A metal wire processing technology

By employing multiple drawing and annealing processes, especially by adjusting the furnace temperature of the third annealing to the range of 978℃ to 982℃, the tensile strength and elongation issues of the frame wire were resolved, the surface quality and cross-sectional condition were improved, and the finished product requirements of the frame wire were met.

CN123102767APending Publication Date: 2026-11-17TANGSHAN EVERBRIGHT GALAXY IND & TRADE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611493642.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-23
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies make it difficult to simultaneously meet the requirements of tensile strength and elongation when processing frame wires. The surface gloss, uniformity of wire color, and cross-sectional structure are not ideal, and the strength fluctuates greatly within the same batch.

Method used

The process involves multiple drawing and annealing steps, with one additional drawing and one additional annealing step. The furnace temperature for the third annealing step is adjusted to the range of 978℃ to 982℃, with 980℃ being preferred. Combined with appropriate annealing time and wire speed, the degree of heating and recrystallization effect of the wire are controlled.

Benefits of technology

It achieves both tensile strength and elongation while meeting the requirements of finished products, and the surface quality and cross-sectional condition meet the requirements for decorative use. The strength fluctuation within the same batch is narrowed, and the elongation has a margin.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102767A_ABST
    Figure CN123102767A_ABST
Patent Text Reader

Abstract

This invention discloses a metal wire processing technology, belonging to the field of picture frame wire processing technology. The process includes: S100, drawing the wire once and annealing it once at a furnace temperature of 1050℃; S200, drawing the annealed wire a second time and annealing it a second time at a furnace temperature of 1050℃; S300, drawing the annealed wire a third time and annealing it a third time at a furnace temperature of 978-982℃, so that the surface quality and cross-sectional condition meet decorative requirements, while narrowing the strength fluctuation within the same batch and allowing for a margin in elongation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of picture frame wire processing technology, specifically relating to a metal wire processing technology. Background Technology

[0002] Decorative stainless steel wire is used for exposed decorative parts such as mirror frames, and is known in the industry as mirror frame wire. This wire is produced by drawing austenitic stainless steel rod through a process of progressively reducing its diameter. During drawing, the grains elongate along the drawing direction, work hardening gradually accumulates, increasing tensile strength while decreasing plasticity. To allow subsequent drawing passes to continue, the wire needs to be annealed between passes to allow recrystallization, eliminating work hardening and restoring plasticity. The surface of the mirror frame wire after subsequent bending and forming becomes the finished surface. Decorative applications have specific requirements for the surface gloss, uniformity of wire color, and fineness of the cross-sectional structure, and also impose limitations on surface abrasion and scratches.

[0003] The industry standard for processing this type of wire is to perform two drawing operations and two annealing operations before finishing the product, with each annealing operation conducted at the same furnace temperature of 1050℃. Taking 304HC wire with a diameter of φ2.4 mm to φ1.6 mm as an example, the wire processed according to the above method has a tensile strength of 645 to 660 MPa, with a strength fluctuation of 15 to 20 MPa within the same batch, an elongation of approximately 45%, a matte to grayish-white surface, and a rough, coarse-grained cross-section.

[0004] For decorative wires, elongation, surface color, and cross-sectional structure are all important indicators: elongation affects whether the wire can withstand deformation without cracking during subsequent bending and forming; surface color affects the appearance of the wire; and cross-sectional structure affects the fineness and consistency of the wire. The fluctuation range of tensile strength within the same batch affects the stability of the wire during continuous forming. However, the wires treated according to the above methods have unsatisfactory elongation, surface color, and cross-sectional structure, and the strength fluctuation range within the same batch is also large. It is difficult to improve the elongation, improve the surface color and cross-sectional structure, and reduce the strength fluctuation.

[0005] Therefore, a metal wire processing technology is needed to ensure that the wire meets the requirements of finished product in terms of tensile strength and elongation, while also meeting the requirements for decorative purposes in terms of surface gloss, wire color uniformity, and cross-sectional structure. Summary of the Invention

[0006] The purpose of this invention is to provide a metal wire processing technology so that the wire meets the requirements of finished product in terms of tensile strength and elongation, while also meeting the requirements of decorative use in terms of surface gloss, wire color uniformity and cross-sectional structure.

[0007] To achieve the above objectives, embodiments of the present invention provide a metal wire processing technology, including: S100, drawing the wire once and annealing it once in a furnace at a temperature of 1050°C; S200: The wire after the first annealing is drawn again and then annealed again in a furnace at 1050℃. S300 involves drawing the wire after secondary annealing three times and then annealing it three times in a furnace at a temperature of 978-982℃.

[0008] One possible implementation also includes: S400 involves drawing the wire after three annealing processes four times, followed by four annealing processes at a furnace temperature of 978-982℃.

[0009] In one possible implementation, the furnace temperature is 980°C during the three annealing processes.

[0010] In one possible implementation, the furnace temperature is 980°C during the four annealing processes.

[0011] In one possible implementation, the annealing time of the wire in the furnace is 58s~62s during a single annealing process, and the wire speed is 7.9m / min-8.1m / min.

[0012] In one possible implementation, during the secondary annealing, the annealing time of the wire in the furnace is 46.5s~50s, and the wire speed is 9.9m / min~10.1m / min.

