An apparatus and method for producing nano-cellulose-reinforced resin

By using integrated production equipment and methods, the shortcomings in the industrialization of nanocellulose-reinforced resins have been solved, and the preparation of nanocellulose-reinforced resins with high mechanical strength and stability has been achieved. These resins are compatible with a variety of resins, meet the production needs of lightweight composite materials for new energy vehicles, and realize stable industrial mass production.

CN123102258APending Publication Date: 2026-11-17JIANGSU JIESI NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611145647.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-30
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies for preparing nanocellulose-reinforced resins have limitations in industrialization. They cannot achieve optimized modification of nanocellulose, resulting in poor hygrothermal stability, large dispersion in mechanical properties, inability to adapt to various resin systems, and inability to achieve stable industrial mass production.

Method used

A production apparatus and method for nanocellulose-reinforced resin is provided, including a pretreatment device, a nanocellulose modification device, a purification device, a gradient dispersion device, and a composite molding device. The devices are connected by an integrated pipeline to realize the pretreatment, oxidative esterification modification, purification, and gradient dispersion of nanocellulose raw materials, avoiding the problems of agglomeration and incomplete modification. This enables the production of various resins and stable industrial mass production.

Benefits of technology

It achieves high mechanical strength and stability of nanocellulose-reinforced resin, is compatible with the production of various resins, ensures the continuity and stability of the production process, meets the stringent working conditions of lightweight composite materials for new energy vehicles, and realizes industrial-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102258A_ABST
    Figure CN123102258A_ABST
Patent Text Reader

Abstract

This application provides a production apparatus for nanocellulose-reinforced resin, including a pretreatment device, a nanocellulose modification device, a purification device, a gradient dispersion device, and a composite molding device. The pretreatment device includes a first inlet, a pretreatment mechanism, and a first outlet connected in sequence. The nanocellulose modification device includes a reaction chamber, a liquid inlet pipe, a second inlet, and a second outlet. The outlet end of the liquid inlet pipe is located inside the reaction chamber, which is connected to both the second inlet and the second outlet. The second inlet and the first outlet are connected via a powder conveying pipe. The purification device includes a third inlet, a solvent replacement mechanism, and a third outlet connected in sequence. The third inlet and the second outlet are connected via a first slurry conveying pipe. The gradient dispersion device includes a fourth inlet, a stirring mechanism, a homogenizing mechanism, a grinding mechanism, and a fourth outlet connected in sequence. The fourth inlet and the third outlet are connected via a second slurry conveying pipe.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of composite material production technology, specifically to an apparatus and method for producing nano-cellulose reinforced resin. Background Technology

[0002] Nanocellulose is a novel bio-based nanomaterial with ultra-high strength, high modulus, lightweight, and biodegradability. Compared with traditional glass fiber and carbon fiber reinforced materials, it has significant advantages such as low density, good toughness, strong interfacial compatibility, and green and low carbon emissions. It is a core strategic alternative material for the lightweight upgrading of new energy vehicles and the reduction of carbon emissions. As new energy vehicles rapidly iterate towards longer range, higher safety, lighter weight, and longer lifespan, traditional general-purpose resins and ordinary glass fiber modified resins can no longer meet the stringent operating conditions of battery casings under high and low temperature alternation, high humidity, and high load. High-end nanocellulose reinforced resins have become the core development direction of automotive composite materials.

[0003] Existing technologies for preparing nanocellulose-reinforced resins have clear shortcomings and technical defects for industrialization: First, existing production lines are mostly designed for the extraction and purification of general-purpose cellulose powders, possessing only the function of primary raw material preparation and unable to optimize and modify nanocellulose; Second, existing modification processes generally adopt high-temperature esterification and a single mechanical stirring dispersion mode, which easily leads to the thermal degradation of nanocellulose and severe fiber agglomeration, resulting in composite materials with poor hygrothermal stability and large dispersion of mechanical properties, failing to meet the consistency standards of automotive parts; Third, existing technologies can only be adapted to a single resin system, unable to flexibly switch to the production of mainstream automotive products, resulting in extremely poor industrial adaptability; Fourth, existing technologies are all still in the laboratory pilot research stage, with fragmented processes and unfixable parameters, making it impossible to achieve stable industrial mass production. Summary of the Invention

[0004] To address the aforementioned problems in the prior art, this application provides an apparatus and method for producing nano-cellulose-reinforced resin. The specific technical solution is as follows: On one hand, this application provides an apparatus for producing nano-cellulose-reinforced resin, comprising: The pretreatment equipment includes a first inlet, a pretreatment mechanism, and a first outlet connected in sequence, wherein the first inlet is used to feed nanocellulose into the pretreatment mechanism. Nanocellulose modification equipment includes a reaction chamber, a liquid inlet pipeline, a second feed port and a second discharge port. The liquid outlet of the liquid inlet pipeline is located inside the reaction chamber. The reaction chamber is connected to the second feed port and the second discharge port respectively. The second feed port and the second discharge port are equipped with on / off valves. The second feed port and the first discharge port are connected through a powder conveying pipeline. The purification equipment includes a third inlet, a solvent replacement mechanism, and a third outlet connected in sequence, wherein the third inlet and the second outlet are connected through a first slurry conveying pipeline; A gradient dispersion device includes a fourth feed inlet, a stirring mechanism, a homogenizing mechanism, a grinding mechanism, and a fourth discharge outlet connected in sequence. The fourth feed inlet and the third discharge outlet are connected through a second slurry conveying pipeline. A composite molding equipment includes a fifth feed inlet, a resin conveying pipeline, a mixing mechanism, and a molding mechanism. The mixing mechanism is connected to the fifth feed inlet, the resin conveying pipeline, and the molding mechanism, respectively. The fifth feed inlet is connected to the fourth discharge outlet through a third slurry conveying pipeline.

[0005] In a possible implementation, the production apparatus further includes a recycling device, which is connected via recycling pipelines to the pretreatment device, the nanocellulose modification device, the purification device, the gradient dispersion device, and the composite molding device, respectively.

[0006] In a possible implementation, the pretreatment equipment includes a screening mechanism, a drying mechanism, and a weighing and feeding mechanism connected in sequence. The top end of the screening mechanism is connected to the first feed inlet, and the bottom end of the weighing and feeding mechanism is connected to the first discharge outlet.

[0007] In a possible implementation, the nanocellulose modification device further includes a constant flow dripping component, a stirring component, and a pH sensor. The constant flow dripping component is located at the liquid outlet, the stirring component is used to stir the slurry in the reaction chamber, and the pH sensor is used to detect the pH of the slurry in the reaction chamber.

