; S5 was changed to humidifying by introducing dry air at 50°C for 6 min, with an air exchange rate of 2.0 times / min of the effective volume of the humidification device, and the moisture loss rate during the humidification stage was not controlled; the remaining conditions were the same as in Example 1.
[0058] Comparative Example 3
[0059] The high hydration activity fine-grained magnesium oxide in Example 1 was replaced with fine-grained magnesium oxide with a D50 of 0.90 μm but a hydration conversion rate that was only 1.5 times that of coarse-grained magnesium oxide, while keeping the mass ratio of coarse and fine-grained magnesium oxide, the solid content of the slurry and other process conditions unchanged.
[0060] Comparative Example 4
[0061] After preparing the slurry according to Example 1, step S3 was omitted, and the slurry was directly subjected to pressure spray pre-drying; the moisture content of the pre-dried particles was kept at 2.5% by adjusting the feed flow rate, and the other conditions were the same as in Example 1.
[0062] Comparative Example 5
[0063] Using the same magnesium oxide mixed powder as in Example 1, the solid content of the slurry was adjusted to 50%, and the slurry was prepared at 25°C without vacuum flash evaporation or humidification. A parallel flow pressure spray dryer was used to perform single-stage spray drying at an inlet air temperature of 190°C, an outlet air temperature of 100°C, and a nozzle pressure of 6.5 MPa until the moisture content of the resulting particles was no higher than 0.5%.
[0064] Performance testing
[0065] Examples 1-4 and Comparative Examples 1-5 were prepared in three independent batches each. Samples from each batch were taken and tested at the specified process nodes using the same method. The results in the table are expressed as the mean ± standard deviation of the three independent batches.
[0066] Table A. Detection Objects, Sampling Points, and Detection Items
[0067]
[0068] (1) Solid content and apparent viscosity of slurry
[0069] Representative samples were taken from each group of slurries before spraying. The solid content of the slurries was determined by drying at 105±2℃ to constant weight, calculated as the percentage of solids mass after drying to the mass of slurry before drying. Apparent viscosity was determined using a rotational rheometer: the slurry was kept at 25±0.5℃ for 100 s... -1 The sample was subjected to a pre-shear for 60 s, and then maintained at that shear rate for another 30 s. The average apparent viscosity during the steady-state phase was recorded. Each batch of samples was measured in triplicate. The test results are summarized in Table 1.
[0070] (2) Hydration increment during pulping stage (Mg(OH)2)
[0071] Using the Mg(OH)₂ content in the magnesium oxide mixed powder before pulping as the initial value, samples were taken before the start of spraying. Solid-liquid separation was immediately performed, and the samples were dried to constant weight at 105±2℃ before TG-DSC-MS analysis. The Mg(OH)₂ content was calculated based on the water loss attributable to the Mg(OH)₂ dehydroxylation reaction within the temperature range of 250–450℃. The difference in Mg(OH)₂ content between the sample before spraying and the mixed powder before pulping was taken as the Mg(OH)₂ increment during the pulping stage, expressed as a percentage of the dry mass of magnesium oxide. The test results are summarized in Table 1.
[0072] (3) Gas content of slurry and vacuum flash evaporation effect
[0073] Samples were taken before vacuum flash evaporation and before the slurry entered the pressure spraying process. The measured density ρ1 of the slurry containing gas was determined using a constant volume density cup; the density ρ0 of the slurry with the same formulation was measured after thorough vacuum degassing. The gas content of the slurry, A = (ρ0 - ρ1) / ρ0 × 100%. For Comparative Examples 4 and 5, which did not undergo vacuum flash evaporation, the gas content was recorded after slurry preparation and before entering the pressure spraying process, respectively. The test results are summarized in Table 1.
[0074] (4) Moisture content of pre-dried particles and Mg(OH)2 increment after pre-drying
[0075] Representative particle samples were taken from the pressure spray pre-drying outlet and the final drying inlet, and sealed immediately. Moisture content was determined using the constant weight method at 105±2℃. For Examples 1-4 and Comparative Examples 2-4, the moisture loss rate was calculated based on the free water mass of the particles before and after conditioning; Comparative Example 1 was not conditioned, and its moisture loss rate was not evaluated. The increase in Mg(OH)2 after pre-drying was the difference in Mg(OH)2 content between the final drying inlet sample and the pressure spray pre-drying outlet sample. The detection value of Comparative Example 1 represents the increase in pre-dried particles during the direct transport from the pressure spray pre-drying outlet to the final drying inlet; Comparative Example 5 did not have an independent post-pre-drying stage, and the relevant indicators are not applicable. The relevant test results are summarized in Table 2.