[0013] In one possible implementation, during the three annealing processes, the annealing time of the wire in the furnace is 135.5s to 138s, and the wire speed is 3.4m / min to 3.65m / min.

[0014] In one possible implementation, during the four annealing processes, the annealing time of the wire in the furnace is 119s~121.5s, and the wire speed is 3.95m / min~4.1m / min.

[0015] The significant technical effect of this invention is as follows: Compared with the conventional method (two drawing and two annealing cycles, each annealing at 1050℃), this example improves surface quality and cross-sectional condition while simultaneously meeting the tensile strength and elongation requirements of the finished product. The conventional method produces wire with a matte to grayish-white surface and a rough, coarse-grained cross-section. In this embodiment, the wire after three annealing cycles has a bright surface with a metallic luster and a fine cross-section. The improvement in surface and cross-sectional condition comes from the third annealing. The wire diameter for the third annealing is φ2.0 mm, which has a larger specific surface area than the wire annealed in the first two cycles. If annealed at 1050℃, the excessive heat would increase grain growth and surface oxidation accumulation during the annealing time. By lowering the furnace temperature to the range of 978℃ to 982℃, the degree of grain growth and surface oxidation is reduced while recrystallizing, thus improving the surface and cross-section. In other words, by adding a drawing and an annealing process to the conventional method, and setting the furnace temperature for the third annealing to be within the range of 978℃ to 982℃ (980℃ in this example), the surface quality and cross-sectional condition can meet the requirements for decorative purposes, while also narrowing the strength fluctuations within the same batch and allowing for a margin in elongation. Attached Figure Description

[0016] To more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0017] Figure 1 This is a schematic flowchart of a metal wire processing procedure involving three annealing processes and three drawing processes, as described in one embodiment of the present invention. Figure 2 This is a schematic flowchart of a metal wire processing technology involving four annealing and four drawing processes in one embodiment of the present invention. Figure 3 This is a comparison chart of metal wire products that have undergone four annealing and four drawing processes versus products from the traditional method that have undergone two annealing and two drawing processes. Detailed Implementation

[0018] The embodiments of the technical solution of this application will now be described in detail with reference to the accompanying drawings. These embodiments are only used to more clearly illustrate the technical solution of this application and are therefore merely examples, and should not be used to limit the scope of protection of this application.

[0019] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains; the terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the application; the terms “comprising” and “having”, and any variations thereof, in the specification, claims, and foregoing description of the drawings are intended to cover non-exclusive inclusion.

[0020] In the description of the embodiments of this application, technical terms such as "first" and "second" are used only to distinguish different objects and should not be construed as indicating or implying relative importance or implicitly specifying the number, specific order, or primary and secondary relationship of the indicated technical features. In the description of the embodiments of this application, "multiple" means two or more, unless otherwise explicitly defined.

[0021] In this document, the term "embodiment" means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of this application. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments.

[0022] In the description of the embodiments of this application, the term "and / or" is merely a description of the association relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A existing alone, A and B existing simultaneously, and B existing alone. Additionally, the character " / " in this document generally indicates that the preceding and following related objects have an "or" relationship. In the description of the embodiments of this application, the term "multiple" refers to two or more (including two), similarly, "multiple groups" refers to two or more groups (including two groups), and "multiple pieces" refers to two or more pieces (including two pieces).

[0023] In the description of the embodiments of this application, the technical terms "center," "longitudinal," "lateral," "length," "width," "thickness," "upper," "lower," "front," "rear," "left," "right," "vertical," "horizontal," "top," "bottom," "inner," "outer," "clockwise," "counterclockwise," "axial," "radial," and "circumferential" indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are only for the convenience of describing the embodiments of this application and simplifying the description, and are not intended to indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on the embodiments of this application.

[0024] In the description of the embodiments in this application, unless otherwise expressly specified and limited, technical terms such as "installation," "connection," "joining," and "fixing" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral part; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium. It can be the internal connection between two components or the interaction between two components.

[0025] When decorative stainless steel wire is used on exposed decorative parts such as mirror frames, its surface is the appearance surface. For this type of wire, elongation, tensile strength, surface quality, and cross-sectional condition are all important indicators, and these four are interrelated: elongation affects whether the wire can withstand deformation without cracking during subsequent bending and forming; tensile strength affects whether the wire can maintain its shape during assembly and use; surface quality affects the appearance of the wire; and cross-sectional condition affects the fineness of the wire and the consistency of different sections of wire within the same batch. Decorative applications have corresponding requirements for the surface gloss, uniformity of wire color, and fineness of cross-sectional structure, and there are also corresponding restrictions on surface abrasion and scratches. It should be noted that the above four indicators are not independent of each other. Selecting a value for one parameter often changes another indicator simultaneously. Therefore, the determination of each process parameter needs to take multiple aspects into account.