[0008] In a possible implementation, the nanocellulose modification device further includes an air inlet pipe connected to the reaction chamber; the reaction chamber is provided with an outer shell covered by a water-cooling jacket.

[0009] In a possible implementation, the purification device further includes a cleaning solution pipeline, and the solvent replacement mechanism includes multiple solvent replacement chambers connected in series, each of which is connected to the cleaning solution pipeline.

[0010] In a possible implementation, the rotational speed gradient of the stirring mechanism, the homogenizing mechanism, and the grinding mechanism increases.

[0011] In a possible implementation, the composite molding equipment further includes a detection mechanism connected to both the molding mechanism and the recovery pipeline. The detection mechanism is capable of detecting and classifying the samples output by the molding mechanism.

[0012] In a possible implementation, the powder conveying pipeline is equipped with a negative pressure conveying mechanism, and the first slurry conveying pipeline, the second slurry conveying pipeline, and the third slurry conveying pipeline are equipped with a high pressure conveying mechanism.

[0013] On the other hand, this application provides a method for producing nano-cellulose reinforced resin, comprising: S1: Nanocellulose is fed into the pretreatment unit through the first feed port to obtain pretreated cellulose; S2: The pretreated cellulose enters the reaction chamber through the first outlet, the powder conveying pipeline and the second inlet. Oxidizing agent and esterifying agent are added dropwise into the reaction chamber through the liquid outlet of the liquid inlet pipeline to carry out modification treatment and obtain modified nanocellulose slurry. S3: The modified nanocellulose slurry enters the solvent replacement mechanism through the second outlet, the first slurry conveying pipeline and the third inlet to purify the modified nanocellulose slurry and obtain purified slurry; S4: The purified slurry enters the stirring mechanism through the third outlet, the second slurry conveying pipeline and the fourth inlet. The purified slurry is then gradient-dispersed by the stirring mechanism, the homogenizing mechanism and the grinding mechanism to obtain a purified dispersion. S5: The purified dispersion enters the mixing mechanism through the fourth outlet, the third slurry conveying pipeline and the fifth inlet. The resin conveying pipeline feeds resin into the mixing mechanism. After the purified dispersion and the resin are mixed, they are solidified in the molding mechanism to obtain nanocellulose reinforced resin.

[0014] In a possible implementation, the modification treatment is carried out in an inert gas atmosphere at a temperature of 25-45°C.

[0015] Based on the above technical solution, this application has the following beneficial effects: This application provides a production apparatus comprising a pretreatment device, a nanocellulose modification device, a purification device, a gradient dispersion device, and a composite molding device connected sequentially by pipelines. This apparatus sequentially pretreats, oxidatively esterifies, purifies, and gradient disperses nanocellulose raw materials, avoiding nanocellulose agglomeration and incomplete modification, thus producing modified nanocellulose with high mechanical strength and stability. The composite molding device combines modified nanocellulose with resin, and the resin delivery pipeline can be used to change the type of resin being transported, enabling the production of multiple resins. All equipment in the production apparatus is connected by an integrated pipeline, and the entire production process is closed, enabling uninterrupted material transport. Compared to separate processes and additional equipment for communication between devices, the production apparatus provided by this application facilitates large-scale industrial production, ensuring production continuity and stability. Attached Figure Description

[0016] To more clearly illustrate the technical solutions and advantages in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0017] Figure 1 This application provides a schematic diagram of the structure of a production apparatus for nanocellulose-reinforced resin. Figure 2 This application provides a schematic diagram of the structure of a pretreatment device. Figure 3 This application provides a schematic diagram of the structure of a nanocellulose modification device. Figure 4 This application provides a schematic diagram of the structure of a solvent replacement device according to an embodiment; Figure 5 This application provides a schematic diagram of the structure of a gradient dispersion device. Reference numerals: 1-Pretreatment equipment, 11-First inlet, 12-Pretreatment mechanism, 121-Sieving mechanism, 122-Drying mechanism, 123-Weighing and feeding mechanism, 13-First outlet, 2-Nanocellulose modification equipment, 21-Second inlet, 22-Reaction chamber, 23-Liquid inlet pipe, 24-Second outlet, 25-Air inlet pipe, 26-Water cooling jacket, 3-Purification equipment, 31-Third inlet, 32-Solvent replacement mechanism, 321-First solvent replacement 322-Second solvent replacement chamber, 323-Third solvent replacement chamber, 33-Third discharge port, 34-Cleaning liquid pipeline, 35-Waste liquid discharge pipeline, 4-Gradient dispersion equipment, 41-Fourth feed port, 42-Stirring mechanism, 43-Homogenizing mechanism, 44-Grinding mechanism, 45-Fourth discharge port, 5-Composite molding equipment, 51-Detection mechanism, 6-Recycling equipment, 61-Crushing station, 62-Defibrilization resin station, 63-Pollutant discharge mechanism, 7-Finished product station. Detailed Implementation

[0018] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of this application.

[0019] It should be noted that, in the description of this application, the following definitions shall apply unless a different definition is given elsewhere in the claims or this specification. All numerical values, whether or not explicitly indicated, are defined herein as being modified by the term "about". The term "about" generally refers to a range of numerical values ​​that a person skilled in the art would consider equivalent to the stated values ​​to produce substantially the same properties, functions, results, etc. A range of numerical values ​​indicated by a low value and a high value is defined as including all numerical values ​​within that range and all subranges included within that range.

[0020] It should be noted that in the description of this application, the terms "first," "second," etc., are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence. It should be understood that such data can be interchanged where appropriate so that the embodiments of this application described herein can be implemented in orders other than those illustrated or described herein. Furthermore, the terms "comprising" and "having," and any variations thereof, are intended to cover non-exclusive inclusion.

[0021] It should be noted that, in the description of this application, the terms "on," "above," "over," and "above" should be interpreted in the broadest sense, meaning that a description containing these terms is interpreted as "a component may be disposed on another component in direct contact, or there may be an intermediate component or layer between the components." Furthermore, for ease of description, this application may also use spatial relative terms such as "below," "under," "below," "on," "above," "lower," and "upper" to describe the relationship between one element or component and another element or component shown in the accompanying drawings. In addition to the orientations described in the figures, spatial relative terms are also intended to cover different orientations of the device during use or operation. The device may be oriented in other ways (rotated 90° or otherwise), and the spatial relative descriptive terms used in this application can be interpreted accordingly.

[0022] The following is for reference Figure 1 -5. This application provides a production apparatus for nanocellulose-reinforced resin, including a pretreatment device 1, a nanocellulose modification device 2, a purification device 3, a gradient dispersion device 4, and a composite molding device 5.

