A process for rolling φ4.5mm wire rod from a 180mm square billet of low-carbon DT430L stainless steel.
By combining 1020℃ low-temperature heating and slow-speed rolling with refined control throughout the entire production line, the problems of instability and low yield in small-scale rolling of low-carbon DT430L stainless steel have been solved, achieving high-precision and high-efficiency production to meet the needs of downstream users.
Patent Information
- Application Number
- CN202611204334.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-10
- Publication Date
- 2026-11-17
AI Technical Summary
Low-carbon DT430L stainless steel suffers from problems such as unstable rolling, low dimensional accuracy, poor surface quality, unstable wire drawing, and low yield during the 4.5mm small-gauge high-speed wire rod rolling process, making it difficult to meet the needs of downstream users.
The rolling process employs a low-temperature heating of 1020℃, a speed reduction rolling (70m/s~75m/s) rolling, and an 8-meter short billet, combined with a fully refined closed-loop control of material shape, tension, and speed. It also incorporates high-end imported equipment such as the German LOI heating furnace, the Italian Danieli continuous rolling mill, and the American Morgan finishing mill, using triple coupling control to solve the challenges in the rolling process.
It achieves high-stability rolling, with high dimensional accuracy and smooth surface of finished products, and a yield rate of over 94.5%, which can directly reduce the number of downstream processing passes and lower costs.
Smart Images

Figure CN123102735A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of metal pressure processing technology, specifically relating to a high-speed wire rod rolling process, which is particularly suitable for rolling φ4.5mm wire rod from a 180mm square billet of low-carbon DT430L stainless steel. Background Technology
[0002] The main equipment in this production line includes: one walking beam furnace from LOI (Germany), a 22-stand continuous rolling mill from Danieli (Italy), and a 10-stand finishing mill and 4-stand finishing mills from Morgan (USA). The reducing and sizing mill is equipped with an online diameter measuring instrument, online flaw detector, controlled rolling and cooling system, wire drawing machine, Stellmore line, online solution treatment furnace, and online slow cooling furnace. It can produce a wide range of steel grades, including austenitic and non-austenitic steels. High-end special steels such as stainless steel, ferritic stainless steel, martensitic stainless steel, valve steel, spring steel, bearing steel, alloy structural steel, alloy tool steel, high-speed tool steel, cold heading steel, and free-cutting steel. Wire rod. Low-carbon DT430L ferritic stainless steel, due to its high resistance to high-temperature deformation and large elongation, is highly susceptible to folding, breakage, steel piling, and head defects during the rolling of 4.5mm small-diameter high-speed wire rod. Problems such as uneven tail size, disordered wire spinning, and rapid wear of the wire spinning tube result in poor stability during conventional 85m / s high-speed rolling, while slowing down the rolling speed easily leads to large fluctuations in the bar size and low yield, failing to meet the requirements. Downstream users have a need to reduce the number of drawing passes and improve efficiency, but there is no mature and stable large-scale production process available in China. Summary of the Invention
[0003] This invention discloses a process for rolling φ4.5mm wire rod from a 180mm square billet of low-carbon DT430L stainless steel. The purpose is to solve the problems of unstable rolling of φ4.5mm specification of medium and low carbon DT430L stainless steel, low dimensional accuracy, poor surface quality, unstable wire drawing state, and many downstream processing passes in the existing production process. Technical solution: The rolling process uses 180mm×180mm low-carbon DT430L stainless steel continuously cast square billets with a carbon content of no more than 0.03% by mass as raw materials. It adopts a triple coupling control of 1020℃ low-temperature heating + speed reduction (70m / s~75m / s) rolling + billet length of 8m, combined with the whole line's refined material shape, tension and speed closed-loop control. The specific process is as follows: 180 square billet (8m) → 1020℃ low-temperature heating → high-pressure water descaling → Danieli 22 Continuous rolling → Morgan finishing mill → Morgan sizing → controlled cooling → wire drawing → Stellmore wire → coiling → φ4.5mm finished product (see...) Figure 1 ); 1) Heating and descaling The German LOI walking beam furnace is used, with a heating temperature of 1020℃ for 180 square billets. The billet length is shortened from the conventional 9m to 8m, reducing the temperature difference between the head and tail and dimensional fluctuations. After high-pressure water descaling, the billets enter the Danieli 22-stand continuous rolling mill. 2) Control of primary rolling mill stands 1-22 To cool the rolling process, an online induction heating furnace is used for supplemental heating; stands 1-12 use micro-tension rolling, and stands 13-22 use looper rolling; the material profile for finishing rolling in stand 22 is controlled at around 14.5mm to compensate for the large width of DT430L stainless steel; the CP3 system adjusts the speed and looper height of stand 22 to the optimal state of no piling up or pulling, and full speed. 