A method for desulfurization and carbon removal separation in low-alkali processes of high-carbon organic copper-sulfur ore.
By combining a low-alkali process with a positive and negative separation method using low-alkali sulfur inhibitors and carbon inhibitors, the problem of separating high-carbon organic copper-sulfur ore has been solved, achieving efficient resource utilization of copper-sulfur ore and improving the grade of copper concentrate.
Patent Information
- Application Number
- CN202611380888.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-07
- Publication Date
- 2026-11-17
AI Technical Summary
Traditional copper-sulfur separation processes suffer from problems such as the high floatability of carbon organic matter, mixing of carbon, sulfur, and copper phases, low recovery rate, and equipment scaling when processing copper-sulfur ores with high carbon organic matter content, making it difficult to achieve efficient separation and resource utilization.
By employing a low-alkali process, through roughing, positive removal of some carbon organic matter and reverse decarbonization steps of copper-suspension carbon flotation, combined with low-alkali sulfur inhibitors, carbon inhibitors and copper collectors, positive and negative separation of copper-sulfur ore is achieved, sulfur enrichment is reduced and copper concentrate grade is improved.
Highly efficient separation of copper-sulfur ore was achieved under low-alkali conditions, resulting in improved copper concentrate grade, reduced copper loss rate, and increased overall resource recovery rate.
Smart Images

Figure CN123102495A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of metallurgical technology, specifically relating to a method for desulfurization and positive and negative carbon removal separation in a low-alkali process for copper-sulfur ores with high carbon content and organic matter. Background Technology
[0002] Traditional copper-sulfur separation commonly employs a high-alkali lime process, which suppresses pyrite by adding large amounts of lime. However, this process has inherent drawbacks such as equipment scaling, sticky froth, low recovery rate of associated gold and silver, and difficulty in treating recycled water. As easily beneficiated ores become increasingly depleted, the proportion of complex copper-sulfur ores with high carbon organic content is growing. Because carbon organic matter has natural floatability, it is easily enriched in flotation froth, thus reducing the grade and quality of the concentrate as it enters the flotation process. The changing properties of ore and the high carbon content of organic matter in the ore pose more severe challenges to traditional flotation processes. First, carbonaceous matter strongly interferes with flotation: organic carbon has excellent natural floatability, preferentially adsorbing large amounts of collectors and floating with the froth, severely polluting copper concentrate and reducing concentrate grade. Second, traditional high-alkali sulfur suppression and carbon removal objectives contradict each other. Under high alkali conditions, carbonaceous organic matter is more prone to mudding and stickiness, resulting in the mixing of copper, sulfur, and carbon phases and a sharp decline in separation efficiency. Third, existing low-alkali processes are insufficient for the recovery and utilization of copper-sulfur ores containing carbonaceous organic matter. Existing low-alkali sulfur suppression technology only solves the sulfur suppression problem and cannot simultaneously achieve efficient carbon removal, and carbonaceous organic matter will still worsen flotation indicators. Fourth, existing processes are too simplistic. Conventional sulfur suppression and copper flotation or decarbonization and sulfur suppression are all unidirectional separations, which are difficult to deal with complex ore conditions where carbon and sulfur coexist and are intertwined, easily leading to copper loss, failure to reduce sulfur, and incomplete carbon removal. Summary of the Invention
[0003] The purpose of this invention is to provide a method for desulfurization and carbon removal separation of high-carbon organic copper-sulfur ore using a low-alkali process.
