A method for preparing large-size fine-grained high-purity copper tubes with trace rare earth modification by low-temperature large deformation extrusion

By selecting the process window based on the measured material state of the furnace batch during the preparation of large-size fine-grained high-purity copper tubes modified with trace rare earth elements, and controlling the extrusion pressure and temperature history, the problems of grain control and conductivity in the prior art have been solved, and the stable preparation of fine-grained high-purity copper tubes by low-temperature large deformation extrusion has been achieved.

CN123102777APending Publication Date: 2026-11-17GUANGDONG OULE NEW METAL MATERIALS CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611546997.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-08
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies struggle to effectively control grain size and conductivity when preparing large-size, fine-grained, high-purity copper tubes modified with trace rare earth elements. Furthermore, the extrusion process fails to accurately reflect the actual material state and temperature history, leading to overload cracking and microstructure differences.

Method used

By selecting the process window based on the measured material state of the batch, controlling the extrusion pressure, demolding temperature, and high-temperature dwell time, and combining the inner wall temperature estimation and natural air cooling, the extrusion process is ensured to be carried out within the verification range, avoiding annealing and aging treatments. The final grain size and conductivity are detected to adjust the process parameters.

Benefits of technology

This method enables the preparation of fine-grained high-purity copper tubes by large deformation extrusion under low-temperature conditions, reducing the risk of overload cracking and differences in grain coarsening, and ensuring the consistency of material properties and the stability of electrical conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102777A_ABST
    Figure CN123102777A_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing large-size fine-grained high-purity copper tubes with trace rare earth modification by low-temperature large deformation extrusion. It belongs to the field of copper material casting and tube extrusion forming. In order to solve the problem of difficulty in coordinating the actual retention of rare earth and the maintenance of extrusion forming and air-cooling structure, the method matches the measured batch material state with the process window verified by hot deformation, trial extrusion and natural air-cooling tests. The extrusion data is aligned to the same tube section according to the metal volume relationship. The temperature history is established by combining the inner wall temperature estimation. The rod speed trajectory that meets the constraints of actual extrusion pressure, demolding temperature and high temperature residence time is selected. The final state grain and conductivity detection results are used to confirm or shrink the subsequent window, forming a material state, forming control and final state detection feedback relationship without annealing, solution or aging treatment after extrusion.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of copper material casting and tube extrusion forming, and in particular to a method for preparing large-size fine-grained high-purity copper tubes with trace rare earth modification by low-temperature large deformation extrusion. Background Technology

[0002] Copper tube manufacturing can employ a process route that integrates copper raw material smelting, casting, billet processing, and extrusion forming. For tubes requiring a balance between grain size and electrical conductivity, raw material composition, ingot microstructure, deformation conditions, and post-extrusion cooling are all process factors that need to be controlled. For large-diameter and thick-walled tubes, it is also necessary to ensure that the effective metal cross-sectional area of ​​the billet, the annular cross-sectional area of ​​the finished product, and the available extrusion pressure of the extrusion equipment are matched.

[0003] In the preparation of copper materials with only trace amounts of lanthanum and yttrium, the element dosage calculated based on the furnace charge cannot directly represent the measured element content in the extruded billet and finished product, and the purity of the cathode copper raw material cannot replace the copper content of the finished product. If the process selection is not related to the rare earth, oxygen content, and initial microstructure of the furnace batch material, it is difficult to determine whether the same set of nominal extrusion parameters is applicable to different furnace batches. For large-section extrusion, the nominal capacity of the equipment and the set preheating temperature cannot independently reflect the actual extrusion pressure and demolding temperature during forming.

[0004] In extrusion processes where annealing, solution treatment, or aging are not performed after extrusion, natural air cooling after demolding still affects the final microstructure. Adjusting the extrusion bar speed solely based on the demolding temperature cannot directly reflect the temperature history of the same pipe section during subsequent air cooling; for thick-walled pipes, external wall temperature measurements must be combined with internal wall temperature measurements to determine thermal history constraints. The actual material state, available extrusion pressure, and the air cooling thermal history of the same pipe section need to be included in a jointly validated framework, and the final state measurements should be fed back to the process selection for subsequent batches.