[0023] The pretreatment equipment 1 includes a first feed inlet 11, a pretreatment mechanism 12 and a first discharge outlet 13 connected in sequence. The first feed inlet 11 is used to feed nanocellulose into the pretreatment mechanism 12.

[0024] The nanocellulose modification equipment 2 includes a reaction chamber 22, a liquid inlet pipe 23, a second feed port 21, and a second discharge port 24. The liquid outlet end of the liquid inlet pipe 23 is located inside the reaction chamber 22. The reaction chamber 22 is connected to the second feed port 21 and the second discharge port 24 respectively. The second feed port 21 and the second discharge port 24 are equipped with on / off valves. The second feed port 21 is connected to the first discharge port 13 through a powder conveying pipe.

[0025] The purification device 3 includes a third feed inlet, a solvent replacement mechanism 32 and a third discharge outlet 33 connected in sequence. The third feed inlet and the second discharge outlet 24 are connected through a first slurry conveying pipeline.

[0026] The gradient dispersion device 4 includes a fourth feed inlet 41, a stirring mechanism 42, a homogenizing mechanism 43, a grinding mechanism 44 and a fourth discharge outlet 45 connected in sequence. The fourth feed inlet 41 and the third discharge outlet 33 are connected through a second slurry conveying pipeline.

[0027] The composite molding equipment 5 includes a fifth feed inlet, a resin conveying pipeline, a mixing mechanism, and a molding mechanism. The mixing mechanism is connected to the fifth feed inlet, the resin conveying pipeline, and the molding mechanism, respectively. The fifth feed inlet and the fourth discharge outlet 45 are connected through a third slurry conveying pipeline.

[0028] Thus, the production apparatus provided in this application includes a pretreatment device 1, a nanocellulose modification device 2, a purification device 3, a gradient dispersion device 4, and a composite molding device 5 connected in sequence by pipelines. Each device is connected in series through a closed pipeline, and the processes are sequentially advanced. This allows for the sequential pretreatment, oxidative esterification modification, purification, and gradient dispersion of nanocellulose raw materials, avoiding the problems of nanocellulose agglomeration and incomplete modification, and preparing modified nanocellulose with high mechanical strength and stability. By using the composite molding device 5 to composite modified nanocellulose and resin, the type of resin transported can be changed through the resin transport pipeline, enabling the production of multiple resins. All devices in the production apparatus are connected by an integrated pipeline, and the entire production process is closed, enabling uninterrupted transport of production materials. Compared to setting up each process separately and transporting materials between devices through additional devices, the production apparatus provided in this application is conducive to large-scale industrial production and ensures the continuity and stability of production.

[0029] The integrated industrial production device for nanocellulose-reinforced resin provided in this application can realize a closed-loop process that connects nanocellulose raw material pretreatment, controllable low-temperature modification, multi-level gradient non-agglomeration dispersion, precise purification, multi-resin adaptive composite molding, and finished product testing and recycling. It achieves integrated and continuous stable industrial mass production of controllable modification of nanocellulose, non-agglomeration monodispersion, and precise resin composite molding, solving the industry pain points of traditional laboratory fragmentation and inability to achieve large-scale mass production, and adapting to the stringent production requirements of lightweight composite materials for new energy vehicles.

[0030] In a possible implementation, the production apparatus further includes a recycling device 6, which is connected via recycling pipelines to the pretreatment device 1, the nanocellulose modification device 2, the purification device 3, the gradient dispersion device 4, and the composite molding device 5. The recycling device 6 can collect waste materials and defective products generated in each production stage, ensuring no dust leakage and no disorderly discharge of waste liquid or waste gas during production, meeting green manufacturing requirements. The recycling device 6 can be connected to other equipment in the production apparatus via independently installed recycling pipelines to form a closed-loop production line.

[0031] In possible implementations, refer to Figure 2 The pretreatment equipment 1 includes a screening mechanism 121, a drying mechanism 122, and a weighing and feeding mechanism 123 connected in sequence. The top end of the screening mechanism 121 is connected to the first feed inlet 11, and the bottom end of the weighing and feeding mechanism 123 is connected to the first discharge outlet 13. After the nanocellulose raw material is fed into the first feed inlet 11, it passes through the screening mechanism 121, the drying mechanism 122, and the weighing and feeding mechanism 123 in sequence, realizing fine screening and impurity removal, low-temperature vacuum drying, and precise quantitative feeding of nanocellulose. This can remove powder impurities and free moisture from the raw material, avoid high-temperature thermal damage to the raw material, and protect the intrinsic mechanical properties of the raw material. The screening mechanism 121, drying mechanism 122, and weighing and feeding mechanism 123 are connected sequentially from top to bottom. Fine screening and impurity removal are completed by an airflow screening machine. Drying is carried out in a constant temperature vacuum environment in the drying mechanism 122 to accurately control the moisture content of the powder. This can remove large particles, agglomerates, and free water from the raw materials. Compared with the traditional high temperature drying mode, constant temperature vacuum drying can avoid high temperature heat damage to nanocellulose and fully preserve the intrinsic mechanical properties of the raw materials. After drying, the intelligent and precise weighing mechanism feeds the raw materials quantitatively according to the process ratio, which helps to ensure the purity, integrity, and mechanical stability of the nanocellulose raw materials and improve the consistency of the finished product performance.

[0032] Specifically, the screening mechanism 121 includes a screening chamber and a vacuum extraction port. The screening chamber is connected to the vacuum extraction port, which is connected to a negative pressure ventilation device. The vacuum extraction port is used to provide airflow power in the screening chamber.

[0033] Specifically, the screening chamber is equipped with a grading screen and an airflow channel. The airflow channel is connected to the drying mechanism 122. The grading screen allows the fine raw material powder to pass through and enter the airflow channel, thereby achieving fine screening and impurity removal of the raw material. It can remove large particles and agglomerated hard lumps, and send the screened raw material to the drying mechanism 122.

[0034] In a possible implementation, the pretreatment device also includes a coarse material discharge port, which is connected to a recycling pipeline. This discharge port can discharge large particles of coarse material removed from the raw materials and enter the recycling equipment 6 through the recycling pipeline, thereby achieving centralized recycling of waste materials and preventing dust from being blown outside the pretreatment device.