[0076] (5) Finished particle D50, moisture content, structure, single particle crushing load and wear pulverization rate
[0077] The moisture content of the finished product was determined by drying at 105±2℃ to constant weight. The particle size distribution (D50) was determined using a laser particle size analyzer with dry injection, and each batch of samples was measured in triplicate.
[0078] The finished particles were impregnated with low-viscosity resin and cured, then subjected to cross-sectional grinding and argon ion polishing before being observed under a scanning electron microscope. At least 300 particles were randomly selected from each batch. Particles with an internal continuous cavity equivalent diameter greater than 20% of the particle's equivalent diameter were classified as hollow particles; particles with cracks extending from the outer surface inwards and with a crack length greater than 20% of the particle's equivalent diameter were classified as cracked particles.
[0079] Finished particles of 45–75 μm were sieved and subjected to a microparticle compression tester at a loading rate of 0.2 mN / s until the particles fractured. At least 100 particles from each batch were randomly tested, and the median fracture load was recorded. Separately, 20 g of particles of the same size were placed in a 500 mL standard drum and rotated at 60 r / min for 10 min. After the test, the particles were sieved using a 45 μm sieve, and the percentage increase in mass of particles smaller than 45 μm relative to the initial mass of the sample was taken as the wear pulverization rate. The relevant test results are summarized in Table 3.
[0080] (6) Comprehensive energy consumption per unit product
[0081] After the equipment was running stably, the energy inputs of the slurry cooling system, vacuum flash evaporation system, spray drying heating and air supply system, humidity conditioning device, and final drying device were measured. Electrical energy was measured using an electricity meter; thermal energy was calculated based on the heat carrier flow rate and inlet / outlet enthalpy difference, converted to 1 kWh = 3.6 MJ. After deducting the no-load energy consumption during the same operating time, the comprehensive energy consumption per unit product was calculated based on the finished particle mass. The relevant test results are summarized in Table 3.
[0082] (7) Purity and impurity content of finished product
[0083] The MgO content of the finished granules was determined after calcination under specified conditions. The contents of Na, K, Ca, Si, and Al were determined by ICP-OES, and their total amounts were calculated. Comparative Examples 1, 2, 4, and 5 used the same magnesium oxide raw material as Example 1; Comparative Example 3 was modified by replacing the magnesium oxide with fine-grained magnesium oxide for the purpose of comparison; Examples 2-4 used their respective specified magnesium oxide raw materials.
[0084] (8) Loose packing density, tapped density and Carr index
[0085] The loose density ρb and tapped density ρt of the finished particles were measured respectively, and the Carr index was calculated according to CI=(ρt-ρb) / ρt×100%.
[0086] Table 1. Test results of slurry and flash evaporation process
[0087]
[0088] Note: The pre-spray gas content of Examples 1-4 and Comparative Examples 1-3 is the gas content measured after vacuum flash treatment and before entering the pressure spray process; Comparative Examples 4 and 5 did not undergo vacuum flash treatment, and their pre-spray gas content is the gas content measured directly after pulping and before entering the pressure spray process.
[0089] Table 2 Results of water retention and hydration tests after pre-drying
[0090]
[0091] Table 3. Test results of finished product structure, strength, moisture content and energy consumption.
[0092]
[0093] Table 4. Results of finished product purity and packing / flow properties tests
[0094]
[0095] Analysis of test results
[0096] The test data in Tables 1 and 3 show that the solid content of the magnesium oxide slurry prepared in Examples 1-4 is 58.0%~65.0%, and the solid content is 100s. -1 Under shear conditions, the apparent viscosity is 560~890 mPa·s, and the increase in Mg(OH)2 during the pulping stage is only 0.05%~0.13%, indicating that the low-temperature pulping-dispersion system of the present invention can achieve high solid content while effectively inhibiting premature hydration of magnesium oxide during the pulping stage; the corresponding finished particle moisture content is 0.26%~0.44%, and the D50 is 39.6~68.4 μm, all within the product index range defined by the present invention.