[0005] Therefore, there is a need for a low-temperature, large-deformation extrusion method for preparing large-size, fine-grained, high-purity copper tubes modified with trace rare earth elements that can overcome the shortcomings of the existing technologies. Summary of the Invention

[0006] One objective of this invention is to propose a low-temperature, large-deformation extrusion method for preparing large-size, fine-grained, high-purity copper tubes modified with trace rare earth elements. Addressing issues such as the discrepancy between the amount of trace elements added and the actual material state, the mutual constraint between the large-section extrusion load and the deformation temperature rise, and the potential impact of subsequent natural air cooling on grain retention, this invention proposes a technical solution: selecting an experimentally verified process window based on the measured material state of the batch; implementing rod speed control according to the temperature history of the same tube section; and providing feedback on the final state test results. This method uses the actual extrusion pressure, demolding temperature, and high-temperature residence time as common constraints, selecting extrusion and preheating conditions within the verified range for the corresponding material and specifications. It also sets up pause and isolation inspection measures for situations where there is no applicable window or the limits have been exceeded. Through corresponding records of material, forming, and final state tests, it provides a basis for process control to reduce overload cracking and microstructural differences in different parts of the tube.

[0007] This invention provides a method for preparing large-size, fine-grained, high-purity copper tubes with trace rare earth modification using low-temperature, large-deformation extrusion, comprising:

[0008] S1. Using high-purity copper as raw material, with only lanthanum and yttrium as alloying additives, the billet is processed into a perforated billet through smelting, casting and extrusion pre-billet treatment, and the measured material state of the furnace batch is obtained.

[0009] S2. Based on the measured material state of the furnace batch, the effective metal cross-sectional area of ​​the perforated billet, and the target tube specifications, select the applicable window from the process window verified by the test of the same material and specifications to obtain the constraints of preheating conditions, rod speed trajectory range, actual extrusion pressure, demolding temperature, and high temperature dwell time.

[0010] S3. Preheat according to the applicable window and extrude the perforated billet through the annular gap formed by the mold and the mandrel, and then air cool it naturally. No annealing, solution treatment or aging treatment is performed after extrusion. Simultaneously collect the extrusion rod displacement, actual extrusion pressure, demolding and downstream temperature.

[0011] S4. Align the collected data to the same pipe section according to the metal volume relationship, determine the temperature history by combining the internal wall temperature estimation applicable to the pipe material, select the subsequent rod speed trajectory that simultaneously meets all constraints from the rod speed trajectory range and execute it, and correct the preheating of the next billet with the execution result.

[0012] S5. Detect the grain size and conductivity of the pipe material after it has been naturally cooled to room temperature. Correlate the test results with the measured material condition and pipe section temperature history of the furnace batch to confirm or narrow the applicable window for subsequent furnace batches.

[0013] Optionally, S1 includes: using cathode copper with a purity of not less than 99.99%, vacuum induction melting at an absolute pressure of not more than 5 Pa and a temperature of 1180–1220 °C, and adding 15–45 ppm of lanthanum and 15–35 ppm of yttrium to a copper rare earth intermediate alloy, with the total of the two being 30–80 ppm, where ppm is the ratio of the mass of the added element to the total mass of the metal charge in parts per million;

[0014] After stirring and holding at a constant temperature for 8–12 minutes, semi-continuous casting of round ingots is performed.

[0015] The round ingot is held at 580-620℃ for 2.5-3.5 hours, cooled in the furnace and finished on the surface to form a perforated billet that fits with the mandrel.

[0016] The measured material condition of the furnace batch includes the lanthanum content, yttrium content, oxygen content, and initial grain size and distribution of the material taken from the same furnace batch after the billet processing before extrusion.