[0026] In the relevant processing method, the wire rod is drawn from coils in multiple passes to gradually reduce its diameter. Drawing causes the grains to elongate along the drawing direction, leading to accumulated work hardening and a decrease in plasticity. Therefore, annealing is performed between passes to allow recrystallization and restore plasticity. This processing method involves two drawing passes and two annealing passes before the finished product is finished, with each annealing pass using the same furnace temperature of 1050℃. Wire rods processed in this way do not have ideal surface conditions and cross-sectional microstructure, exhibit significant strength fluctuations within the same batch, and show discrepancies between tensile strength and elongation requirements and the final product specifications.

[0027] After setting requirements for various properties of wire for decorative applications, ensuring that all four properties are met simultaneously becomes a problem. Because these four properties are interrelated, the parameters during processing often cannot be determined independently; changing one parameter can alter the trends of the others, potentially improving one property while worsening another. Wire processing involves multiple cycles of drawing and annealing. Adjustable parameters include the number of drawing and annealing cycles, the furnace temperature for each annealing cycle, the annealing time in the furnace, and the wire speed. Among these, the number of drawing and annealing cycles and the furnace temperature for each annealing cycle have the greatest impact on the microstructure and surface condition after each annealing. The following section, starting from conventional practices, describes various possible methods and their results to determine suitable processing parameters.

[0028] Based on conventional methods, the first thing that comes to mind is to increase the number of drawing and annealing cycles. Specifically, the number of drawing and annealing cycles is increased from two to three, with each annealing cycle still using the conventional furnace temperature of 1050℃. The properties of the wire obtained by this method are shown in Table 1.

[0029] Table 1

[0030] In Table 1, the tensile strength is the measured range of multiple samples in the same batch. The strength fluctuation is relatively poor within the same batch.

[0031] As shown in Table 1, after adding one drawing and one annealing cycle, the tensile strength of the wire decreased from 650-670 to 640-655, the strength fluctuation narrowed from 20 MPa to 15 MPa, and the elongation increased from 43% to 46%. However, the surface quality and cross-sectional condition after each annealing cycle did not improve. The surface of the wire after three annealing cycles was still grayish-white, and the cross-section still showed coarse, large particles. In other words, simply increasing the number of drawing and annealing cycles and using the same furnace temperature for each annealing cycle cannot achieve the surface quality and cross-sectional condition required for decorative applications.

[0032] To further adjust the parameters, it is necessary to first understand the basic principles of annealing. Cold drawing elongates the grains of the wire along the drawing direction, increases the dislocation density, and raises the strength of the wire while decreasing its plasticity. Heating the wire to above the recrystallization temperature allows atomic diffusion to occur, the deformed structure first recovers, then forms new equiaxed grains that gradually grow, and residual work hardening is eliminated, thus restoring plasticity. The furnace temperature determines two things in this process: first, the extent to which recrystallization and microstructure homogenization can proceed; the higher the furnace temperature, the faster the atomic diffusion, the more complete the recrystallization, and the more thoroughly the residual work hardening is eliminated; second, the degree of grain growth and surface oxidation after recrystallization; the higher the furnace temperature, the easier it is for the grains to grow, and the heavier the surface oxidation. It is clear that the annealing result is not only determined by the furnace temperature, but also by the actual degree of heating reached by the wire during the annealing time; the degree of heating of the wire is related not only to the furnace temperature, but also to the radiant heat received per unit volume of the wire, which is proportional to the specific surface area of ​​the wire.

[0033] The reason why increasing the number of annealing passes cannot solve the surface and cross-sectional issues lies in this. As the wire diameter decreases with each pass, the specific surface area increases accordingly. When the wire diameter decreases from φ2.7 mm to φ2.0 mm, the specific surface area increases. At the same furnace temperature and wire speed, the smaller diameter wire receives more radiant heat per unit volume, resulting in increased heating and consequently, increased grain growth and surface oxidation accumulation within the furnace. When all annealing passes are performed at the same furnace temperature, the surface and cross-sectional condition of later passes will be worse than earlier passes. Based on this principle, one way to improve surface quality and cross-sectional condition is to reduce the degree of heating of the wire. A second approach is to lower the furnace temperature of the third annealing pass from 1050℃, in addition to increasing the number of annealing passes, to compensate for the increased heating caused by the reduced wire diameter.

[0034] The exact reduction amount cannot be determined from the aforementioned principles. Conventional reasoning based on this principle suggests that the properties of the wire rod change monotonically with furnace temperature: as the furnace temperature decreases, grain growth and surface oxidation lessen, leading to improved surface quality; simultaneously, the degree of recrystallization and homogenization decreases, residual work hardening is not completely eliminated, and elongation decreases accordingly. Since these two trends are opposite, conventional reasoning treats this as a trade-off: lowering the temperature improves the surface finish at the cost of sacrificing elongation; by gradually adjusting the furnace temperature along the cooling direction, a value that balances both requirements can always be found, and this value can be calculated proportionally from existing data.

[0035] Following this hypothesis, experiments were conducted using 1000℃ and 960℃ as the furnace temperatures for the third annealing, and the results are shown in Table 2. The three groups of samples in Table 2 were taken from the same batch of material, with the same pass arrangement and wire diameter, differing only in the furnace temperature of the third annealing.

[0036] Table 2

[0037] The group in Table 2 with a furnace temperature of 1050℃ is the same as the wire after three annealings in Table 1.