[0035] In a possible implementation, the nanocellulose modification device 2 further includes a constant-flow dripping component, a stirring component, and a pH sensor. The constant-flow dripping component is located at the liquid outlet, the stirring component is used to stir the slurry in the reaction chamber 22, and the pH sensor is used to detect the pH of the slurry in the reaction chamber 22. The constant-flow dripping component enables the addition of minute amounts of the reagent at a uniform rate, which is beneficial for controlling the uniform ratio of the reagent to nanocellulose. The constant-flow dripping component, stirring component, and pH sensor work together to achieve real-time pH control and low-speed homogenization during reagent addition, achieving uniform oxidation and activation of the nanocellulose fiber surface, effectively avoiding localized over-oxidation and uneven activation of nanocellulose, thereby preventing material performance defects.

[0036] Specifically, refer to Figure 3 The second feed inlet 21 is located at the top of the reaction chamber 22 and is connected to the reaction chamber 22. The liquid inlet pipe 23 is connected to the top of the reaction chamber 22 and the liquid outlet of the liquid inlet pipe 23 extends into the interior of the reaction chamber 22. It is used to deliver oxidant into the reaction chamber 22 to perform controllable and uniform surface oxidation activation on the pretreated nanocellulose, accurately increase the number of hydroxyl and carboxyl active functional groups on the surface of nanocellulose, and provide uniform, stable and high-density reaction sites for subsequent esterification grafting reaction.

[0037] In a possible implementation, the nanocellulose modification device 2 further includes an air inlet pipe 25, which is connected to the reaction chamber 22. The reaction chamber 22 is equipped with a water-cooling jacket 26 encased in its outer shell. The air inlet pipe 25 is used to introduce inert gas into the reaction chamber 22 to ensure that the nanocellulose esterification reaction is carried out in an inert gas atmosphere, thus preventing the nanocellulose from oxidizing and aging. The water-cooling jacket 26 is used to regulate the temperature inside the reaction chamber 22, preventing the nanocellulose from being degraded by high temperatures due to excessive heat. This is beneficial for improving the hygrothermal stability and service life of the modified nanocellulose.

[0038] Specifically, the water-cooled jacket 26 has a double-layer structure. The water-cooled jacket 26 is provided with a water inlet and a water outlet. The water inlet is located at the top of the water-cooled jacket 26, and the water outlet is located at the bottom of the water-cooled jacket 26. This enables water circulation within the water-cooled jacket 26, which helps to disperse heat within the reaction chamber 22 and ensures stable temperature within the reaction chamber 22.

[0039] In a possible implementation, the liquid inlet pipe 23 includes a first liquid inlet pipe 23 and a second liquid inlet pipe 23, which are respectively connected to the reaction chamber 22. The first liquid inlet pipe 23 is used to deliver an oxidant into the reaction chamber 22, and the second liquid inlet pipe 23 is used to deliver an esterifying agent into the reaction chamber 22, thereby realizing a low-temperature hydrophobic esterification modification reaction in the reaction chamber 22. Through the nanocellulose modification equipment 2, after the pretreated raw materials are oxidized and activated, the directional hydrophobic esterification modification of the nanocellulose surface can be completed in a low-temperature oxygen-free closed environment, accurately replacing the hydrophilic groups on the fiber surface and grafting hydrophobic functional groups with high density, which is beneficial to improving the wet and heat stability of nanocellulose and the composite materials subsequently prepared.

[0040] In one specific embodiment, the nanocellulose modification device 2 includes a second inlet 21, a reaction chamber 22, and a second outlet 24 connected in sequence. It also includes a liquid inlet pipe 23, an air inlet pipe 25, a water-cooled jacket 26, a constant flow dripping assembly, a stirring assembly, and a pH sensor. The liquid inlet pipe 23 and the air inlet pipe 25 are respectively connected to the reaction chamber 22. The constant flow dripping assembly is located at the liquid outlet end of the liquid inlet pipe 23. The stirring assembly and the pH sensor are located inside the reaction chamber 22. The liquid inlet pipe 23 includes a first liquid inlet pipe 23 and a second liquid inlet pipe 24. The second inlet 21 and the second outlet 24 are equipped with on / off valves. Thus, the constant flow dripping component enables the addition of reagents in minute, uniform amounts. Combined with real-time monitoring by a pH sensor and low-speed homogenization by a stirring component, the rate and extent of oxidation activation and esterification grafting reactions are precisely controlled, avoiding localized over-oxidation or uneven activation. The water-cooled jacket 26 enables full-process temperature control, preventing fiber thermal degradation caused by high temperatures. At the same time, an inert gas atmosphere is introduced through the air inlet pipe 25 to prevent fiber oxidation and aging. This enhances the active functional groups of hydroxyl and carboxyl groups on the surface of nanocellulose, and allows for high-density grafting of hydrophobic functional groups to replace hydrophilic groups, significantly improving the interfacial bonding between the fiber and resin and the wet and heat stability of the finished product.

[0041] In possible implementations, refer to Figure 4 The purification device 3 also includes a cleaning solution pipeline 34, and a solvent replacement mechanism 32 includes multiple solvent replacement chambers connected in series, each of which is connected to the cleaning solution pipeline 34. Through multiple solvent replacement chambers, residual solvents, unreacted monomers, and acidic byproducts from the oxidation-activation reaction can be replaced in a step-by-step gradient, effectively reducing trace impurities in the production system, significantly improving the purity of the modified nanocellulose powder, and contributing to improved stability and storage time of the modified nanocellulose.

[0042] Specifically, the solvent replacement chamber includes a first solvent replacement chamber 321, a second solvent replacement chamber 322, and a third solvent replacement chamber 323 connected in series. These chambers can sequentially match polar solvent replacement, residual acid and alkali neutralization and removal, and ultrafine powder suspension purification processes. They remove residual impurities in the system step by step, avoid solvent residue, improve the purity of modified nanocellulose, reduce the aging and performance degradation of finished products caused by impurity residue, extend the storage time of materials, and improve the high and low temperature aging resistance and long-term mechanical stability of nanocellulose reinforced resin products.

[0043] In some embodiments, the top of the first solvent replacement chamber 321 is connected to the third inlet. The first solvent replacement chamber 321 includes a first filter chamber, a first solvent replacement port, and a first waste liquid discharge port. The first filter chamber is disposed within the inner cavity of the first solvent replacement chamber 321 and is connected to the third inlet. The first solvent replacement port is disposed on the side wall of the first solvent replacement chamber 321 and is connected to the inner cavity of the first solvent replacement chamber 321. The first waste liquid discharge port is disposed at the bottom end of the first solvent replacement chamber 321. Thus, the modified nanocellulose slurry can enter the first filter chamber through the third inlet, where the solvent and solute of the modified nanocellulose slurry are separated. The solvent is discharged through the first waste liquid discharge port, and the first solvent replacement port allows the first solvent replacement to be input into the first solvent replacement chamber 321 and then into the first filter chamber.

