An R23 conversion catalyst, its preparation method and application

By preparing a Cr-In-Fe-Ga-Mn pentagonal composite chromium-based oxide catalyst, the problems of low activity and insufficient stability of existing chromium-based catalysts in the coupled conversion reaction of R23 and chloroform were solved, realizing efficient and stable resource utilization of R23, which is suitable for industrial production.

CN123102375APending Publication Date: 2026-11-17ZHEJIANG QUHUA FLUOR CHEM CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611376738.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-07
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing chromium-based catalysts exhibit low activity and poor selectivity in the coupled conversion reaction of R23 and chloroform, and lack long-term operational stability, making them unsuitable for the demands of wide operating conditions and continuous industrial production.

Method used

A 5-membered composite chromium-based oxide catalyst, Cr-In-Fe-Ga-Mn, was prepared by co-precipitation. By controlling the specific mass ratio of metal elements, it was adapted to the high-fluorine reaction conditions. The excess in-situ decomposition of R23 provided F active components, which inhibited carbon deposition and synergistically improved the catalyst stability.

Benefits of technology

It achieves efficient co-conversion of R23 and chloroform under mild conditions, significantly improves the selectivity of dichlorofluoromethane and dichlorofluoromethane and the stability of the catalyst, reduces equipment corrosion risk and operating costs, and is suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102375A_ABST
    Figure CN123102375A_ABST
Patent Text Reader

Abstract

This invention discloses an R23 conversion catalyst, its preparation method, and its applications. The R23 conversion catalyst is composed of multiple metal oxides. Based on the total mass of metals in the metal oxides as 100%, the R23 conversion catalyst contains the following metal elements in the following mass percentages: Cr 54%~77%, In 10%~18%, Fe 6%~12%, Ga 5%~10%, and Mn 2%~6%; all metal elements exist in oxide form. The preparation method includes raw material preparation, co-precipitation reaction, post-treatment, and calcination activation at 250~450℃. The R23 conversion catalyst can be used for the catalytic conversion reaction of trifluoromethane and chloroform to prepare difluorochloromethane and difluorochloromethane. In specific applications, an excess of R23 can be used, utilizing the in-situ decomposition of excess R23 to continuously provide the active component F, which can be directly used as the fluorine source for the chloroform fluorination reaction without the need for external hydrogen fluoride.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of catalytic conversion technology of trifluoromethane (HFC-23 or R23), specifically to an R23 conversion catalyst, its preparation method, and its application. Background Technology

[0002] In existing technologies, R23 treatment mainly relies on high-temperature incineration, which is energy-intensive and polluting, and cannot be utilized as a resource. A few R23 conversion processes use chromium-based catalysts, but under high-temperature conditions, active components are prone to agglomeration and valence imbalance, resulting in insufficient long-term operational stability. This makes it difficult to adapt to the needs of wide-condition, continuous industrial production, thus restricting the improvement of the quality and efficiency of R23 resource conversion processes and their low-cost large-scale application.

[0003] Existing chromium-based catalysts are commonly used catalytic systems in the fluorochemical industry. However, traditional chromium-based catalysts have single active sites and poor adaptability to the coupled conversion reaction of R23 and chloroform, resulting in defects such as low feed conversion rate, poor selectivity of target product, and easy deactivation at high temperatures. Therefore, developing a dedicated catalyst with multi-component synergy, high activity, good stability, and adaptability to the co-conversion reaction of R23 and chloroform is the key to overcoming the current technological bottlenecks.

[0004] The following existing technologies were found through a search: Patent specification CN110833837A discloses a catalyst for the resource utilization of trifluoromethane, comprising a main catalyst selected from at least one of chromium, aluminum, magnesium oxides or fluorides, and a co-catalyst selected from at least one of Cr, Mg, Al, Ni, Co, Zn, Fe, Cu, In, Mn, La, Ce, Sm oxides or fluorides. The molar ratio of the main catalyst to the co-catalyst is 1:0.01 to 1:0.5. Although this patent document discloses that the main catalyst and the co-catalyst can be oxides, the preparation method disclosed herein involves activation first in an inert gas atmosphere at 200-350°C, followed by activation in a diluted HF gas atmosphere at 200-350°C, and the diluted HF gas is HF gas diluted with an inert gas. Furthermore, although this patent document also discloses a molar ratio of halogenated hydrocarbons to trifluoromethane of 1:1 to 3, in all its embodiments, the molar amount of halogenated hydrocarbons is greater than that of trifluoromethane.