[0038] As shown in Table 2, when the furnace temperature for the third annealing is 1000℃, the elongation of the wire is approximately 44%, the surface is whitish and lacks metallic luster, and the texture is relatively hard; when the furnace temperature is 960℃, the elongation of the wire is approximately 42%, the surface is bluish, and the texture is also relatively hard. However, the elongation of both is below 45%, and the surface condition and cross-sectional structure are both rough and hard; all four indicators cannot be simultaneously met. In other words, lowering the furnace temperature for the third annealing does not allow all the required indicators to be met simultaneously.

[0039] The results above show that continuing to adjust the furnace temperature according to conventional assumptions is not a viable solution. The results for both the 1000℃ and 960℃ groups are consistent with the assumption of monotonic change: as the furnace temperature decreased from 1050℃ to 1000℃ and then to 960℃, the elongation decreased from 46% to approximately 44% and 42% respectively; the surface quality did not improve with the decrease in furnace temperature, remaining whitish at 1000℃ and bluish at 960℃ – only the manifestation of failure changed. According to this assumption, to further improve the surface, the furnace temperature must be further reduced, but since the elongation has already decreased to approximately 42%, further reduction will only cause it to decrease further; to maintain the elongation, the furnace temperature must be raised back to a value close to 1050℃, which would exacerbate surface oxidation. These two requirements cannot be met simultaneously at the same furnace temperature. The conclusion drawn from conventional assumptions is that there is no usable furnace temperature for the third annealing; therefore, adjusting the furnace temperature should be abandoned, and the surface quality problem should be addressed through other means. According to this conclusion, values ​​between 1000℃ and 960℃ are also not among the candidates.

[0040] It should be noted that, based on the assumption of monotonic change, the two failures mentioned above could be attributed to the same direction. The elongation decreased sequentially with decreasing furnace temperature (46%, approximately 44%, approximately 42%), indicating that cooling reduced the softening degree and consequently impaired the elongation. The surface quality was whitish at 1000℃ and bluish at 960℃; although the two appearances were different, neither met the requirements, indicating that the surface could not be adjusted to acceptable levels along the cooling direction. According to this attribution, values ​​falling between 1000℃ and 960℃ would only yield results in between, no better than the 1000℃ group. Therefore, this range would not be considered a direction for further experimentation under conventional assumptions.

[0041] This scheme did not continue adjusting along the cooling direction, nor did it raise the furnace temperature back to the values ​​of the first two annealing processes. Instead, it selected an intermediate value between the two confirmed unqualified temperatures, specifically 978℃ to 982℃, which is between 1000℃ and 960℃. When the furnace temperature for the third annealing was taken within this range, the various properties are shown in Table 3. The samples in the 980℃ group in Table 3 and the two groups in Table 2 were taken from the same batch of material, with the same pass arrangement and wire diameter.

[0042] Table 3

[0043] As shown in Table 3, when the furnace temperature for the third annealing was within the range of 978℃ to 982℃, all the wire rod's properties exceeded the finished product requirements: the elongation of the three groups of samples was approximately 46% to 48%, all higher than the finished product requirement of 45%; the tensile strength was 625 to 645 MPa, all above 610 MPa; the surface was bright and maintained a metallic luster, and the cross-section was fine. All four properties met the requirements simultaneously at each value within this range. Among the three groups of samples, the elongation of the wire rod at a furnace temperature of 980℃ was 48%, the highest among the three temperature points, exceeding the finished product requirement by three percentage points. This result was contrary to the conventional expectation: 978℃ to 982℃ falls between two confirmed unacceptable temperatures. According to the assumption of monotonic change, values ​​falling within this range would only result in a value between 1000℃ and 960℃, with an elongation between approximately 44% and approximately 42%, and the surface quality would also fail to meet the requirements; however, the actual result was that all four properties met the requirements simultaneously within this range.

[0044] As can be seen from Tables 1 to 3, the various properties of the wire do not change monotonically with furnace temperature, but rather reach extreme values ​​around 980℃. Regarding elongation: as the furnace temperature decreases from 1050℃ to 1000℃, the elongation decreases from 46% to approximately 44%; further decreasing to 980℃, the elongation recovers to 48%; further decreasing to 960℃, it drops again to approximately 42%, showing a trend of first decreasing, then increasing, and then decreasing again. Regarding surface quality: at a furnace temperature of 1000℃, oxidation is excessive, resulting in a white surface; at 960℃, oxidation is insufficient, resulting in a bluish surface; when the furnace temperature is within the range of 978℃ to 982℃, the degree of oxidation is moderate, and the surface is bright. Plotting furnace temperature on the x-axis and elongation on the y-axis, connecting the data points forms a curve that reaches a maximum value around 980℃; the position and shape of this curve are determined by the data in Tables 1 to 3. Based on the assumption of monotonic change, values ​​falling between the two unacceptable temperatures should also be unacceptable. However, the above curve relationship shows that the range of 978℃ to 982℃, which lies between the two, allows all indicators to simultaneously meet the requirements. The curve flattens out near its maximum value, therefore, the value that allows all indicators to simultaneously meet the requirements is not limited to 980℃, but rather to a narrower range centered around 980℃; this range lies between the two confirmed unacceptable temperatures, which in this embodiment is 978℃ to 982℃.