[0017] Optionally, S2 includes: using the measured material state of the furnace batch, the effective metal cross-sectional area of ​​the perforated billet, and the target wall thickness as test inputs, conducting hot deformation, trial extrusion, and natural air cooling tests on the same material and specifications, recording the trajectory of the preheating temperature, the rod speed as the extrusion rod displacement changes, the actual extrusion pressure, and the temperature history of the tube section, and detecting forming cracks, final grain size, and conductivity.

[0018] The test parameter combination and the range of variation covered by the test are saved as process windows, which are formed without cracks and have an average grain size of no more than 15 μm and an conductivity of no less than 100% IACS for the same final state tube. Each process window is bound to the material state range, effective metal cross-sectional area, target wall thickness, preheating conditions, rod speed trajectory range, upper limit of actual extrusion pressure, upper limit of demolding temperature, upper limit of high temperature dwell time, and temperature limit for accumulating high temperature dwell time.

[0019] The process window is selected only when the measured material condition and pipe specifications of the production batch fall within the corresponding applicable parameter range.

[0020] Furthermore, the upper limit of the actual extrusion pressure is taken as the lower limit of the value between the upper limit of the crack-free forming extrusion pressure verified by the test and the upper limit of the actual usable extrusion pressure of the extruder.

[0021] The upper limit of demolding temperature, the upper limit of high-temperature dwell time, and the temperature limit for accumulating high-temperature dwell time are determined in groups based on the temperature history of the natural air cooling test and the corresponding final state grain size and conductivity test results, and are kept together with the preheating conditions and rod speed trajectory range that have passed the trial extrusion.

[0022] When selecting a process window, verify the grouped parameters simultaneously. Do not combine the upper limit values ​​from different process windows, and do not extrapolate to material states, cross sections, wall thicknesses, or rod speed trajectory ranges that have not been covered by the test.

[0023] Optionally, S3 includes: making the ratio of the effective metal cross-sectional area of ​​the perforated blank to the annular cross-sectional area of ​​the finished product 25 to 40, and selecting the size of the perforated blank and the annular gap size between the mold and the mandrel according to the finished product outer diameter not less than 100 mm and the wall thickness not less than 5 mm.

[0024] Within the applicable window, preheat the perforated billet to 650–720°C, the die to 630–680°C, and the extrusion cylinder to 640–690°C;

[0025] A forward extrusion press with a nominal capacity of not less than 5,000 tons of force and an actual available extrusion force that meets the selected working conditions is used to extrude pipe in a single cycle.

[0026] After online finishing, the material is naturally air-cooled to room temperature and then extruded without annealing, solution treatment, or aging.

[0027] Optionally, S4 includes: determining the corresponding extruded metal volume by the displacement increment of the extrusion rod and the effective metal cross-sectional area of ​​the perforated billet, converting the extruded metal volume into the axial position of the pipe, and establishing the temperature measurement correspondence of the same pipe section by combining the extrusion temperature measurement position, downstream temperature measurement position and temperature measurement time.

[0028] The upper limit of the measured temperature value on the outer wall and the estimated temperature value on the inner wall of the same pipe section is used as the judgment temperature. The time from demolding to the judgment temperature reaches the temperature limit used for accumulating high temperature residence time in the applicable window is accumulated.

[0029] Based on the actual extrusion pressure, demolding temperature and accumulated time, the extrusion pressure, demolding temperature and natural air cooling residual temperature history corresponding to the candidate subsequent rod speed trajectory are evaluated using the test records corresponding to the applicable window. Only candidate subsequent rod speed trajectories that are expected to not exceed the applicable window constraints are executed.

[0030] Furthermore, the inner wall temperature estimation is calibrated using test pipes with the same wall thickness as the production pipes. The correspondence between the outer wall temperature, the time elapsed after demolding, and the inner wall temperature is established by synchronously measuring the inner and outer wall temperatures during natural air cooling. The estimated inner wall temperature is then compensated upwards according to the upper limit of the underestimation deviation in the calibration test.

[0031] The compensated inner wall temperature estimate is used only as a candidate value for the determination temperature within the range of wall thickness, demolding temperature, and air cooling conditions covered by the calibration test.