[0005] Patent specification CN112979410A discloses a method for improving catalyst stability in the resource utilization of HFC-23. The resource utilization is achieved through a fluorine-chlorine exchange reaction between HFC-23 and a haloalkane. The haloalkane is chloroform or a mixture containing chloroform, and the molar ratio of HFC-23 to the haloalkane is 1:1 to 3. The catalyst for the fluorine-chlorine exchange reaction includes a host catalyst and a metal oxide. The host catalyst is a chromium, aluminum, or magnesium-based catalyst or a chromium, aluminum, or magnesium catalyst supported on activated carbon / graphite. The metal oxide is selected from at least one metal oxide from K, Na, Fe, Co, Cu, Ni, Zn, or Ti, and the addition amount is 0.1 to 5 wt%. This catalyst requires a two-stage fluorination treatment during preparation. Summary of the Invention

[0006] This invention aims to overcome the technical defects of existing single chromium-based catalysts, such as low catalytic activity, poor product selectivity, insufficient reaction stability, harsh conditions for R23 resource conversion, and low raw material utilization. It provides a method for preparing a multi-component composite chromium-based R23 conversion catalyst and its application, which realizes the efficient co-conversion of R23 and chloroform under mild conditions and the highly selective preparation of dichlorofluoromethane (R21) and dichlorofluoromethane (R22).

[0007] The specific technical solution of this invention is as follows: In a first aspect, the present invention provides an R23 conversion catalyst composed of a composite of multiple metal oxides; Based on the total mass of metals in the metal oxide being 100%, the R23 conversion catalyst contains the following metal elements by mass percentage: chromium (Cr) 54%~77% (e.g., 55%, 56%, 57%, 58%, 59%, 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69%, 70%, 71%, 72%, 73%, 74%, 75%, 76%, etc.), indium (In) 10%~18% (e.g., 11%, 12%, 13%, 14%, 15%, 16%, 17%, etc.), iron (Fe) 6%~12% (e.g., 7%, 8%, 9%, 10%, 11%, etc.), gallium (Ga) 5%~10% (e.g., 6%, 7%, 8%, 9%, etc.), and manganese (Mn) 2%~6% (e.g., 3%, 4%, 5%, etc.); all metal elements exist in oxide form.

[0008] This invention provides a Cr-In-Fe-Ga-Mn pentagonal composite chromium-based oxide catalyst, which limits the specific mass ratio of each metal element and is suitable for high fluorine (R23 excess) reaction conditions.

[0009] In some preferred embodiments, the sum of the mass percentages of Cr, In, Fe, Ga and Mn is 100%.

[0010] In a second aspect, the present invention provides a method for preparing the R23 conversion catalyst as described in the first aspect, wherein the R23 conversion catalyst is prepared by co-precipitation.

[0011] Furthermore, the preparation method includes the following steps: S1. Raw material preparation: Weigh the chromium precursor, indium precursor, iron precursor, gallium precursor and manganese precursor according to the mass ratio of each metal element, dissolve them in deionized water, stir evenly, and prepare a mixed metal precursor solution. S2. Coprecipitation reaction: Add precipitant dropwise to the mixed metal precursor solution and stir continuously to carry out the coprecipitation reaction until the reaction is complete, and a mixed suspension is obtained. S3. Post-processing: The mixed suspension is allowed to stand and age, the solid is separated and washed until neutral, and then dried to obtain the precursor powder. S4. Calcination and activation: The precursor powder is calcined at a constant temperature of 250~450℃ (e.g., 320℃) to obtain the R23 conversion catalyst.

[0012] In step S1, the chromium precursor, indium precursor, iron precursor, gallium precursor, and manganese precursor may each independently include at least one of water-soluble nitrates and chlorides.

[0013] In step S2, the precipitant may include one or more of ammonia, sodium hydroxide solution, and sodium carbonate solution.