3) Finishing mill control The finishing mill uses a 10-stand Morgan mill from the United States; the material height of the 23 stands is controlled at around 9.8mm, and excessive steel pulling is strictly prohibited. Roll rings must be replaced in a timely manner if they are worn; the ovality of the 32 stands is controlled at 0.4mm to 0.5mm to avoid the head ears affecting the sizing and reducing; the cross-sectional area for sizing and reducing is controlled at 27.2mm² to 27.7mm². 4) Control of reducing and sizing unit The Morgan 4-stand reduction and sizing mill unit is used, and the sequence of the pass pattern is: ellipse – circle – olive circle – circle; Inspection benchmark roll gap: 1.3mm for frame 33, 1.3mm for frame 34, 1.7mm for frame 35, and 1.7mm for frame 36; During production, the online diameter measuring instrument, intelligent pinch roller, and spinning machine status are adjusted in real time to stabilize the stacking relationship between the 34th and 35th frames. When the finished material shape is regular but the spinning speed is too fast, the 35th and 36th frames are pressed to increase the sensing speed of the pinch roller and optimize the spinning state. 5) Intelligent pinch roller control The closing degree is set at 1.5mm to 2mm, and the production of DT430L series stainless steel mainly uses loose clamping. 6) CP3+PDA speed closed-loop control Rolling speed is 70m / s to 75m / s; during normal production: the spinning machine speed is controlled between 0% and -3%, and the ratio of the intelligent pinch roller sensing speed to the set speed is controlled between 1.5% and 3%. Cooling and finished products After rolling, the wire is processed through a controlled rolling and cooling device, a wire drawing machine, a Stellmore line, and online slow cooling / solution treatment to be wound into φ4.5mm finished wire rods. Invention and Innovation 1) The first-ever triple coupling control of 1020℃ low-temperature heating + speed reduction (70m / s~75m / s) rolling + 8-meter short billet solves the industry problems of low carbon DT430L stainless steel being wide, easy to fold, stacking steel, and uneven head and tail dimensions from the source. 2) Establish a complete and precise control system of Danieli roughing mill + Morgan finishing mill + Morgan sizing and reducing + CP3 / PDA intelligent speed regulation to adapt to high-end imported equipment for stable production of small-specification stainless steel wire. 3) The finished product has high dimensional accuracy, good roundness and smooth surface, which can directly reduce the number of drawing steps for downstream users, greatly reducing costs and increasing efficiency. Beneficial effects 1) Thoroughly solve common industry problems such as wide and large span, folding, breakage, steel stacking, uneven size, and messy wire splicing of φ4.5mm low carbon DT430L stainless steel; 2) It has good rolling stability, can be mass-produced, and has a yield rate of over 94.5%; 3) The finished strips are uniform and have excellent surface quality, directly reducing one drawing step and significantly lowering the user's processing costs; 4) It is the only domestic production process technology that can stably and massively produce this steel grade and specification. Attached Figure Description
[0004] Figure 1 This is a process flow diagram of the present invention. Detailed Implementation
[0005] The present invention will be described in detail with reference to the accompanying drawings. Example 1 Steel grade DT430L, specification 4.5mm; heat number 2510602329; chemical composition: carbon: 0.036%; chromium: 16.71%; manganese: 0.40%; heating temperature 1020℃; rolling speed 72m / s; 26 pieces rolled, 47.19 tons, yield 94.8%. Example 2 Steel grade DT430L, specification 4.5mm; heat number 2510602332; chemical composition: carbon: 0.034%; chromium: 16.75%; manganese: 0.37%; heating temperature 1020℃; rolling speed 72m / s; 29 pieces rolled, 53.505 tons, yield 96.0%. Example 3 Steel grade DT430L, specification 4.5mm; heat number 2510602331; chemical composition: carbon: 0.036%; chromium: 17.00%; manganese: 0.37%; heating temperature 1020℃; rolling speed 71m / s; 24 pieces rolled, 44.28 tons, yield 96.7%. Example 4 Steel grade DT430L, 4.5mm diameter; heat number 2510602330; chemical composition: carbon: 0.028%; chromium: 16.76%; manganese: 0.39%; heating temperature 1020℃; rolling speed 71m / s; 27 pieces rolled, 47.97 tons, yield 96.5%. Example 5 Steel grade DT430L, 4.5mm diameter; heat number 266001051A; chemical composition: carbon: 0.037%; Chromium: 16.66%; Manganese: 0.34%; Heating temperature: 1020℃; Rolling speed: 73m / s; 23 strips rolled, 42.435 tons; Yield: 94.9%.