[0032] Furthermore, when there is no subsequent rod speed trajectory that simultaneously satisfies the constraints of actual extrusion pressure, demolding temperature, and high-temperature dwell time, or when there is no applicable window for the batch and specification, the extrusion route for the corresponding batch and specification is paused and the cause of the abnormality is recorded.

[0033] For pipe sections whose actual extrusion pressure, demolding temperature, or high-temperature residence time has exceeded the applicable window constraint, they shall be isolated for inspection according to the axial position of the pipe section.

[0034] Based on the bar speed trajectory, actual extrusion pressure, and temperature history of this billet, select the next billet preheating condition that simultaneously meets all constraints within the range of verified preheating conditions. If no preheating condition is available, remain paused.

[0035] Optionally, S5 includes: taking samples at the head, middle and tail of the same final state pipe, setting detection positions along the circumferential and wall thickness directions for each sampling section, detecting grain size and conductivity at the corresponding positions and maintaining the correspondence between the detection positions and the temperature history of the pipe section;

[0036] Compare the test results with the final grain size and conductivity targets according to the same sampling and judgment rules used when verifying the process window. If they all meet the target, the applicable window is confirmed. If they do not meet the target, the material state and process parameter combination corresponding to the non-compliant pipe section is removed from the subsequent optional parameter combinations.

[0037] The lanthanum, yttrium, and copper contents of the finished product were tested and recorded separately along with the amount of raw materials fed and the purity of the raw materials.

[0038] Furthermore, corresponding identifiers are established for furnace batches, perforated billets, and tube sections. The actual material status, process window version, preheating conditions, rod speed trajectory, actual extrusion pressure, temperature history, and circumferential and wall thickness direction detection positions and results of the furnace batch are saved according to the corresponding identifiers.

[0039] After the process window is shrunk, the corresponding relationship between the removed material state and process parameter combination and the non-compliance test results is saved. Subsequent batches will only select the applicable window from the parameter combination that is retained after shrinkage and matches the measured material state and pipe specifications of the subsequent batch.

[0040] The beneficial effects of this invention are:

[0041] 1. By verifying the process window through furnace batch measurements of lanthanum content, yttrium content, oxygen content, and initial microstructure correlation tests, the selection of production conditions is based on the actual material state. Recording the feed rate, raw material purity, and finished product testing separately helps to identify the impact of material state differences on forming and final performance.

[0042] 2. By aligning the temperature measurement data of the same pipe section according to the metal volume relationship, and combining the inner wall temperature estimate calibrated by the wall thickness, the demolding temperature and the high-temperature residence time of subsequent natural air cooling are used together for rod speed selection. This helps to control the forming thermal process of the pipe without annealing, solution treatment or aging treatment after extrusion.

[0043] 3. By verifying and calling the actual extrusion pressure constraints and temperature history constraints in groups, and performing pause and isolation inspections on pipe sections with no feasible conditions and those that have exceeded the limits, and then narrowing the subsequent process window based on the final state test results of the head, middle, tail and circumferential and wall thickness directions, it helps to reduce overload cracking and differences in grain coarsening in different parts. Attached Figure Description

[0044] The accompanying drawings are provided to further illustrate the invention and form part of the specification. They are used in conjunction with embodiments of the invention to explain the invention and do not constitute a limitation thereof. In the drawings:

[0045] Figure 1 This is a flowchart of a low-temperature large deformation extrusion method for preparing large-size fine-grained high-purity copper tubes modified with trace rare earth elements according to the present invention.

[0046] Figure 2 This is a flowchart of the lever speed closed-loop decision-making process for S4 of the present invention. Detailed Implementation

[0047] The present invention will now be described in further detail with reference to the accompanying drawings. These drawings are simplified schematic diagrams, illustrating only the basic structure of the invention, and therefore only show the components relevant to the invention.