[0014] In some preferred embodiments, during step S2, the pH value of the coprecipitation reaction system is controlled at 8-10 (e.g., 9) during the addition of the precipitant.

[0015] In step S3, the aging time can be 2 to 6 hours, such as 4 hours.

[0016] In step S3, the drying temperature can be 80~120℃, for example 100℃.

[0017] In step S3, the drying time can be 8 to 12 hours, such as 10 hours.

[0018] In step S4, the calcination heating rate can be 2~5℃ / min, for example 3℃ / min.

[0019] In step S4, the constant temperature calcination time can be 3~8 hours, for example, 5 hours.

[0020] Thirdly, the present invention provides an application of the R23 conversion catalyst as described in the first aspect. The R23 conversion catalyst can be used in the catalytic conversion reaction of trifluoromethane and chloroform to prepare difluorochloromethane and difluorochloromethane.

[0021] In some preferred embodiments, the process conditions for the catalytic conversion reaction include: a molar ratio of trifluoromethane to chloroform greater than 1:1 and not exceeding 20:1 (e.g., 2:1), a reaction temperature of 200-400°C (e.g., 300°C), a reaction pressure of 0.1-1.5 MPa (e.g., 0.5 MPa), and a reaction space velocity of 50-1500 h⁻¹. -1 (e.g., 500h) -1 wait).

[0022] As a general inventive concept, in a fourth aspect, the present invention provides a method for preparing dichlorofluoromethane and dichlorofluoromethane by catalytic conversion of trifluoromethane with chloroform, using the R23 conversion catalyst described in the first aspect.

[0023] In some preferred embodiments, the process conditions for the catalytic conversion reaction include: a molar ratio of trifluoromethane to chloroform greater than 1:1 and not exceeding 20:1 (e.g., 2:1), a reaction temperature of 200-400°C (e.g., 300°C), a reaction pressure of 0.1-1.5 MPa (e.g., 0.5 MPa), and a reaction space velocity of 50-1500 h⁻¹. -1 (e.g., 500h) -1 wait).

[0024] Compared with the prior art, the beneficial effects of this invention are as follows: 1. Achieve in-situ fluorine supply and simplify process safety: This invention uses an excess R23 ratio, which utilizes the in-situ decomposition of excess R23 to continuously provide the active F component, which can be directly used as the fluorine source for the chloroform fluorination reaction without the need for external hydrogen fluoride, thus significantly reducing equipment corrosion and process safety risks.

[0025] 2. Significantly inhibits carbon buildup and improves catalyst stability from the root: Excess R23 creates a fluorine-rich micro-atmosphere, which can effectively inhibit high-temperature cracking, polymerization and coking of chloroform. Combined with the synergistic modification mechanism of five-element metals, it eliminates carbon buildup on the catalyst surface covering active sites, solves the defects of traditional catalyst carbon buildup and deactivation, and realizes a high-efficiency, long-cycle stable catalytic conversion process of chloroform and R23, fundamentally alleviates the catalyst deactivation problem and significantly extends service life.

[0026] 3. Synergistic effect of multiple metals and high reaction selectivity: The five-element composite oxide synergistically optimizes the surface structure and electronic properties, resists fluorine corrosion, stabilizes the crystal structure, reduces side reactions, and stably obtains high-purity monofluorodichloromethane and difluoromonochloromethane products.

[0027] 4. Strong industrial applicability: It enables the resource utilization of by-product R23, eliminates the need for frequent catalyst regeneration, reduces operating costs, and has better continuous production stability and economy compared to existing technologies. Attached Figure Description

[0028] Figure 1 A comparison chart of catalyst lifetimes under different R23 / chloroform molar ratios. Detailed Implementation

[0029] The present invention will be further described below with reference to the accompanying drawings and specific embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. Operating methods not specifically specified in the following embodiments are generally performed under conventional conditions or as recommended by the manufacturer.

[0030] Example 1: This embodiment provides an R23 conversion catalyst, which is composed of multiple metal oxides. Based on the total mass of metals in the metal oxides being 100%, the mass percentage of each metal element is: Cr 65%, In 15%, Fe 8%, Ga 7%, and Mn 5%. All metal elements exist in oxide form.