[0045] The reason these values ​​need to be determined point-by-point through experiments is that the relationship between various properties and furnace temperature is not linear. If it were linear, the performance at intermediate temperatures could be extrapolated proportionally from the results at 1000℃ and 960℃, without the need for point-by-point experiments. Based on this relationship, the elongation at 980℃ should be around 42.5%, lower than the required 45% for the finished product and also lower than the approximately 44% at 1000℃. Therefore, 980℃, like 1000℃ and 960℃, is not usable when extrapolated linearly and is not among the candidate values. The actual results do not match this extrapolation: the measured elongation at 980℃ is 48%, about five percentage points higher than the extrapolated value. In other words, the various properties change with furnace temperature in a curved relationship, with the curve reaching a maximum near 980℃. Both sides of the maximum tend to deteriorate, while the trend near the maximum is relatively gentle. The usable values ​​lie within a narrow range near this maximum, namely 978℃ to 982℃. This range cannot be calculated proportionally from the data on both sides; it can only be determined through point-by-point testing within the range where both directions tend to deteriorate. The decay rate on both sides of the curve's maximum is also different, with faster decay on the lower temperature side and slower decay on the higher temperature side. Based on this, this embodiment provides a metal wire processing technology. This process adds a drawing and an annealing step to the conventional method, and the furnace temperature for the third annealing is set within the range of 978℃ to 982℃, preferably 980℃.

[0046] like Figure 1 As shown, the wire processing technology in this embodiment includes three sequential drawing and three annealing processes. The wire material is 304HC austenitic stainless steel. Step S100: The first drawing pass is a single drawing, where the wire is drawn from φ5.5 mm to φ2.7 mm; after drawing, it undergoes a first annealing at a furnace temperature of 1050℃. Step S200: The second drawing pass is a double drawing, where the wire is drawn from φ2.7 mm to φ2.4 mm; after drawing, it undergoes a second annealing at a furnace temperature of 1050℃. Step S300: The third drawing pass is a triple drawing, where the wire is drawn from φ2.4 mm to φ2.0 mm; after drawing, it undergoes a third annealing at a furnace temperature within the range of 978℃ to 982℃, with a preferred example of 980℃.

[0047] The furnace temperatures and corresponding wire diameters for each of the three annealing processes are shown in Table 4.

[0048] Table 4

[0049] In Table 4, the tensile strength is the measured range of multiple samples in the same batch, and the strength fluctuation is the range of tensile strength within the same batch; in the surface quality column, matte refers to a surface without metallic luster and exhibiting uniform diffuse reflection; the furnace temperature for the third annealing is 980℃ as used in this embodiment, which is within the range of 978℃ to 982℃.

[0050] The data in Table 4 show that after three drawing and three annealing processes, the tensile strength range of the wire gradually decreased from 650 to 670 MPa to 630 to 640 MPa, all of which are higher than the finished product requirement of 610 MPa. The strength fluctuation within the same batch gradually narrowed from 20 MPa to 10 MPa. The elongation increased from 43% to 48%, with 43% after the first annealing and 45% after the second annealing, which is the same as the finished product requirement of 45% without any margin. After the third annealing, it increased to 48%, exceeding the finished product requirement by three percentage points. The surface condition changed from matte to glossy. The cross-sectional condition changed from rough to smooth.

[0051] Compared to the conventional method (two drawing and two annealing cycles, each annealing at 1050℃), this example improves surface quality and cross-sectional appearance while simultaneously meeting the tensile strength and elongation requirements of the finished product. The conventional method produces wire with a matte to grayish-white surface and a rough, coarse-grained cross-section. In this embodiment, the wire after three annealing cycles has a bright surface with a metallic luster and a fine cross-section. This improvement in surface and cross-sectional appearance stems from the third annealing. The wire diameter used in the third annealing was φ2.0 mm, with a larger specific surface area than the wires annealed in the first two cycles. Annealing at 1050℃ would result in excessive heating, increasing grain growth and surface oxidation accumulation during the annealing time. By lowering the furnace temperature to between 978℃ and 982℃, the wire recrystallizes while simultaneously reducing grain growth and surface oxidation, thus improving both the surface and cross-section. In other words, by adding a drawing and an annealing process to the conventional method, and setting the furnace temperature for the third annealing to be within the range of 978℃ to 982℃ (980℃ in this example), the surface quality and cross-sectional condition can meet the requirements for decorative purposes, while also narrowing the strength fluctuations within the same batch and allowing for a margin in elongation.