[0097] (1) Effects of conditioning process and conditioning atmosphere on hydration increment and particle mechanical properties
[0098] Combining the hydration and moisture loss data after pre-drying in Table 2 with the finished product performance in Table 3, it can be seen that: Example 1 uses a closed-loop humidification process, with a moisture loss rate of 6.8±0.7% during the humidification stage. The increase in Mg(OH)2 after pre-drying reaches 0.46±0.04%, the median breakage load of the finished product is 23.8±1.2 mN, and the wear pulverization rate is 1.7±0.2%. Comparative Example 1 has no moisture loss rate during the humidification stage. Its 0.02±0.01% increase in Mg(OH)2 only comes from the weak water vapor effect in the environment during particle conveying. The corresponding median breakage load of the finished product is only 12.4±0.7 mN, and the wear pulverization rate is as high as 5.6±0.4%. Compared with Comparative Example 1, the median breakage load of Example 1 increases by 91.9%, and the wear pulverization rate decreases by 69.6%. This confirms that adding a short-term closed / low-exchange humidification process after spray pre-drying can promote limited in-situ hydration of fine magnesium oxide particles, constructing a hydration junction inside the particles, effectively improving particle strength and reducing the wear pulverization rate. Comparative Example 2 used high-flow-rate dry air with high ventilation for humidity conditioning. As shown in Table 2, the moisture loss rate during the humidity conditioning stage was as high as 72.4±3.1%, and the particles lacked the residual moisture required for the hydration reaction. The increase in Mg(OH)2 was only 0.09±0.02%. Further, combined with the data in Table 3, the median crushing load of the finished product was only 14.1±0.8 mN, and the wear and pulverization rate increased to 4.8±0.4%. This confirms that a closed or low-ventilation mode must be adopted during the humidity conditioning stage to control moisture loss in order to retain the residual moisture inside the particles for limited hydration and achieve particle self-reinforcement.
[0099] (2) Effect of differences in hydration activity between coarse and fine-grained magnesium oxide on hydration increment and particle strength
[0100] In Example 1, the hydration conversion rate of fine-grained magnesium oxide was 3.2 times that of coarse-grained magnesium oxide. In Comparative Example 3, under the condition that the other processes remained unchanged, the hydration conversion rate of fine-grained magnesium oxide was reduced to 1.5 times that of coarse-grained magnesium oxide. As shown in Table 2, the increase in Mg(OH)₂ after pre-drying in Example 1 was 0.46±0.04%, while in Comparative Example 3 it was only 0.18±0.03%. Combined with Table 3, the median crushing load of the finished product in Example 1 was 23.8±1.2 mN, and the wear pulverization rate was 1.7±0.2%. In Comparative Example 3, the median crushing load decreased to 16.2±0.9 mN, and the wear pulverization rate increased to 3.5±0.3%.
[0101] The above results indicate that only by ensuring that the hydration conversion rate of fine-grained magnesium oxide is more than twice that of coarse-grained magnesium oxide can a sufficient amount of magnesium hydroxide hydration junction be generated under short-term humidification conditions, thereby effectively improving the mechanical strength of the granulated particles.
[0102] (3) Effect of vacuum flash degassing on the gas content of slurry and the inhibition of hollow and cracked defects in finished products
[0103] As shown in Table 1, after vacuum flash evaporation, the gas content of the slurry in Example 1 decreased from 3.2±0.2% before flash evaporation to 0.46±0.06% after flash evaporation; in Comparative Example 4, vacuum flash evaporation was omitted and the gas content of the slurry before spraying remained at 3.1±0.2%.
[0104] Based on the finished product test results in Table 3, the hollow rate of the finished product in Example 1 was 5.3±0.8%, and the cracking rate was 2.7±0.5%; the hollow rate of the finished product in Comparative Example 4 was 13.7±1.4%, and the cracking rate was 7.6±0.9%. Under the same other process conditions, omitting vacuum flash degassing resulted in a relative increase of 158.5% in particle hollow rate and a relative increase of 181.5% in cracking rate. This demonstrates that vacuum flash degassing can effectively remove air bubbles entrained in the slurry, reduce the source of air bubbles inside the droplets, and significantly reduce the defects of hollow and cracked particles in the finished product.