[0044] Specifically, the second solvent replacement chamber 322 is connected to the first solvent replacement chamber 321. The second solvent replacement chamber 322 includes a second filtration chamber, a second solvent replacement port, and a second waste liquid discharge port. The second filtration chamber is located within the inner cavity of the second solvent replacement chamber 322 and is connected to the first filtration chamber. The second solvent replacement port is located on the side wall of the second solvent replacement chamber 322 and is connected to the inner cavity of the second solvent replacement chamber 322. The second waste liquid discharge port is located at the bottom end of the second solvent replacement chamber 322. Thus, the slurry from the first solvent replacement chamber 321 can enter the second filtration chamber, where the solvent and solute of the modified nanocellulose slurry are separated. The solvent is discharged through the second waste liquid discharge port, and the second solvent replacement port allows the second solvent replacement to be introduced into the second solvent replacement chamber 322 and then into the second filtration chamber.

[0045] Specifically, the third solvent replacement chamber 323 is connected to both the second solvent replacement chamber 322 and the third discharge port 33. The third solvent replacement chamber 323 includes a third filtration chamber, a third solvent replacement port, and a third waste liquid discharge port. The third filtration chamber is located within the inner cavity of the third solvent replacement chamber 323 and is connected to the second filtration chamber. The third solvent replacement port is located on the side wall of the third solvent replacement chamber 323 and is connected to its inner cavity. The third waste liquid discharge port is located at the bottom of the third solvent replacement chamber 323. Thus, the slurry from the second solvent replacement chamber 322 can enter the third filtration chamber, where the solvent and solute of the modified nanocellulose slurry are separated. The solvent is discharged through the third waste liquid discharge port, and the third solvent replacement port allows the third solvent to be introduced into the third solvent replacement chamber 323 and then into the third filtration chamber.

[0046] Specifically, the sidewalls of the first, second, and third filter chambers are all filter mesh structures, which can filter the liquid in the modified nanocellulose slurry.

[0047] Specifically, the first solvent replacement chamber 321 can be a polar solvent replacement chamber, the second solvent replacement chamber 322 is an acid-base neutralization chamber, and the third solvent replacement chamber 323 is a powder suspension purification chamber. The first solvent replacement chamber 321, the second solvent replacement chamber 322 and the third solvent replacement chamber 323 are connected in series through a closed pipeline. The closed pipeline is equipped with a delivery pump to realize pressurized delivery of the slurry.

[0048] Specifically, the purification equipment 3 also includes a waste liquid discharge pipeline 35, which is connected to the first waste liquid discharge port, the second waste liquid discharge port and the third waste liquid discharge port respectively, and is used to discharge the waste liquid generated after purification.

[0049] In a possible implementation, the gradient dispersion mechanism adopts a multi-stage speed-increasing and pressurizing structure. Through the step-by-step speed-increasing and pressurizing of the multi-stage speed-increasing and pressurizing structure, gradient shearing and homogeneous grinding can be achieved, realizing the layer-by-layer dissociation of agglomerated nanocellulose from large agglomerates to micro agglomerates and then to single nanofibers, eliminating fiber agglomeration defects and achieving a good dispersion effect.

[0050] Specifically, refer to Figure 5 The rotational speed gradients of the stirring mechanism 42, homogenizing mechanism 43, and grinding mechanism 44 are increased. Through a three-stage gradient shearing mode of progressively increasing speed and pressure, the nanocellulose agglomerates are gradually dissociated and refined, avoiding the inability of single stirring dispersion to completely remove particle agglomerates, which is beneficial to obtaining a fully dispersed nanocellulose slurry without agglomeration defects.

[0051] In a possible implementation, the stirring mechanism 42 includes a stirring chamber, a stirring element, and a turbine guide plate. The stirring element is disposed in the stirring chamber, and the turbine guide plate is disposed at the bottom of the stirring chamber. The stirring chamber can be a vertical, sealed, pressure-resistant chamber, and the outside of the stirring chamber is covered with a water-cooled temperature-controlled jacket. The stirring element is disposed at the center of the inner cavity of the stirring chamber and includes a vertical stirring shaft and multiple wide blades. The multiple wide blades are spaced apart on the vertical stirring shaft, and the stirring shaft can drive the wide blades to rotate, forming a large flow of agitation in the stirring chamber, which is beneficial for breaking up millimeter-sized cellulose agglomerates and completing the pre-dispersion of the purified slurry. The turbine guide plate is used to prevent the slurry from depositing at the bottom of the stirring chamber.

[0052] Specifically, the mixing chamber is connected to the fourth feed inlet 41, and the mixing chamber is connected to the third solvent replacement chamber 323 through the second slurry conveying pipeline, which allows the purified slurry to be directly fed into the mixing chamber.

[0053] In a possible implementation, the stirring mechanism 42 and the homogenizing mechanism 43 are connected by a low-pressure conveying pipeline, through which the stirred slurry is conveyed to the homogenizing mechanism 43.

[0054] Specifically, the homogenizing mechanism 43 includes a booster pump and a bidirectional impact valve. The booster valve is connected to a low-pressure delivery pipeline. The bidirectional impact valve includes a high-pressure branch pipe and two sets of valve cores. The discharge port of the booster pump is connected to the high-pressure branch pipe, and the high-pressure branch pipe is connected to the high-pressure feed rods of the two sets of valve cores respectively. The valve core also includes a valve core body, a diamond valve seat, and an impact chamber. The impact chamber is located at the outlet of the diamond valve seat. The diamond valve seat outlets of the two sets of valve cores are arranged opposite to each other. Through high-pressure bidirectional impact, the slurry collides at high speed in the impact chamber, breaking up the micron-sized fiber agglomerates and achieving further homogenization of the slurry after initial stirring and dispersion.

[0055] Specifically, the stirring mechanism 42 and the grinding mechanism 44 are connected by a high-pressure delivery pipeline.

[0056] In a possible implementation, the grinding mechanism 44 includes a coarse grinding chamber, a fine grinding chamber, and a nano-precision grinding chamber connected in sequence; a coarse grinding disc is provided in the coarse grinding chamber, and the coarse grinding disc includes a first rotor and a first stator arranged coaxially, the mating surface of the first rotor and the first stator is the grinding surface, the first rotor rotates relative to the first stator, and the coarse grinding of the homogenized slurry can be achieved through the friction between the first rotor and the first stator.