[0031] The above-mentioned method for preparing the R23 conversion catalyst includes the following steps: S1. Weigh chromium nitrate, indium nitrate, ferric nitrate, gallium nitrate, and manganese nitrate according to the ratio, add deionized water, stir at room temperature for 40 minutes, and completely dissolve to obtain a mixed metal salt solution. S2. Slowly add dilute ammonia water as a precipitant while stirring continuously. Control the pH of the system to 9. After the addition is complete, continue stirring for 1.5 hours to obtain a uniform suspension. S3. After aging at room temperature for 4 hours, filter, wash the filter cake with deionized water until neutral, and dry at 100℃ for 10 hours to obtain the catalyst precursor. S4. Place the precursor in a muffle furnace, heat it to 320℃ at 3℃ / min, and calcine it at a constant temperature for 5 hours to obtain the finished catalyst.

[0032] Catalyst Application: The catalyst was used in the catalytic reaction of R23 and chloroform. The process conditions were controlled as follows: molar ratio of R23 to chloroform 2:1, reaction temperature 300℃, reaction pressure 0.5MPa, and reaction space velocity 500h⁻¹. -1 The test results after 50 h of reaction showed that the chloroform conversion rate reached 85.1%, the total selectivity of monofluorodichloromethane and difluorochloromethane reached 98.5%, and the selectivity of other products was 1.5%.

[0033] Example 2: This embodiment provides an R23 conversion catalyst, which is composed of multiple metal oxides. Based on the total mass of metals in the metal oxides being 100%, the mass percentage of each metal element is: Cr 77%, In 10%, Fe 6%, Ga 5%, and Mn 2%. All metal elements exist in oxide form.

[0034] The above-mentioned method for preparing the R23 conversion catalyst includes the following steps: S1. Weigh chromium nitrate, indium nitrate, ferric nitrate, gallium nitrate, and manganese nitrate according to the ratio, add deionized water, stir at room temperature for 40 minutes, and completely dissolve to obtain a mixed metal salt solution. S2. Slowly add dilute ammonia water as a precipitant while stirring continuously. Control the pH of the system to 9. After the addition is complete, continue stirring for 1.5 hours to obtain a uniform suspension. S3. After aging at room temperature for 4 hours, filter, wash the filter cake with deionized water until neutral, and dry at 100℃ for 10 hours to obtain the catalyst precursor. S4. Place the precursor in a muffle furnace, heat it to 320℃ at 3℃ / min, and calcine it at a constant temperature for 5 hours to obtain the finished catalyst.

[0035] Catalyst Application: The catalyst was used in the catalytic reaction of R23 and chloroform. The process conditions were controlled as follows: molar ratio of R23 to chloroform 2:1, reaction temperature 300℃, reaction pressure 0.5MPa, and reaction space velocity 500h⁻¹. -1 The test results after 50 h of reaction showed that the chloroform conversion rate reached 88.2%, the total selectivity of monofluorodichloromethane and difluorochloromethane reached 97.7%, and the selectivity of other products was 2.3%.

[0036] Example 3: This embodiment provides an R23 conversion catalyst, which is composed of multiple metal oxides. Based on the total mass of metals in the metal oxides being 100%, the mass percentage of each metal element is as follows: Cr 54%, In 18%, Fe 12%, Ga 10%, and Mn 6%. All metal elements exist in oxide form.

[0037] The above-mentioned method for preparing the R23 conversion catalyst includes the following steps: S1. Weigh chromium nitrate, indium nitrate, ferric nitrate, gallium nitrate, and manganese nitrate according to the ratio, add deionized water, stir at room temperature for 40 minutes, and completely dissolve to obtain a mixed metal salt solution. S2. Slowly add dilute ammonia water as a precipitant while stirring continuously. Control the pH of the system to 9. After the addition is complete, continue stirring for 1.5 hours to obtain a uniform suspension. S3. After aging at room temperature for 4 hours, filter, wash the filter cake with deionized water until neutral, and dry at 100℃ for 10 hours to obtain the catalyst precursor. S4. Place the precursor in a muffle furnace, heat it to 320℃ at 3℃ / min, and calcine it at a constant temperature for 5 hours to obtain the finished catalyst.