[0004] The objective of this invention is achieved as follows: the method for desulfurization and carbon removal separation of high-carbon organic copper-sulfur ore using a low-alkali process includes roughing, positive removal of some carbon organic matter, and reverse carbon removal steps of copper suppression and carbon floating, specifically including: A. Preliminary selection: 1) Crush and grind the raw ore to a fineness of -0.074mm, accounting for 55~70%, adjust the slurry concentration to 30~35%, and transfer it into the flotation cell for slurry preparation; 2) Add a pulp conditioner to the flotation cell to adjust the pH of the pulp for flotation to 8.5~10; 3) Low-alkali sulfur inhibitor, high-efficiency copper collector and frother are added to the slurry in sequence. After roughing, copper rough concentrate a and roughing tailings b are obtained. 4) Add low-alkali sulfur inhibitor, high-efficiency copper collector and frother to rough tailings b in sequence and perform 1 to 3 stages of scavenging to obtain middlings c and tailings d. Middlings c are returned to the previous stage of operation in sequence. B. Some carbon-based organic matter is positively eliminated: 5) Re-mill the copper rough concentrate a to a fineness of -0.038mm, accounting for 80-95%, and adjust the pulp concentration to 10-20%; 6) Add low-alkali sulfur inhibitor, carbon inhibitor and high-efficiency copper collector to the slurry in sequence, and perform 1 to 3 cleaning processes to obtain carbon organic copper concentrate e and middlings f. Middlings f are returned to the previous operation. C. Reverse carbon removal by suppressing copper and floating carbon: 7) Adjust the pulp concentration of carbon organic copper concentrate e to 5~15%, add copper inhibitor and frother in sequence, and carry out separation roughing to obtain separation roughing foam g and separation tailings k; 8) Adjust the pulp concentration to 5-15% by separating the roughing froth g, add copper inhibitor in sequence and perform 2-4 copper scavenging to obtain carbon organic impurities t and middlings h. The middlings h are returned to the previous operation in sequence. 9) Add copper inhibitors to the separated tailings k in sequence and perform copper beneficiation 1 to 3 times to obtain middlings m and copper concentrate. The middlings m are returned to the previous operation in sequence. The low-alkali sulfur inhibitor is two or more of luteolin, tannin, sodium sulfite, and sodium dithiocarbamate.
[0005] The specific steps are as follows: A. Preliminary selection (1) Grinding: Crush and grind the raw ore to a fineness of -0.074mm, accounting for 55%~70%, adjust the slurry concentration to 30%~35%, and transfer it into the flotation cell for slurry preparation; (2) Pulp conditioning: Add 100~800g / t of pulp conditioning agent to the flotation cell to adjust the pH value of the pulp flotation to 8.5-10; (3) Roughing: In step (2), add 100-300 g / t of low-alkali sulfur inhibitor, 20-40 g / t of high-efficiency copper collector and 20-40 g / t of frother to the slurry in sequence. After one stage of roughing, copper rough concentrate a and roughing tailings b are obtained. (4) Scavenging: In step (3), 0-100 g / t of low-alkali sulfur inhibitor, 0-20 g / t of high-efficiency copper collector, and 0-10 g / t of frother are added sequentially to the roughing tailings. After scavenging in stages 1-3, middlings c and tailings d are obtained. Middlings c are returned to the previous operation in sequence, while tailings d enter the tailings pool and are not returned to any operation.
[0006] B. Some carbon-organic matter is positively eliminated. (5) The copper rough concentrate a from step (3) is regrinded to a fineness of -0.038 mm, accounting for 80-95%, and the flotation concentration is adjusted to 10-20%. (6) In the regrinding copper rough concentrate slurry of step (5), add 50-100 g / t of low-alkali sulfur inhibitor, 40-100 g / t of carbon inhibitor, and 0-20 g / t of high-efficiency copper collector in sequence, and perform 1-3 cleaning processes to obtain copper concentrate c and middlings f, which still contain some highly floatable carbon organic matter. Middlings f are returned to the previous operation; C. Reverse carbon removal by suppressing copper and floating carbon (7) Adjust the slurry concentration of the copper concentrate c containing carbon organic matter with very good floatability from step (6) to 5~15%, and add copper inhibitor 50~300g / t and foaming agent 0~10g / t in sequence to carry out the separation roughing of carbon organic matter and copper minerals for negative carbon removal, and obtain the separation roughing foam g and the separation "tailings" k. (8) Adjust the slurry concentration of the separation roughing foam g from step (7) to 5-15%, add copper inhibitor 0-100g / t in sequence, and perform 2-4 copper scavenging to obtain carbon organic impurities t and middlings h; return middlings h to the previous operation in sequence; (9) Add copper inhibitor 0-100g / t to the separated "tailings" k from step (7) in sequence, and perform copper beneficiation 1-3 times to obtain middlings m and copper concentrate. The middlings m are returned to the previous operation in sequence.