[0057] Specifically, a fine grinding disc is provided in the fine grinding chamber. The fine grinding disc includes a second rotor and a second stator that cooperate with each other. The gap between the second rotor and the second stator is smaller than the gap between the first rotor and the first stator.

[0058] Specifically, a nano-grinding disc is provided in the nano-grinding cavity. The nano-grinding disc includes a third rotor and a third stator that cooperate with each other. The gap between the third rotor and the third stator is smaller than the gap between the second rotor and the second stator.

[0059] In some embodiments, the chamber pressure in the coarse grinding chamber, fine grinding chamber, and nano-fine grinding chamber increases progressively. The nano-fine grinding chamber is connected to the fourth discharge port 45 and can be used to output the purified dispersion. In this way, through progressive fine grinding, the shear force of grinding is matched with the particles to be ground, thereby improving the grinding fineness.

[0060] In a possible implementation, the composite molding equipment 5 is used to composite and shape nanocellulose with resin to obtain a nanocellulose-reinforced resin product. A fifth feed inlet is used to deliver the purified dispersion into the mixing mechanism, and a resin delivery pipeline is used to deliver the resin into the mixing mechanism. The mixing mechanism is equipped with a mixing and stirring assembly to ensure uniform mixing of the purified dispersion and the resin. The mixing mechanism is connected to the molding mechanism, enabling the delivery of the mixed slurry to the molding mechanism for product shaping.

[0061] Specifically, the mixing mechanism also includes a proportioning and feeding mechanism and a mixing chamber. The fifth feed port and the resin conveying pipeline are connected to the mixing chamber through the proportioning and feeding mechanism. The proportioning and feeding mechanism is used to control the feed ratio of the fifth feed port and the resin conveying pipeline, thereby controlling the ratio of nanocellulose to resin in the mixing chamber, so as to achieve precise proportioning of modified nanocellulose dispersion with various resins.

[0062] Specifically, the composite molding equipment 5 also includes a closed plasticizer and a twin-screw extruder. The mixing mechanism, the closed plasticizer, and the twin-screw extruder are connected in sequence. The mixing mechanism can convey the uniformly mixed slurry of nanocellulose and resin to the closed plasticizer. The plasticized slurry in the closed plasticizer can then be extruded through the twin-screw extruder. In this way, after the mixing mechanism pre-mixes the nanocellulose and resin evenly, the closed plasticizer, through shearing and kneading, enables the nanocellulose to achieve uniform and stable dispersion in the resin, giving the mixed slurry good melt flowability and processability. This is beneficial for the efficient and continuous extrusion of the subsequent twin-screw extruder. By connecting the three in series, there is no need for intermediate material transfer, which is conducive to achieving continuous large-scale production.

[0063] Specifically, the twin-screw extruder is connected to the molding mechanism, which can be a constant-temperature pressure platen molding machine.

[0064] In a possible implementation, the mixing mechanism is provided with multiple resin inlets, which are detachably connected to the resin delivery pipeline. This facilitates the replacement of the resin delivery pipeline connected to the mixing mechanism, thereby changing the type of resin. This enables the mixing of modified nanocellulose with different types of resins and the blending of multiple types of resins. The process can be flexibly switched according to production needs to complete the automated industrial molding production of thermoplastic modified resin granules and thermosetting modified epoxy sheets.

[0065] In a possible implementation, the composite molding equipment 5 further includes a testing mechanism 51, which is connected to both the molding mechanism and the recycling equipment 6. The testing mechanism 51 is capable of testing and classifying the samples output from the molding mechanism. The testing mechanism 51 can perform real-time testing on each batch and continuously flowing samples, enabling real-time monitoring of product quality.

[0066] Specifically, the testing organization 51 can test the samples output by the molding organization and classify the samples into qualified samples and unqualified samples; the testing organization 51 can transport qualified samples to the finished product station 7 and unqualified samples to the recycling equipment 6, realizing production cycle, which helps to reduce raw material loss rate and reduce waste discharge.

[0067] Specifically, the testing institution 51 includes a tensile strength detector, a flexural strength detector, a high and low temperature alternating weathering aging device, a moisture content detector, and a thermal deformation stability detector. It can simultaneously perform online testing of the mechanical properties, weathering aging properties, and thermal stability of the sample in all dimensions, adapt to quality control standards, and realize closed-loop quality control throughout the entire production process.

[0068] In a possible implementation, the recycling equipment 6 includes a pollutant emission mechanism 63 and a recycling processing mechanism. The pollutant emission mechanism 63 is used to uniformly discharge pollutants that cannot be recycled, and the recycling processing mechanism is used to reprocess unqualified samples.

[0069] Specifically, the recycling and processing mechanism includes a crushing station 61, a defibrillation and resin dissolution station 62, and a pipeline return conveying system connected sequentially by pipelines. The crushing station 61 is used to pulverize the substandard product into micron-sized composite powder. The defibrillation and resin dissolution station 62 is used to dissolve the composite powder and peel off the resin matrix to separate and recover nanocellulose. The pipeline return conveying system is used to transport the purified and recovered fiber powder to the pretreatment equipment 1 via the recycling pipeline. Understandably, the physicochemical properties of the recovered fiber powder after crushing and resin dissolution are consistent with the properties of the nanocellulose raw material, making it suitable for processing in the pretreatment equipment 1. This allows for the effective recovery of the solid finished product and direct return to the nanocellulose processing step.

[0070] In a possible implementation, the powder conveying pipeline is equipped with a negative pressure conveying mechanism. The negative pressure conveying mechanism can create a vacuum suction force in the powder conveying pipeline, so that the powder is conveyed in the closed pipeline. The pressure inside the pipeline is lower than the external atmospheric pressure, which can effectively prevent powder leakage from the pipeline and prevent dust from escaping.

[0071] Specifically, the first, second, and third slurry conveying pipelines are equipped with high-pressure conveying mechanisms. Understandably, the slurry has the characteristics of high viscosity, easy settling, and poor fluidity. The high-pressure conveying mechanism can provide propulsion force to overcome the frictional and local resistance of the slurry in the pipeline, ensuring that the slurry is delivered to each device at a stable flow rate and pressure. Furthermore, nanocellulose is extremely prone to fiber settling and agglomeration under static or low-pressure conditions, which can lead to pipeline blockage. High-pressure conveying can maintain a high flow rate of the slurry in the pipeline, effectively inhibiting settling and ensuring smooth pipeline flow.

[0072] In a possible implementation, a conveying control component is provided on the powder conveying pipeline, the first slurry conveying pipeline, the second slurry conveying pipeline, and the third slurry conveying pipeline. The conveying control component includes a gate valve, a flow meter, and a concentration sensor to ensure uninterrupted automatic conveying of materials.