[0038] Catalyst Application: The catalyst was used in the catalytic reaction of R23 and chloroform. The process conditions were controlled as follows: molar ratio of R23 to chloroform 2:1, reaction temperature 300℃, reaction pressure 0.5MPa, and reaction space velocity 500h⁻¹. -1The test results after 50 h of reaction showed that the chloroform conversion rate reached 87.8%, the total selectivity of monofluorodichloromethane and difluorochloromethane reached 96.8%, and the selectivity of other products was 3.2%.

[0039] Example 4: This embodiment provides an R23 conversion catalyst, which is composed of multiple metal oxides. Based on the total mass of metals in the metal oxides being 100%, the mass percentage of each metal element is: Cr 65%, In 15%, Fe 8%, Ga 7%, and Mn 5%. All metal elements exist in oxide form.

[0040] The above-mentioned method for preparing the R23 conversion catalyst includes the following steps: S1. Weigh chromium nitrate, indium nitrate, ferric nitrate, gallium nitrate, and manganese nitrate according to the ratio, add deionized water, stir at room temperature for 40 minutes, and completely dissolve to obtain a mixed metal salt solution. S2. Slowly add dilute ammonia water as a precipitant while stirring continuously. Control the pH of the system to 9. After the addition is complete, continue stirring for 1.5 hours to obtain a uniform suspension. S3. After aging at room temperature for 4 hours, filter, wash the filter cake with deionized water until neutral, and dry at 100℃ for 10 hours to obtain the catalyst precursor. S4. Place the precursor in a muffle furnace, heat it to 250℃ at 3℃ / min, and calcine it at a constant temperature for 5 hours to obtain the finished catalyst.

[0041] Catalyst Application: The catalyst was used in the catalytic reaction of R23 and chloroform. The process conditions were controlled as follows: molar ratio of R23 to chloroform 2:1, reaction temperature 300℃, reaction pressure 0.5MPa, and reaction space velocity 500h⁻¹. -1 The test results after 50 h of reaction showed that the chloroform conversion rate reached 84.5%, the total selectivity of monofluorodichloromethane and difluorochloromethane reached 98.1%, and the selectivity of other products was 1.9%.

[0042] Example 5: This embodiment provides an R23 conversion catalyst, which is composed of multiple metal oxides. Based on the total mass of metals in the metal oxides being 100%, the mass percentage of each metal element is: Cr 65%, In 15%, Fe 8%, Ga 7%, and Mn 5%. All metal elements exist in oxide form.

[0043] The above-mentioned method for preparing the R23 conversion catalyst includes the following steps: S1. Weigh chromium nitrate, indium nitrate, ferric nitrate, gallium nitrate, and manganese nitrate according to the ratio, add deionized water, stir at room temperature for 40 minutes, and completely dissolve to obtain a mixed metal salt solution. S2. Slowly add dilute ammonia water as a precipitant while stirring continuously. Control the pH of the system to 9. After the addition is complete, continue stirring for 1.5 hours to obtain a uniform suspension. S3. After aging at room temperature for 4 hours, filter, wash the filter cake with deionized water until neutral, and dry at 100℃ for 10 hours to obtain the catalyst precursor. S4. Place the precursor in a muffle furnace, heat it to 450℃ at 3℃ / min, and calcine it at a constant temperature for 5 hours to obtain the finished catalyst.

[0044] Catalyst Application: The catalyst was used in the catalytic reaction of R23 and chloroform. The process conditions were controlled as follows: molar ratio of R23 to chloroform 2:1, reaction temperature 300℃, reaction pressure 0.5MPa, and reaction space velocity 500h⁻¹. -1 The test results after 50 h of reaction showed that the chloroform conversion rate reached 86.3%, the total selectivity of monofluorodichloromethane and difluorochloromethane reached 97.4%, and the selectivity of other products was 2.6%.

[0045] Comparative Example 1: The difference from Example 1 is that no metal doping components In, Fe, Ga, and Mn are added; only Cr is used to prepare the catalyst.

[0046] The test results showed that the chloroform conversion rate in this comparative example was 72.8%, the total selectivity for dichlorofluoromethane and dichlorofluoromethane was 97.3%, and the selectivity for other products was 2.7%, indicating that the effect of a single metal catalyst is far inferior to that of the catalyst of this invention.