[0007] This invention involves grinding finely crushed ore samples (-3mm) into a slurry with a fineness of -0.074mm accounting for 55%~70%, adjusting the slurry concentration to 30%~35%, and stirring the slurry in a flotation cell while simultaneously adding a slurry conditioner, a low-alkali sulfur inhibitor, a high-efficiency copper collector, and a frother for roughing. The roughing froth is then regrinded and subjected to cleaning, during which a low-alkali sulfur inhibitor, a carbon inhibitor, and a copper collector are added sequentially. The low-alkali sulfur inhibitor reduces sulfur content, and the carbon inhibitor inhibits some of the carbonaceous organic matter, resulting in the initial improvement in copper concentrate grade. The cleaned froth undergoes further fine separation of copper minerals and carbonaceous organic matter using a reverse carbon removal method that suppresses copper and floats carbon, achieving a further improvement in copper concentrate grade. The final product is a copper concentrate with a copper grade ≥20%, and the copper loss rate in carbonaceous organic impurities is <3%. By employing a low-alkali process to reduce sulfur content and a positive and negative carbon removal method, the enrichment of pyrite in copper concentrate is reduced, achieving fine separation of carbon organic matter from copper concentrate, thereby realizing the efficient comprehensive recycling of high-carbon organic matter copper-sulfur ore.
[0008] The present invention describes a low-alkali process for separating high-carbon organic copper-sulfur ores using positive and negative carbon removal. This method, under low-alkali conditions, employs a systematic process of positive and negative joint regulation of carbon removal through the synergistic effects of "sulfurization, carbon removal, and copper preservation." This provides a low-alkali, synergistic, and efficient separation technology for the development and utilization of high-carbon organic copper-sulfur ores. It provides key technical support for the efficient development and utilization of high-copper organic copper-sulfur ores.
[0009] The technical principles and features of this invention are as follows: 1. Adding pulp conditioner to the roughing process adjusts the pulp flotation environment, reduces interference from harmful ions, especially reduces the activation effect of copper ions on pyrite, and creates favorable conditions for the flotation of copper minerals.
[0010] 2. Low-alkali sulfur inhibitors are used in roughing and cleaning operations to enhance the inhibition effect of pyrite in a low-alkali environment, reduce the large amount of pyrite floating, and create the primary conditions for improving the grade of copper concentrate.
[0011] 3. Using a high-efficiency copper collector in the roughing operation improves the selective capture of copper minerals, but has a weaker collecting effect on pyrite minerals, thus reducing the impact of high pyrite mineral flotation on process stability during the flotation cycle.
[0012] 4. Adding carbon inhibitors during the fine processing removes some carbonaceous organic matter, thereby achieving the first improvement in the grade of copper concentrate.
[0013] 5. In the fine separation of copper and carbon, a reverse carbon removal method of suppressing copper and floating carbon is adopted to achieve precise separation of carbon organic impurities and copper minerals, further reducing the impact of impurity content and improving copper flotation indicators. Attached Figure Description
[0014] Figure 1 This is a schematic diagram of the process flow of the present invention. Detailed Implementation
[0015] The present invention will be further described below with reference to embodiments, but this is not intended to limit the present invention in any way. Any modifications or substitutions made based on the teachings of the present invention shall fall within the protection scope of the present invention.
[0016] The method for desulfurization and carbon removal separation of high-carbon organic copper-sulfur ore using a low-alkali process according to the present invention includes roughing, positive removal of some carbon organic matter, and reverse carbon removal steps of copper suppression and carbon floating, specifically including: A. Preliminary selection: 1) Crush and grind the raw ore to a fineness of -0.074mm, accounting for 55~70%, adjust the slurry concentration to 30~35%, and transfer it into the flotation cell for slurry preparation; 2) Add a pulp conditioner to the flotation cell to adjust the pH of the pulp for flotation to 8.5~10; 3) Low-alkali sulfur inhibitor, high-efficiency copper collector and frother are added to the slurry in sequence. After roughing, copper rough concentrate a and roughing tailings b are obtained. 4) Add low-alkali sulfur inhibitor, high-efficiency copper collector and frother to rough tailings b in sequence and perform 1 to 3 stages of scavenging to obtain middlings c and tailings d. Middlings c are returned to the previous stage of operation in sequence. B. Some carbon-based organic matter is positively eliminated: 5) Re-mill the copper rough concentrate a to a fineness of -0.038mm, accounting for 80-95%, and adjust the pulp concentration to 10-20%; 6) Add low-alkali sulfur inhibitor, carbon inhibitor and high-efficiency copper collector to the slurry in sequence, and perform 1 to 3 cleaning processes to obtain carbon organic copper concentrate e and middlings f. Middlings f are returned to the previous operation. C. Reverse carbon removal by suppressing copper and floating carbon: 7) Adjust the pulp concentration of carbon organic copper concentrate e to 5~15%, add copper inhibitor and frother in sequence, and carry out separation roughing to obtain separation roughing foam g and separation tailings k; 8) Adjust the pulp concentration to 5-15% by separating the roughing froth g, add copper inhibitor in sequence and perform 2-4 copper scavenging to obtain carbon organic impurities t and middlings h. The middlings h are returned to the previous operation in sequence. 9) Add copper inhibitors to the separated tailings k in sequence and perform copper beneficiation 1 to 3 times to obtain middlings m and copper concentrate. The middlings m are returned to the previous operation in sequence. The low-alkali sulfur inhibitor is two or more of luteolin, tannin, sodium sulfite, and sodium dithiocarbamate.