[0073] Specifically, gate valves are installed at the inlet and outlet ends of the pipeline for pipeline on / off control and maintenance isolation; flow meters are used to monitor the instantaneous and cumulative flow in the pipeline; and concentration sensors are used to detect the solid content or component concentration of the material in the pipeline to ensure that the concentration of the material entering the next process meets the process requirements.

[0074] Gate valves can be synchronized with flow meters to control the start and stop of various devices.

[0075] Specifically, the powder conveying pipeline, the first slurry conveying pipeline, the second slurry conveying pipeline, and the third slurry conveying pipeline are all equipped with insulation layers to control the pipeline temperature and adapt to the operating temperature requirements of each piece of equipment.

[0076] In a possible implementation, the production apparatus also includes control equipment, which is electrically connected to the pretreatment equipment 1, the nanocellulose modification equipment 2, the purification equipment 3, the gradient dispersion equipment 4, the composite molding equipment 5, and the recycling equipment 6, respectively, to achieve integrated control of each production stage.

[0077] Specifically, the control equipment is configured to digitally and precisely regulate, store and record in real time, and trace the entire process of temperature, reaction pressure, stirring speed, reagent drop acceleration rate, shear pressure, and molding temperature and pressure parameters of the production unit. It can accurately solidify core production process parameters. Compared with traditional laboratory processes, the production unit provided in this application can achieve large-scale mass production and provide reliable parameter support for subsequent production.

[0078] Specifically, the control device is electrically connected to the conveying control assembly, and the control device is configured to control each section of the conveying pipeline. On the other hand, the following describes a method for producing nano-cellulose-reinforced resin according to embodiments of this application. This specification provides the method operation steps as described in the embodiments, but based on conventional or non-inventive labor, more or fewer operation steps may be included. The order of steps listed in the embodiments is merely one possible order of execution among many steps and does not represent the only possible order. In actual preparation, the method can be executed in the order shown in the embodiments or accompanying drawings, or in parallel. The method for producing nano-cellulose-reinforced resin may include steps S1-S5.

[0079] S1: Nanocellulose is fed into the pretreatment unit 12 through the first feed port 11 to obtain pretreated cellulose; S2: Pretreated cellulose enters the reaction chamber 22 through the first discharge port 13, the powder conveying pipeline and the second inlet 21. Oxidizing agent and esterifying agent are added dropwise into the reaction chamber 22 through the liquid outlet end of the liquid inlet pipeline 23 to carry out modification treatment and obtain modified nanocellulose slurry. S3: The modified nanocellulose slurry enters the solvent replacement mechanism 32 through the second outlet 24, the first slurry conveying pipeline and the third inlet to purify the modified nanocellulose slurry and obtain purified slurry. S4: The purified slurry enters the stirring mechanism 42 through the third outlet 33, the second slurry conveying pipeline and the fourth inlet 41. The purified slurry is gradient dispersed by the stirring mechanism 42, the homogenizing mechanism 43 and the grinding mechanism 44 to obtain a purified dispersion. S5: The purified dispersion enters the mixing mechanism through the fourth outlet 45, the third slurry conveying pipeline and the fifth inlet. The resin conveying pipeline feeds resin into the mixing mechanism. After the purified dispersion and the resin are mixed, they are solidified in the molding mechanism to obtain nanocellulose reinforced resin.

[0080] Based on the above production method, integrated closed-loop continuous production is achieved, and the process parameters of each production stage can be precisely fixed and traceable throughout the entire process. This solves the problems of fragmentation and poor stability in traditional processes. The production method provided in this application is adaptable to stable industrial mass production. The above production method achieves controllable fiber modification and non-agglomerated monodispersity by sequentially pretreating, oxidative esterification modification, purification, and gradient dispersion of nanocellulose raw materials. This avoids the problems of nanocellulose agglomeration and incomplete modification at the interface, and prepares modified nanocellulose with high mechanical strength and stability. By compositing the modified nanocellulose with resin, the bonding force between nanocellulose and resin can be improved, thereby improving the hygrothermal stability of nanocellulose-reinforced resin composites. This production method uses the nanocellulose-reinforced resin production equipment provided in the above embodiments, has process repeatability, and can achieve stable industrial mass production.

[0081] In a possible implementation, the modification treatment is carried out in an inert gas atmosphere at a temperature of 25-45°C. Understandably, the modification temperature can be any value within the range of 25-45°C, and will not be enumerated here. Controlling the temperature within this range ensures the stable progress of the modification reaction.

[0082] The following describes specific embodiments of this application in conjunction with the aforementioned production apparatus and method for nanocellulose-reinforced resin. The following embodiments further illustrate the technical solutions of this application. These embodiments are for illustrative purposes only, as various modifications and variations within the scope of the disclosure of this application will be apparent to those skilled in the art.

[0083] Example 1 This embodiment provides an apparatus and method for producing nano-cellulose reinforced resin. The production method specifically includes the following steps: 1. Nanocellulose is fed into the pretreatment unit 12 through the first feed port 11 to obtain pretreated cellulose; 2. Pretreated cellulose enters the reaction chamber 22 through the first discharge port 13, the powder conveying pipeline, and the second feed port 21. Oxidizing agent and esterifying agent are sequentially added into the reaction chamber 22 through the liquid outlet end of the liquid inlet pipeline 23 to carry out modification treatment and obtain modified nanocellulose slurry; wherein, the modification treatment temperature is 35℃; 3. The modified nanocellulose slurry enters the solvent replacement mechanism 32 through the second outlet 24, the first slurry conveying pipeline and the third inlet to purify the modified nanocellulose slurry and obtain purified slurry; 4. The purified slurry enters the stirring mechanism 42 through the third discharge port 33, the second slurry conveying pipeline and the fourth feed port 41. The purified slurry is gradient dispersed by the stirring mechanism 42, the homogenizing mechanism 43 and the grinding mechanism 44 to obtain a purified dispersion. 5. The purified dispersion enters the mixing mechanism through the fourth outlet 45, the third slurry conveying pipeline and the fifth inlet. PA6 resin is fed into the mixing mechanism through the resin conveying pipeline. After the purified dispersion and resin are mixed, they are solidified in the molding mechanism to obtain nanocellulose-reinforced resin. The amount of nanocellulose added is 3wt%.

[0084] Compared to pure PA6 resin, the nanocellulose-reinforced resin prepared in this embodiment has a 32% increase in tensile strength, a 28% increase in flexural strength, a mechanical property decay rate of ≤8% after 2000 hours of high and low temperature alternating aging, and excellent hygrothermal stability.