[0047] Comparative Example 2: The difference from Example 1 is that the molar ratio of R23 to chloroform in the catalyst application is 1:2.

[0048] The results showed that the chloroform conversion rate in this comparative example was 30.5%, the total selectivity for dichlorofluoromethane and dichlorofluoromethane was 96.5%, and the selectivity for other products was 3.5%.

[0049] Stability testing: The catalysts of Example 1 and Comparative Example 2 were subjected to stability tests, respectively. See Figure 1 After 500 hours of life testing, it was found that the chloroform conversion rate remained unchanged when the R23 / chloroform molar ratio was 2:1, while the chloroform conversion rate continued to decrease when the R23 / chloroform molar ratio was 1:2. This indicates that an excess of R23 is beneficial to improving catalyst life and is more suitable for industrial production.

[0050] Comparative Example 3: The difference from Example 1 is that the mass percentage of each metal element is: Cr 72%, In 15%, Fe 8%, Ga 0%, Mn 5%.

[0051] The results showed that the chloroform conversion rate in this comparative example was 73.1%, the total selectivity for dichlorofluoromethane and dichlorofluoromethane was 96.8%, and the selectivity for other products was 3.2%.

[0052] Comparative Example 4: The difference from Example 1 is that the mass percentage of each metal element is: Cr 80%, In 0%, Fe 8%, Ga 7%, Mn 5%.

[0053] The results showed that the chloroform conversion rate in this comparative example was 75.9%, the total selectivity for dichlorofluoromethane and dichlorofluoromethane was 97.4%, and the selectivity for other products was 2.6%.

[0054] Comparative Example 5: The difference from Example 1 is that the mass percentage of each metal element is: Cr 73%, In 15%, Fe 0%, Ga 7%, Mn 5%.

[0055] The results showed that the chloroform conversion rate in this comparative example was 82.6%, the total selectivity for dichlorofluoromethane and dichlorofluoromethane was 98.1%, and the selectivity for other products was 1.9%.

[0056] Comparative Example 6: The difference from Example 1 is that the mass percentage of each metal element is: Cr 70%, In 15%, Fe 8%, Ga 7%, Mn 0%.

[0057] The results showed that the chloroform conversion rate in this comparative example was 80.7%, the total selectivity for dichlorofluoromethane and dichlorofluoromethane was 96.9%, and the selectivity for other products was 3.1%.

[0058] Comparative Example 7: The difference from Example 1 is that the mass percentage of each metal element is: Cr 50%, In 20%, Fe 12%, Ga 10%, Mn 8%.

[0059] The results showed that the chloroform conversion rate in this comparative example was 70.9%, the total selectivity for dichlorofluoromethane and dichlorofluoromethane was 95.8%, and the selectivity for other products was 4.2%.

[0060] Comparative Example 8: The difference from Example 1 is that the mass percentage of each metal element is: Cr 80%, In 8%, Fe 5%, Ga 4%, Mn 3%.

[0061] The results showed that the chloroform conversion rate in this comparative example was 74.4%, the total selectivity for dichlorofluoromethane and dichlorofluoromethane was 96.3%, and the selectivity for other products was 3.7%.

[0062] Comparative Example 9: The difference from Example 1 is that the mass percentage of each metal element is: Cr 69%, In 15%, Fe 8%, Ga 3%, Mn 5%.

[0063] The results showed that the chloroform conversion rate in this comparative example was 80.6%, the total selectivity for dichlorofluoromethane and dichlorofluoromethane was 97.1%, and the selectivity for other products was 2.9%.

[0064] Comparative Example 10: The difference from Example 1 is that the mass percentage of each metal element is: Cr 60%, In 15%, Fe 8%, Ga 12%, Mn 5%.

[0065] The results showed that the chloroform conversion rate in this comparative example was 79.1%, the total selectivity for dichlorofluoromethane and dichlorofluoromethane was 98.4%, and the selectivity for other products was 1.6%.

[0066] Comparative Example 11: The difference from Example 1 is that the catalyst used is the catalyst prepared in Example 1 of patent document CN110833837A.