[0017] The low-alkali sulfur inhibitor is two or more of luteolin, tannin, sodium sulfite, and sodium dithiocarbamate.
[0018] The slurry conditioner is one or more of lime, sodium hydroxide, sodium hypochlorite, and sodium carbonate.
[0019] The highly efficient copper collector is two or three of the following: thiourethane, isobutyl xanthate, and propenyl isothiourea.
[0020] The carbon inhibitor is two or more of ferric chloride, dextrin, water-soluble starch, and sodium silicate.
[0021] The copper inhibitor is composed of aminopropionate and sodium hydrosulfide.
[0022] The mass ratio of aminopropionate to sodium hydrosulfide is (2~6):(4~8).
[0023] The foaming agent is methyl isobutyl methanol and / or diethylene glycol butyl ether.
[0024] The present invention will be further described below with reference to specific embodiments: Example 1
[0025] (1) Grinding: Take raw ore A, which contains 0.3% copper and 1.68% sulfur. Crush and grind the raw ore to a fineness of -0.074mm, accounting for 65%. Adjust the slurry concentration to 30% and transfer it to the flotation tank for slurry preparation. (2) Pulp conditioning: Add 500g / t of pulp potential conditioner to the flotation cell to adjust the pH value of the pulp flotation to 9; (3) Roughing: In step (2), 100g / t of low-alkali sulfur inhibitor, 40g / t of high-efficiency copper collector and 30g / t of frother are added to the slurry in sequence. After one roughing stage, copper rough concentrate a and roughing tailings b are obtained. (4) Scavenging: 50 g / t of low-alkali sulfur inhibitor, 10 g / t of high-efficiency copper collector, and 10 g / t of frother are added sequentially to the roughing tailings in step (3). After one stage of scavenging, middlings c and tailings d are obtained. Middlings c are returned to the previous stage of operation in sequence, while tailings d enter the tailings pool and are not returned to any operation.
[0026] B. Forward carbon removal of some carbon-organic compounds (5) The copper rough concentrate a from step (3) is regrinded to a fineness of -0.038 mm, accounting for 85%, and the flotation concentration is adjusted to 15%. (6) In the regrinding copper rough concentrate slurry of step (5), add 50+30g / t of low-alkali sulfur inhibitor, 40+20g / t of carbon inhibitor, and 10+5g / t of high-efficiency copper collector in sequence, and perform two cleaning processes to obtain copper concentrate c and middlings f, which still contain some carbon organic matter with very good floatability. Middlings f are returned to the previous operation; C. Reverse carbon removal by suppressing copper and floating carbon (7) Adjust the slurry concentration of the copper concentrate c containing carbon organic matter with very good floatability from step (6) to 15%, add 300g / t of copper inhibitor and 10g / t of foaming agent in sequence, and carry out the separation roughing of carbon organic matter and copper minerals for negative carbon removal to obtain separation roughing foam g and separation "tailings" k. (8) Adjust the slurry concentration of the separation roughing foam g from step (7) to 10%, and add copper inhibitor 100+40g / t in sequence for two copper scavenging to obtain carbon organic impurities t and middlings h; return middlings h to the previous operation in sequence; (9) The separated "tailings" k from step (7) is added sequentially with copper inhibitor 100+30g / t, and copper is selected twice to obtain middlings m and copper concentrate. Middlings m is returned sequentially to the previous stage of operation. The copper grade of the copper concentrate is 21.63%, and the copper recovery rate is 88.02%. Compared with the conventional lime-suppressed sulfur process without carbon removal, the copper grade is increased by 8 percentage points.