[0085] Example 2 The similarities between this embodiment and Embodiment 1 will not be repeated here. The difference between this embodiment and Embodiment 1 is that the amount of nanocellulose added in the nanocellulose-reinforced resin is 2.5 wt%, and the resin is E51 epoxy resin.

[0086] Compared to pure E51 epoxy resin, the nanocellulose-reinforced resin prepared in this embodiment has a 30% higher tensile strength, a 45% lower dimensional heat distortion rate, and exhibits no water absorption or stratification even after long-term placement in high-humidity environments, making it suitable for the harsh operating conditions of the outer protective casing of power batteries.

[0087] Comparative Example 1 Nanocellulose and nanocellulose-reinforced resin were prepared using traditional high-temperature esterification modification and a single stirring dispersion process. The prepared nanocellulose-reinforced resin showed obvious fiber agglomeration, large dispersion of mechanical properties, performance degradation rate of over 25% after 500 hours of hygrothermal aging, and poor dimensional stability.

[0088] The nanocellulose-reinforced resin production apparatus provided in this application can effectively achieve stable industrial mass production of nanocellulose-reinforced resin. The process parameters can be precisely cured, the product performance is highly consistent and repeatable, which solves the shortcomings of existing technologies that cannot achieve stable industrial mass production. It can be directly used for large-scale application in the production line of lightweight supporting new energy vehicles, and provides mature equipment and process support for subsequent large-scale industrial mass production.

[0089] The foregoing description has fully disclosed the specific embodiments of this application. It should be noted that any modifications made by those skilled in the art to the specific embodiments of this application do not depart from the scope of the claims. Accordingly, the scope of the claims of this application is not limited to the foregoing specific embodiments.

Claims

1. A production apparatus for nanocellulose-reinforced resin, characterized in that, include: The pretreatment equipment includes a first inlet, a pretreatment mechanism, and a first outlet connected in sequence, wherein the first inlet is used to feed nanocellulose into the pretreatment mechanism. Nanocellulose modification equipment includes a reaction chamber, a liquid inlet pipeline, a second feed port and a second discharge port. The liquid outlet of the liquid inlet pipeline is located inside the reaction chamber. The reaction chamber is connected to the second feed port and the second discharge port respectively. The second feed port and the second discharge port are equipped with on / off valves. The second feed port and the first discharge port are connected through a powder conveying pipeline. The purification equipment includes a third inlet, a solvent replacement mechanism, and a third outlet connected in sequence, wherein the third inlet and the second outlet are connected through a first slurry conveying pipeline; A gradient dispersion device includes a fourth feed inlet, a stirring mechanism, a homogenizing mechanism, a grinding mechanism, and a fourth discharge outlet connected in sequence. The fourth feed inlet and the third discharge outlet are connected through a second slurry conveying pipeline. A composite molding equipment includes a fifth feed inlet, a resin conveying pipeline, a mixing mechanism, and a molding mechanism. The mixing mechanism is connected to the fifth feed inlet, the resin conveying pipeline, and the molding mechanism, respectively. The fifth feed inlet is connected to the fourth discharge outlet through a third slurry conveying pipeline.

2. The production apparatus according to claim 1, characterized in that, The production apparatus also includes a recycling device, which is connected to the pretreatment device, the nanocellulose modification device, the purification device, the gradient dispersion device, and the composite molding device via recycling pipelines.

3. The production apparatus according to claim 1, characterized in that, The pretreatment equipment includes a screening mechanism, a drying mechanism, and a weighing and feeding mechanism connected in sequence. The top end of the screening mechanism is connected to the first feed inlet, and the bottom end of the weighing and feeding mechanism is connected to the first discharge outlet.

4. The production apparatus according to any one of claims 1-3, characterized in that, The nanocellulose modification equipment also includes a constant flow dripping component, a stirring component, and an acid-base sensor. The constant flow dripping component is located at the liquid outlet, the stirring component is used to stir the slurry in the reaction chamber, and the acid-base sensor is used to detect the acidity or alkalinity of the slurry in the reaction chamber.

5. The production apparatus according to any one of claims 1-3, characterized in that, The nanocellulose modification equipment also includes an air inlet pipe, which is connected to the reaction chamber; the reaction chamber is provided with an outer shell covered by a water-cooling jacket.

6. The production apparatus according to any one of claims 1-3, characterized in that, The purification equipment also includes a cleaning solution pipeline, and the solvent replacement mechanism includes multiple solvent replacement chambers connected in series, each of which is connected to the cleaning solution pipeline.

7. The production apparatus according to any one of claims 1-3, characterized in that, The rotational speed gradient of the stirring mechanism, the homogenizing mechanism, and the grinding mechanism increases.

8. The production apparatus according to any one of claims 1-3, characterized in that, The composite molding equipment also includes a testing mechanism, which is connected to the molding mechanism and the recovery pipeline respectively. The testing mechanism is capable of testing and classifying the samples output by the molding mechanism.

9. The production apparatus according to any one of claims 1-3, characterized in that, The powder conveying pipeline is equipped with a negative pressure conveying mechanism, and the first slurry conveying pipeline, the second slurry conveying pipeline, and the third slurry conveying pipeline are equipped with high pressure conveying mechanisms.

10. A method for producing a nano-cellulose-reinforced resin, characterized in that, include: S1: Nanocellulose is fed into the pretreatment unit through the first feed port to obtain pretreated cellulose; S2: The pretreated cellulose enters the reaction chamber through the first outlet, the powder conveying pipeline and the second inlet. Oxidizing agent and esterifying agent are added dropwise into the reaction chamber through the liquid outlet of the liquid inlet pipeline to carry out modification treatment and obtain modified nanocellulose slurry. S3: The modified nanocellulose slurry enters the solvent replacement mechanism through the second outlet, the first slurry conveying pipeline and the third inlet to purify the modified nanocellulose slurry and obtain purified slurry; S4: The purified slurry enters the stirring mechanism through the third outlet, the second slurry conveying pipeline and the fourth inlet. The purified slurry is then gradient-dispersed by the stirring mechanism, the homogenizing mechanism and the grinding mechanism to obtain a purified dispersion. S5: The purified dispersion enters the mixing mechanism through the fourth outlet, the third slurry conveying pipeline and the fifth inlet. The resin conveying pipeline feeds resin into the mixing mechanism. After the purified dispersion and the resin are mixed, they are solidified in the molding mechanism to obtain nanocellulose reinforced resin.

11. The production method according to claim 10, characterized in that, The modification treatment is carried out in an inert gas atmosphere at a temperature of 25-45°C.