[0067] The results showed that the chloroform conversion rate in this comparative example was 40.2%, the total selectivity for dichlorofluoromethane and dichlorofluoromethane was 94.3%, and the selectivity for other products was 5.7%.

[0068] Furthermore, it should be understood that after reading the above description of the present invention, those skilled in the art can make various alterations or modifications to the present invention, and these equivalent forms also fall within the scope defined by the appended claims.

Claims

1. An R23 conversion catalyst characterized by, Composed of a composite of various metal oxides; Based on the total mass of metals in the metal oxide being 100%, the R23 conversion catalyst contains the following metal elements by mass percentage: Cr 54%~77%, In 10%~18%, Fe 6%~12%, Ga 5%~10%, Mn 2%~6%; all metal elements exist in oxide form.

2. The R23 conversion catalyst according to claim 1, characterized by The sum of the mass percentages of Cr, In, Fe, Ga and Mn is 100%.

3. A process for the preparation of a R23 conversion catalyst as claimed in claim 1 or 2, characterized in that, The R23 conversion catalyst was prepared by co-precipitation.

4. The production method according to claim 3, characterized by, The preparation method includes the following steps: S1. Raw material preparation: Weigh the chromium precursor, indium precursor, iron precursor, gallium precursor and manganese precursor according to the mass ratio of each metal element, dissolve them in deionized water, stir evenly, and prepare a mixed metal precursor solution. S2. Coprecipitation reaction: Add precipitant dropwise to the mixed metal precursor solution and stir continuously to carry out the coprecipitation reaction until the reaction is complete, and a mixed suspension is obtained. S3. Post-processing: The mixed suspension is allowed to stand and age, the solid is separated and washed until neutral, and then dried to obtain the precursor powder. S4. Calcination and activation: The precursor powder is calcined at a constant temperature of 250~450℃ to obtain the R23 conversion catalyst.

5. The preparation method according to claim 4, characterized in that, In step S1, the chromium precursor, indium precursor, iron precursor, gallium precursor, and manganese precursor each independently include at least one of water-soluble nitrates and chlorides.

6. The preparation method according to claim 4, characterized in that, In step S2, the precipitant includes one or more of ammonia, sodium hydroxide solution, and sodium carbonate solution.

7. The preparation method according to claim 4, characterized in that, In step S2, the pH value of the coprecipitation reaction system is controlled at 8~10 during the dropwise addition of the precipitant.

8. The preparation method according to claim 4, characterized in that, In step S3, the aging time is 2 to 6 hours.

9. The preparation method according to claim 4, characterized in that, In step S3, the drying temperature is 80~120℃.

10. The preparation method according to claim 4, characterized in that, In step S3, the drying time is 8~12 hours.

11. The preparation method according to claim 4, characterized in that, In step S4, the calcination heating rate is 2~5℃ / min.

12. The preparation method according to claim 4, characterized in that, In step S4, the constant temperature calcination time is 3~8 hours.

13. An application of the R23 conversion catalyst as described in claim 1 or 2, characterized in that, The R23 conversion catalyst is used for the catalytic conversion reaction of trifluoromethane and chloroform to prepare difluorochloromethane and difluorochloromethane.

14. The application according to claim 13, characterized in that, The process conditions of the catalytic conversion reaction include: the molar ratio of trifluoromethane to chloroform is greater than 1:1 and does not exceed 20:1, the reaction temperature is 200-400℃, the reaction pressure is 0.1-1.5MPa, the reaction space velocity is 50-1500h -1 .

15. A method for preparing dichlorofluoromethane and dichlorofluoromethane by catalytic conversion of trifluoromethane with chloroform, characterized in that, The R23 conversion catalyst described in claim 1 or 2 is used.

16. The method according to claim 15, characterized in that, The process conditions of the catalytic conversion reaction include: the molar ratio of trifluoromethane to chloroform is greater than 1:1 and does not exceed 20:1, the reaction temperature is 200-400℃, the reaction pressure is 0.1-1.5MPa, the reaction space velocity is 50-1500h -1 .

Citation Information

Patent Citations

  • Catalyst for resource utilization of trifluoromethane

    CN110833837A

  • Method for improving stability of catalyst during resource utilization of HFC-23

    CN112979410A