[0052] In a further example, after the three drawing and three annealing processes described above, one more drawing and one more annealing process can be added, resulting in four drawing and four annealing processes sequentially. For example... Figure 2As shown, step S400: the fourth drawing pass is a quadruple drawing, where the wire is drawn from φ2.0 mm to φ1.6 mm; after drawing, it enters the fourth annealing, i.e., the fourth annealing, with the furnace temperature ranging from 978℃ to 982℃ (980℃ in this embodiment). The wire diameter for the fourth annealing is smaller than that for the third annealing, further increasing the specific surface area of ​​the wire. The furnace temperature is determined in the same way as for the third annealing: a narrow range is selected between 1000℃ and 960℃, where all values ​​within this range meet the requirements of the four indicators, with the highest elongation and the largest allowance at 980℃. When the fourth annealing uses values ​​within this range, the wire completes recrystallization while limiting grain growth and surface oxidation, maintaining a fine and bright surface quality and cross-sectional state, further improving the wire's performance. The wire diameter for the fourth annealing and the performance of the wire after the fourth annealing are shown in Table 5 and... Figure 3 As shown, Figure 3 Table 1 and 2 represent the traditional scheme, i.e., products that are drawn twice and annealed twice at a temperature of 1050℃. Table 3 and 4 represent products that are drawn four times and annealed four times. The furnace temperature used for the fourth annealing in Table 5 is within the same range as that for the third annealing. The other conditions are the same as those in Table 4.

[0053] Table 5

[0054] As shown in Table 5, after adding a fourth drawing and a fourth annealing, the tensile strength of the wire decreased from 630-640 MPa to 615-620 MPa, but remained above the finished product requirement of 610 MPa; the elongation further increased from 48% to 50%, exceeding the finished product requirement by five percentage points; the strength fluctuation within the same batch further narrowed from 10 MPa to 5 MPa, and the overall strength of the wire became more uniform; the surface condition changed from bright color to the natural color of stainless steel, and the cross-section remained fine. In other words, adding one more drawing and one more annealing on top of three drawing and three annealing processes can further narrow the strength fluctuation within the same batch, increase the elongation, and improve the wire color. The surface quality and cross-sectional condition of the wire after four annealing processes are shown in Table 5. The wire exhibits the natural color of stainless steel, and there is no visible oxide film on the surface; the furnace temperature used for the fourth annealing is within the range of 978℃ to 982℃, consistent with the furnace temperature and aperture of the third annealing process.

[0055] After determining the furnace temperature and wire diameter for each annealing cycle, the wire speed and annealing time within the furnace can be further limited. The annealing time within the furnace is determined by the ratio of the furnace length to the wire speed. In this embodiment, the furnace length is 8 meters, and the wire speed and corresponding annealing time for each annealing cycle are shown in Table 6.

[0056] Table 6

[0057] In Table 6, the wire speed is the speed at which the wire passes through the furnace body at a constant speed, and the annealing time is the residence time of the wire in the furnace body, determined by the ratio of the furnace body length to the wire speed; the two correspond to each other. In the furnace temperature column, the ranges for three-stage and four-stage annealing are listed as 978℃ to 982℃; four-stage annealing is a further example. The parameters listed in Table 6 are the value ranges for each annealing under the above conditions; the specific values ​​used in this embodiment are described below.

[0058] In this embodiment, the furnace body length of the annealing furnace is 8 meters. The line speeds used for each annealing cycle are 8 meters per minute, 10 meters per minute, 3.5 meters per minute, and 4 meters per minute, respectively, all within the corresponding ranges listed in Table 6; the corresponding annealing times are 60 seconds, 48 ​​seconds, 137 seconds, and 120 seconds, respectively, also within the corresponding ranges listed in Table 6.

[0059] The wire speed varies with both wire diameter and furnace temperature, and its value is explained as follows.

[0060] Firstly, between two annealing processes at the same furnace temperature, the wire with the smaller diameter has a higher wire feed rate and a shorter annealing time. For the first and second annealing processes, the furnace temperature is the same at 1050℃. With the wire diameter reduced from φ2.7 mm to φ2.4 mm, the wire feed rate increases accordingly from 8 m / min to 10 m / min, and the annealing time decreases from 60 seconds to 48 seconds. For the third and fourth annealing processes, the furnace temperature is within the range of 978℃ to 982℃ (980℃ in this example). With the wire diameter reduced from φ2.0 mm to φ1.6 mm, the wire feed rate increases accordingly from 3.5 m / min to 4 m / min, and the annealing time decreases from 137 seconds to 120 seconds. As the wire diameter decreases, the time required for heat penetration is proportionally shortened, allowing for a higher wire feed rate through the furnace.

[0061] Secondly, as the furnace temperature decreases, the wire speed decreases and the annealing time increases, and the increase exceeds the reduction caused by the decrease in wire diameter. Between the second and third annealing processes, the furnace temperature drops from 1050℃ to 980℃, and the wire diameter decreases from φ2.4 mm to φ2.0 mm. While the reduction in wire diameter should have shortened the annealing time by about 20%, the decrease in furnace temperature increases the time required for recrystallization and homogenization. After offsetting these factors, the annealing time still increases from 48 seconds to 137 seconds. Based on the apparent activation energy of 280 kJ / mol for the softening process, when the furnace temperature decreases from 1050℃ to 980℃, the recrystallization rate decreases to about one-quarter of that at 1050℃, and the time required to achieve the same degree of softening increases to about four times. However, the increase in the time required for recrystallization and homogenization due to the decrease in furnace temperature exceeds the reduction caused by the decrease in wire diameter, thus extending the annealing time from 48 seconds to 137 seconds.