[0105] (4) Comparison of the energy-saving effect of the complete combined process of the present invention with that of the particle structure
[0106] Based on 1 kg of dry magnesium oxide material, the water content was calculated as follows: Example 1 had a slurry solid content of 62%, and the water introduced during slurry preparation was approximately 0.613 kg; Comparative Example 5 used traditional single-stage spray drying, with a slurry solid content of 50%, and the water introduced during slurry preparation was approximately 1 kg. According to the comprehensive energy consumption data per unit product in Table 3, the comprehensive energy consumption of Example 1 was 0.95±0.04 kWh / kg, while that of Comparative Example 5 was 1.55±0.06 kWh / kg, representing a relative reduction of approximately 38.7% in the comprehensive energy consumption per unit product. Furthermore, Example 1 had a void ratio of 5.3±0.8% and a cracking rate of 2.7±0.5%, significantly lower than the void ratio of 21.8±1.7% and the cracking rate of 12.4±1.2% in Comparative Example 5.
[0107] It should be noted that Comparative Example 5 is a traditional single-stage direct spray drying process, which does not have a pre-drying-conditioning-final drying stage. Therefore, the relevant indicators for the post-pre-drying stage in Table 2 are not applicable to this group. This comparison reflects the comprehensive gain effect of the entire process of this invention. The changes in energy consumption and performance are the result of multiple steps working together and cannot be attributed to a single process.
[0108] (5) Finished product purity, bulking and flow properties
[0109] As shown in Table 4, after calcination, the MgO mass fraction of Examples 1-4 was 99.68%-99.76%, and the total impurity (Na+K+Ca+Si+Al) content was 980-1320ppm, thus maintaining the high purity of the product.
[0110] The loose bulk density of Example 1 was 1.08 ± 0.03 g / cm³. 3 Tap density: 1.25 ± 0.03 g / cm³ 3 The Carr index was 13.6±1.1%; while the loose density of the traditional process in Comparative Example 5 was only 0.76±0.03 g / cm³. 3 Tap density: 1.07 ± 0.03 g / cm³ 3 The Carr index is as high as 29.0±1.8%. It can be seen that the particles prepared by the present invention have higher loose packing and tap density and lower Carr index, and the powder flow and packing properties are significantly better than those of the traditional single-stage spray granulation process.
[0111] In summary, by combining coarse and fine magnesium oxide particle sizes with hydration activity, low-temperature high-solids pulping, vacuum flash degassing, pressure spray pre-drying, closed / low-exchange humidity conditioning for limited hydration, low-temperature final drying, and waste heat recovery from spray exhaust gas, premature hydration of magnesium oxide during the pulping stage can be suppressed, and the residual moisture inside the pre-dried particles can be used to achieve in-situ self-bonding of the particles. The final product has low moisture content, low hollowness, low cracking rate, low abrasion pulverization rate, high particle crushing strength, and good powder flowability, while significantly reducing the overall energy consumption per unit product.
[0112] Obviously, the above embodiments are merely illustrative examples for clear explanation and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations here. However, obvious variations or modifications derived therefrom are still within the scope of protection of this invention.
Claims
1. A low-energy granulation and rapid drying method for preparing granular magnesium oxide, characterized in that, Includes the following steps: S1. Coarse-grained magnesium oxide with a D50 of 8~25 μm and fine-grained magnesium oxide with a D50 of 0.3~2.0 μm are mixed at a dry basis mass ratio of 65:35~85:15; wherein the hydration conversion rate of the fine-grained magnesium oxide is more than twice that of the coarse-grained magnesium oxide. S2. Dissolve the ammonium salt type organic dispersant in deionized water at 3~10℃, add the mixed powder obtained in S1 and disperse it to obtain a magnesium oxide slurry with a solid content of 58~65 wt%; control the slurry temperature ≤12℃ during the slurry preparation process; S3. The magnesium oxide slurry is subjected to vacuum flash evaporation to degas it, so that the amount of water evaporated accounts for 0.3~1.0% of the mass of the slurry before flash evaporation, and the temperature of the slurry after flash evaporation is more than 3°C lower than that before flash evaporation; S4. Within 60 min after the magnesium oxide mixed powder comes into contact with water, the slurry after vacuum flash evaporation and degassing is pre-dried by pressure spray to obtain magnesium oxide pre-dried particles with a water content of 1.5~3.5 wt%. S5. The pre-dried magnesium oxide particles are conditioned at 40~60℃ in a sealed environment or with low ventilation for 2~12 minutes to allow limited hydration of the fine-grained magnesium oxide at the contact points inside the particles, and to control the moisture loss rate during the conditioning stage to not exceed 20%; S6. The conditioned magnesium oxide particles are then dried at 65~85℃ to obtain magnesium oxide particles with a moisture content ≤0.5wt%.