Claims
1. A process for rolling of low carbon DT430L stainless steel 180 mm square billet to φ4.5 mm wire rod, characterized by, The rolling process uses 180mm×180mm low-carbon DT430L stainless steel continuous casting square billets with a carbon content of no more than 0.03% by mass as raw materials. It adopts a triple coupling control of 1020℃ low-temperature heating + rolling speed reduction of 70m / s~75m / s + billet length of 8m, combined with the whole line's refined material shape, tension, and speed closed-loop control. The specific process is as follows: 180 square billet (8m) → 1020℃ low temperature heating → high pressure water descaling → Danieli 22-stand continuous rolling → Morgan finishing rolling → Morgan sizing → controlled cooling → wire drawing → Steyrmo line → coiling → φ4.5mm finished product; The heating and descaling process is carried out using a German LOI walking beam furnace, with a heating temperature of 1020℃ for 180 square billets. The billet length is shortened from the conventional 9m to 8m, reducing the temperature difference between the head and tail and dimensional fluctuations. After high-pressure water descaling, the billets enter the Danieli 22-stand continuous rolling mill. The control of the primary and intermediate rolling mills from stands 1 to 22 is as follows: for the cooling rolling process, the online induction heating furnace is used for heat compensation; stands 1 to 12 adopt micro-tension rolling, and stands 13 to 22 adopt looper rolling; the material profile for finishing rolling on stand 22 is controlled at around 14.5mm to compensate for the large width of DT430L stainless steel; the CP3 system adjusts the speed and looper height of stand 22 to the optimal state of no piling up or pulling, and the speed is fully reached; The finishing mill control is as follows: the finishing mill adopts a 10-stand finishing mill from Morgan in the United States; the material height of the 23 stands is controlled at about 9.8mm, and excessive steel pulling is strictly prohibited. The worn roll rings are replaced in time; the ellipticity of the 32 stands is controlled at 0.4mm~0.5mm to avoid the head ears affecting the sizing and reducing; the cross-sectional area for sizing and reducing is controlled at 27.2mm²~27.7mm². The sizing and reducing mill control adopts a Morgan 4-stand sizing and reducing mill, with the die pattern sequence being: elliptical – circular – olive-shaped – circular. The benchmark roll gaps for inspection are: 1.3mm for frame 33, 1.3mm for frame 34, 1.7mm for frame 35, and 1.7mm for frame 36. During production, adjustments are made in real time based on the online diameter measuring instrument, intelligent pinch rollers, and the status of the spinning machine, with a focus on stabilizing the stacking relationship between frames 34 and 35. When the finished material shape is regular but the spinning speed is too fast, the material is pressed down on frames 35 and 36, the sensing speed of the pinch rollers is increased, and the spinning state is optimized. Intelligent pinch roll control: the closing degree is set to 1.5mm~2mm, and the production of DT430L series stainless steel mainly uses loose pinching; CP3+PDA speed closed-loop control: rolling speed is 70m / s to 75m / s; the ratio of the intelligent pinch roll sensing speed to the set speed is controlled at 1.5% to 3%; The controlled cooling, wire drawing, and finished product process: After rolling, the wire is controlled by a controlled rolling and cooling device, the wire drawing speed is controlled at 0% to -3%, the Stelmo line is used, and online slow cooling / solution treatment is performed before winding into φ4.5mm finished wire rods.
2. A process for rolling of 180 mm square bloom of low carbon DT430L stainless steel to φ 4.5 mm wire rod as claimed in claim 1 wherein, Furnace number 2510602329; Chemical composition: Carbon: 0.036%; Chromium: 16.71%; Manganese: 0.40%; Heating temperature 1020℃; Rolling speed 72m / s; 26 strips rolled, 47.19 tons, yield 94.8%.
3. A process for rolling of low carbon DT430L stainless steel 180 mm square billet to φ 4.5 mm wire rod as claimed in claim 1, wherein the process is characterized by, Furnace number 2510602332; Chemical composition: Carbon: 0.034%; Chromium: 16.75%; Manganese: 0.37%; Heating temperature 1020℃; Rolling speed 72m / s; 29 strips rolled, 53.505 tons, yield 96.0%.
4. A process for rolling of low carbon DT430L stainless steel 180 mm square billet to φ 4.5 mm wire rod as claimed in claim 1, wherein, Furnace number 2510602331; Chemical composition: Carbon: 0.036%; Chromium: 17.00%; Manganese: 0.37%; Heating temperature 1020℃; Rolling speed 71m / s; 24 strips rolled, 44.28 tons, yield 96.7%.
5. A process for rolling of low carbon DT430L stainless steel 180 mm square billet to φ 4.5 mm wire rod as claimed in claim 1, wherein the process is characterized by, Furnace number 2510602330; Chemical composition: Carbon: 0.028%; Chromium: 16.76%; Manganese: 0.39%; Heating temperature 1020℃; Rolling speed 71m / s; 27 strips rolled, 47.97 tons, yield 96.5%.
6. A method for rolling low-carbon DT430L stainless steel 180mm square billets according to claim 1 A φ 4.5 mm rod process, characterized in that, Furnace number 266001051A; Chemical composition: Carbon: 0.037%; Chromium: 16.66%; Manganese: 0.34%; Heating temperature 1020℃; Rolling speed 73m / s; 23 strips rolled, 42.435 tons; Yield 94.9%.