[0062] Third, the annealing time for each annealing process is longer than the heat penetration time of the wire. After the wire enters the furnace, it needs a certain period of time to reach its temperature close to the furnace temperature. This time is determined by the thermal inertia of the wire: considering the wire as a cylinder, the time constant for its temperature to approach the furnace temperature is τ=ρ·c·d / (4h), where ρ is the density of the wire, c is the specific heat capacity of the wire, d is the wire diameter, and h is the comprehensive heat transfer coefficient between the wire and the furnace environment. Taking the density of austenitic stainless steel as 7900 kg / m³ and the specific heat capacity as 500 J / kg Kelvin, and considering that radiative heat transfer is the main method in the furnace, with a comprehensive heat transfer coefficient of 300 W / m² to 400 W / m² Kelvin, the time constant for φ2.0 mm wire is approximately 5.6 seconds, and the time required for the wire temperature to reach 95% of the furnace temperature is approximately 17 seconds; the time constant for φ1.6 mm wire is approximately 4.5 seconds, and the required time is approximately 14 seconds. The annealing time for each annealing cycle ranges from 48 to 137 seconds, several times the aforementioned heat penetration time. Since the wire spends most of its time in the furnace at furnace temperature, the annealing time is determined by the time required for recrystallization and homogenization, not by the heat penetration time. Therefore, the wire feed rate and annealing time correspond to the wire diameter and furnace temperature: smaller wire diameters and lower furnace temperatures require longer annealing times.

[0063] The precision of the wire drawing speed control is determined by the speed regulating device of the annealing furnace. When the wire drawing speed varies within the range listed in Table 6, the annealing time varies accordingly, ensuring the wire remains under heating conditions that allow recrystallization to complete without excessive grain growth or surface oxidation. When the wire drawing speed is below this range, the time the wire spends in the furnace is prolonged, resulting in excessive heating, increased grain growth and surface oxidation, and consequently, poorer surface quality and cross-sectional condition. When the wire drawing speed is above this range, the heating time in the furnace is insufficient, recrystallization and homogenization are inadequate, elongation decreases, and the texture becomes harder. The rotational speed of the traction wheel is controlled by the speed regulating device to stabilize the wire drawing speed within the corresponding range listed in Table 6 for each annealing cycle.

[0064] The annealing furnace maintains a constant temperature, and the wire passes through the furnace at a uniform speed without pausing. The constant furnace temperature is maintained by a temperature control device, which collects the temperature of the soaking zone via thermocouples. A controller adjusts the power of the heating elements based on the deviation between the collected value and the set value, keeping the temperature of the soaking zone near the set value. The wire is released by the unloading device, pulled through the soaking zone by the traction wheel, and then wound up by the take-up device. The speed of the traction wheel is controlled by a speed regulating device according to the set wire feeding speed.

[0065] The length of the soaking zone and the division of the temperature zones in the annealing furnace are determined according to the specifications of the annealing furnace. The specific type and dew point value of the protective atmosphere inside the furnace are determined according to the operating conditions of the annealing furnace and are not limited here.

[0066] The annealing furnace can be a continuous tube furnace, in which the wire passes through the soaking zone along the axis of the furnace tube; it can also be an induction heating furnace, in which the wire is heated by induced current as it passes through the induction coil; or it can be a mesh belt continuous furnace, in which the wire is laid flat on the mesh belt and passes through the soaking zone with the mesh belt. No particular limitation is made here.

[0067] The wire spools used in each drawing pass of the wire have been changed from steel spools to polymer spools. Steel spools are harder than stainless steel wire, and when the wire passes over the spool, contact stress is generated between the wire surface and the spool, making the wire surface prone to scratches. Metal shavings generated by friction between the spool and wire surfaces are also easily pressed into the wire surface. Polymer spools are less hard than the wire and have elasticity. When the wire passes over the spool, the contact stress is distributed more evenly on the contact surface, and the contact surface can deform according to the shape of the wire, thus reducing the degree of scratches and metal shaving indentation. Besides nylon, the spools can also be made of polyoxymethylene, polyurethane, or ultra-high molecular weight polyethylene; the specific materials used are not limited here.

[0068] Drawing dies are customized according to the wire diameter of each pass, and the die orifice shape matches the inlet and outlet wire diameters of each pass. When the orifice shape and wire diameter do not match, the additional shear deformation of the wire at the die inlet increases, and cracks and scratches are easily generated on the wire surface. The working area of ​​the die can be made of cemented carbide, polycrystalline diamond, or tool steel, and there is no limitation here.

[0069] During drawing, drawing fluid is supplied between the die and the wire. The drawing fluid forms a lubricating film on the contact surface and provides cooling, reducing adhesive wear between the die and the wire. The drawing fluid can be an emulsion, a synthetic fluid, or a semi-synthetic fluid; drawing fluids containing extreme pressure additives form a reaction film on the contact surface, further reducing friction in passes with large diameter reductions. In this embodiment, imported drawing fluid is used.

[0070] The specific specifications of the drawing wheel, die, and drawing fluid are selected according to the wire diameter and reduction amount for each pass, and are not limited here.