2. The method for preparing granulated magnesium oxide with low energy consumption through granulation and rapid drying according to claim 1, characterized in that, The hydration activity test method is as follows: Weigh 10.0 g of magnesium oxide to be tested, add it to 100.0 g of deionized water, stir at 300 r / min for 30 min at 25±0.5℃, and immediately perform solid-liquid separation after stirring. Dry the obtained solid at 105±2℃ to constant weight. Weigh the dried solid for thermogravimetric analysis. Under nitrogen atmosphere, the temperature is increased from room temperature to 600℃ at a rate of 10℃ / min. The same batch of unhydrated magnesium oxide to be tested is used as a blank sample. The hydration conversion rate is calculated based on the amount of water lost by dehydroxylation of Mg(OH)2 in the range of 250~450℃ after blank correction. The hydration conversion rate refers to the percentage of MgO molar amount that has been converted to Mg(OH)2 after the hydration test to the initial molar amount of MgO used in the hydration test.
3. The low-energy granulation and rapid drying method for preparing granular magnesium oxide according to claim 2, characterized in that, The coarse-grained magnesium oxide has a BET specific surface area of 0.2~2.0 m². 2 / g, the BET specific surface area of the fine-grained magnesium oxide is 3~15 m² / g. 2 / g.
4. The low-energy granulation and rapid drying method for preparing granular magnesium oxide according to claim 3, characterized in that, The purity of both the coarse-grained magnesium oxide and the fine-grained magnesium oxide is not less than 99.5 wt%, and the D50 ratio between the two is 5~30.
5. The low-energy granulation and rapid drying method for preparing granular magnesium oxide according to claim 1, characterized in that, The ammonium salt type organic dispersant includes one or more of ammonium polyacrylate, ammonium polymethacrylate and ammonium polycarboxylate, and its dosage is 0.03~0.12 wt% of the total dry basis mass of the magnesium oxide mixed powder.
6. The method for preparing granulated magnesium oxide with low energy consumption through granulation and rapid drying according to claim 1, characterized in that, In S5, the increase in Mg(OH)2 content in the granules after conditioning relative to the amount before conditioning is 0.1~0.8 wt% of the dry basis mass of magnesium oxide; the moisture loss rate during the conditioning stage is the percentage of the difference in the mass of free water contained in the granules before and after conditioning relative to the mass of free water contained in the granules before conditioning, under the same dry basis mass of magnesium oxide.
7. The method for preparing granulated magnesium oxide with low energy consumption through granulation and rapid drying according to claim 1, characterized in that, Vacuum flash degassing in S3 is carried out for 1 to 8 minutes under an absolute pressure of 0.8 to 1.2 kPa. The temperature of the slurry after vacuum flash degassing is 3 to 9°C, and the solid content of the slurry is increased by 0.1% to 0.7% compared with that before flash degassing.
8. The method for preparing granulated magnesium oxide with low energy consumption through granulation and rapid drying according to claim 1, characterized in that, The S4 uses a parallel-flow pressure spray dryer with a feed temperature of 3~9℃, an inlet air temperature of 145~175℃, an outlet air temperature of 72~88℃, and a nozzle pressure of 4~9 MPa.
9. The preparation method according to claim 7, characterized in that, S6 uses a vibrating fluidized bed, low-speed fluidized bed, or shallow belt dryer for final drying, with a particle heating rate ≤10℃ / min, and utilizes the sensible heat of the outlet gas of the pressure spray dryer to heat the final drying gas.
10. A granular magnesium oxide prepared by the method according to any one of claims 1 to 9, characterized in that, It includes a particle skeleton formed by coarse-grained magnesium oxide, fine-grained magnesium oxide distributed in the gaps between the particle skeleton, and Mg(OH)2-containing hydration bonding parts formed at the contact parts of magnesium oxide particles; the particle magnesium oxide has a D50 of 30~80 μm, a moisture content of ≤0.5wt%, and a Mg(OH)2 content of 0.1~1.2 wt%.