Claims
1. A method for desulfurization and carbon removal separation of high-carbon organic copper-sulfur ore using a low-alkali process, characterized in that, The aforementioned method for desulfurization and carbon removal separation in low-alkali processes for high-carbon organic copper-sulfur ores includes roughing, positive removal of some carbon organic matter, and reverse carbon removal steps of copper suppression and carbon flotation. Specifically, it includes: A. Preliminary selection: 1) Crush and grind the raw ore to a fineness of -0.074mm, accounting for 55~70%, adjust the slurry concentration to 30~35%, and transfer it into the flotation cell for slurry preparation; 2) Add a pulp conditioner to the flotation cell to adjust the pH of the pulp for flotation to 8.5~10; 3) Low-alkali sulfur inhibitor, high-efficiency copper collector and frother are added to the slurry in sequence. After roughing, copper rough concentrate a and roughing tailings b are obtained. 4) Add low-alkali sulfur inhibitor, high-efficiency copper collector and frother to rough tailings b in sequence and perform 1 to 3 stages of scavenging to obtain middlings c and tailings d. Middlings c are returned to the previous stage of operation in sequence. B. Some carbon-based organic matter is positively eliminated: 5) Re-mill the copper rough concentrate a to a fineness of -0.038mm, accounting for 80-95%, and adjust the pulp concentration to 10-20%; 6) Add low-alkali sulfur inhibitor, carbon inhibitor and high-efficiency copper collector to the slurry in sequence, and perform 1 to 3 cleaning processes to obtain carbon organic copper concentrate e and middlings f. Middlings f are returned to the previous operation. C. Reverse carbon removal by suppressing copper and floating carbon: 7) Adjust the pulp concentration of carbon organic copper concentrate e to 5~15%, add copper inhibitor and frother in sequence, and carry out separation roughing to obtain separation roughing foam g and separation tailings k; 8) Adjust the pulp concentration to 5-15% by separating the roughing froth g, add copper inhibitor in sequence and perform 2-4 copper scavenging to obtain carbon organic impurities t and middlings h. The middlings h are returned to the previous operation in sequence. 9) Add copper inhibitors to the separated tailings k in sequence and perform copper beneficiation 1 to 3 times to obtain middlings m and copper concentrate. The middlings m are returned to the previous operation in sequence. The low-alkali sulfur inhibitor is two or more of luteolin, tannin, sodium sulfite, and sodium dithiocarbamate.
2. The method for desulfurization and carbon removal separation of high-carbon organic copper-sulfur ore using a low-alkali process according to claim 1, characterized in that, The slurry conditioner is one or more of lime, sodium hydroxide, sodium hypochlorite, and sodium carbonate.
3. The method for desulfurization and carbon removal separation of high-carbon organic copper-sulfur ore using a low-alkali process according to claim 1, characterized in that, The highly efficient copper collector is two or three of the following: thiourethane, isobutyl xanthate, and propenyl isothiourea.
4. The method for desulfurization and carbon removal separation of high-carbon organic copper-sulfur ore using a low-alkali process according to claim 1, characterized in that, The carbon inhibitor is two or more of ferric chloride, dextrin, water-soluble starch, and sodium silicate.
5. The method for desulfurization and carbon removal separation of high-carbon organic copper-sulfur ore using a low-alkali process according to claim 1, characterized in that, The copper inhibitor is composed of aminopropionate and sodium hydrosulfide.
6. The method for desulfurization and carbon removal separation of high-carbon organic copper-sulfur ore using a low-alkali process according to claim 5, characterized in that, The mass ratio of aminopropionate to sodium hydrosulfide is (2~6):(4~8).
7. The method for desulfurization and carbon removal separation of high-carbon organic copper-sulfur ore using a low-alkali process according to claim 1, characterized in that, The foaming agent is methyl isobutyl methanol and / or diethylene glycol butyl ether.