[0071] The wire is made of 304HC austenitic stainless steel. 304HC is a cold-working wire with a carbon content not exceeding 0.08%, a chromium content of 18.0% to 20.0%, a nickel content of 8.0% to 10.0%, and a copper content of 1.0% to 3.0%. The addition of copper improves the cold-working formability of the wire; during multi-pass deformation, the surface of the wire is less prone to cracking and peeling, maintaining a clean surface. Simultaneously, 304HC has low magnetism, making it less likely to attract metal shavings during subsequent assembly in decorative applications. Other cold-working austenitic stainless steels can also be used for the wire; this is not limited here.

[0072] Surface damage to the wire during multiple drawing processes is controlled separately by the drawing system. By changing the wire rollers from steel to polymer materials, customizing the dies according to the wire diameter for each pass, and supplying drawing fluid during drawing, the wire surface remains free of abrasions and scratches in each pass. This effect is independent of changes in the annealing furnace temperature.

[0073] The color of annealed wire is determined by the thickness of the surface oxide film, which varies with furnace temperature and annealing time within the furnace. At 960℃, the oxidation level is low, resulting in a thinner oxide film. The interference of light by the oxide film gives the surface a blue hue. At 980℃, the oxide film thickens further but has not yet formed a coarse oxide layer with diffuse reflection, resulting in a bright surface with a metallic luster. At 1000℃, the oxidation level is high, and the oxide layer thickens to the point where light interference is no longer dominant, resulting in a white surface that loses its metallic luster. The color change from blue to bright to white can be used as a criterion for judging whether the furnace temperature for the third and fourth annealing processes deviates from the 978℃ to 982℃ range: a blue surface indicates the furnace temperature is below this range; a white surface indicates the furnace temperature is above this range; and a bright surface indicates the furnace temperature is within this range.

[0074] After the first annealing, the wire surface has a matte finish. A matte finish refers to a surface without metallic luster, exhibiting uniform diffuse reflection. The difference between this and the three color states mentioned above is that the surfaces in the bluish, glossy, and whitish states still primarily exhibit metallic reflection, with color differences arising from the interference and absorption of the oxide film. The matte surface, however, has a thicker oxide layer and increased surface roughness, resulting in predominantly diffuse reflection and a weakened metallic luster. Wires processed using conventional methods have a matte to grayish-white surface, which does not meet the surface gloss requirements for decorative applications. By lowering the furnace temperature to the range of 978℃ to 982℃ during the third annealing, the degree of oxidation on the surface decreases, and the wire surface changes from grayish-white to glossy. After a fourth annealing, it reveals the natural color of stainless steel.

[0075] In summary, the metal wire processing technology of this embodiment works through the following four aspects: First, by adding a drawing and an annealing step to the conventional method, the total diameter reduction is distributed over more passes, reducing the diameter reduction and work hardening degree per pass, and the annealing between passes gradually homogenizes the microstructure; Second, the first two annealings are performed at 1050℃, allowing recrystallization and microstructure homogenization to be completed at a higher furnace temperature for the larger wire diameter stage, leaving plasticity reserves for subsequent drawing passes; Third, the furnace temperatures for the third and fourth annealings are taken within the range of 978℃ to 982℃ (980℃ in this embodiment), which limits grain growth and surface oxidation while completing recrystallization, thereby improving surface quality and cross-sectional condition; Fourth, the drawing-related measures ensure that the wire surface remains intact during multiple deformation passes. All of the above factors combined enable the wire to achieve a tensile strength of over 610 MPa and an elongation of over 45%, with the strength fluctuation within the same batch narrowed to 5 MPa, and the surface quality and cross-sectional condition meeting the requirements for decorative use, making it suitable for replacing imported wire.

[0076] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and not to limit them. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the spirit and scope of the technical solutions of the present invention, and all such modifications or substitutions should be covered within the scope of protection of the claims of the present invention.

Claims

1. A wire processing process for processing 304HC wire, characterized by, include: S100: The wire is drawn once and then annealed once in a furnace at 1050℃. S200: The wire after the first annealing is drawn again and then annealed again in a furnace at 1050℃. S300 involves drawing the wire after secondary annealing three times and then annealing it three times in a furnace at a temperature of 978-982℃.

2. The metal wire processing technology according to claim 1, characterized in that, Also includes: S400 involves drawing the wire after three annealing processes four times, followed by four annealing processes at a furnace temperature of 978-982℃.

3. The metal wire processing technology according to claim 2, characterized in that, During the three annealing processes, the furnace temperature was 980℃.

4. The metal wire processing technology according to claim 3, characterized in that, During the four annealing processes, the furnace temperature was 980℃.

5. The metal wire processing technology according to claim 2, characterized in that, In the first annealing process, the annealing time of the wire in the furnace is 58s~62s, and the wire speed is 7.9m / min-8.1m / min.

6. The metal wire processing technology according to claim 3, characterized in that, In the secondary annealing, the annealing time of the wire in the furnace is 46.5s~50s, and the wire speed is 9.9m / min~10.1m / min.

7. The metal wire processing technology according to claim 4, characterized in that, In the three annealing processes, the annealing time of the wire in the furnace is 135.5s to 138s, and the wire speed is 3.4m / min to 3.65m / min.

8. The metal wire processing technology according to claim 5, characterized in that, During the four annealing processes, the annealing time of the wire in the furnace is 119s~121.5s, and the wire speed is 3.95m / min~4.1m / min.