[0048] refer to Figures 1-2 A method for preparing large-size, fine-grained, high-purity copper tubes with trace rare earth modification by low-temperature large deformation extrusion, comprising:

[0049] S1. Using high-purity copper as raw material, with only lanthanum and yttrium as alloying additives, the billet is processed into a perforated billet through smelting, casting and extrusion pre-billet treatment, and the measured material state of the furnace batch is obtained.

[0050] S2. Based on the measured material state of the furnace batch, the effective metal cross-sectional area of ​​the perforated billet, and the target tube specifications, select the applicable window from the process window verified by the test of the same material and specifications to obtain the constraints of preheating conditions, rod speed trajectory range, actual extrusion pressure, demolding temperature, and high temperature dwell time.

[0051] S3. Preheat according to the applicable window and extrude the perforated billet through the annular gap formed by the mold and the mandrel, and then air cool it naturally. No annealing, solution treatment or aging treatment is performed after extrusion. Simultaneously collect the extrusion rod displacement, actual extrusion pressure, demolding and downstream temperature.

[0052] S4. Align the collected data to the same pipe section according to the metal volume relationship, determine the temperature history by combining the internal wall temperature estimation applicable to the pipe material, select the subsequent rod speed trajectory that simultaneously meets all constraints from the rod speed trajectory range and execute it, and correct the preheating of the next billet with the execution result.

[0053] S5. Detect the grain size and conductivity of the pipe material after it has been naturally cooled to room temperature. Correlate the test results with the measured material condition and pipe section temperature history of the furnace batch to confirm or narrow the applicable window for subsequent furnace batches.

[0054] In this specific embodiment, S1 includes:

[0055] In this specific embodiment, a copper tube with an outer diameter of 120 mm and a wall thickness of 8 mm is selected as the preparation object throughout the process. The melting and casting station establishes corresponding records for raw materials, melting, casting ingots and perforated billets according to the batch. The actual measured value of the material after extrusion pretreatment is used as the input of S2. The calculated value of feeding does not replace the actual amount of rare earth retained. The predetermined process values ​​in the text are used to determine the test and execution conditions. The final grain size and conductivity are determined by the test results obtained by the following method.

[0056] Based on a total metal charge mass of 1000 kg, cathode copper with a purity of not less than 99.99% and intermediate alloys with copper as the base and lanthanum or yttrium as the additive elements are selected. The lanthanum addition amount is set at 30 ppm and the yttrium addition amount is set at 25 ppm, totaling 55 ppm. The addition amount is within the range of 15-45 ppm for lanthanum, 15-35 ppm for yttrium, and 30-80 ppm for the total amount. ppm represents the mass of the added element divided by the total mass of the metal charge including the intermediate alloy and then multiplied by one million. The target masses of lanthanum and yttrium are 30 g and 25 g, respectively.

[0057] The batching personnel calculate the required alloy mass based on the element mass fraction of the batch of intermediate alloy tested, and include copper in the total mass of the furnace charge. When the rare earth mass fraction of the intermediate alloy is 1.00%, the amount of copper-lanthanum intermediate alloy is 3.000 kg, the amount of copper-yttrium intermediate alloy is 2.500 kg, and the amount of cathode copper is 994.500 kg. If the measured composition of the intermediate alloy deviates from the above mass fraction, it is recalculated. The performance is not adjusted by adding other alloying elements. Impurities attached to the raw materials and intermediate alloy are registered separately.

[0058] The smelting station uses a vacuum induction furnace. Clean and dry copper charge is loaded into a crucible that has been verified by copper blank smelting to not introduce excessive impurities. The pressure is evacuated to no more than 5 Pa. The melt temperature is set to 1200℃ and maintained within the range of 1180~1220℃. The intermediate alloy is pressed into the copper liquid through a vacuum feeding device and homogenized by induction stirring. The stirring is held for 10 minutes, and the process time limit of 8~12 minutes is maintained during the holding period. The pressure, melt temperature, feeding time and holding start and end time are continuously recorded. Furnaces with vacuum or temperature exceeding the limit are kept separately and are not combined with normal furnaces to form a window.

[0059] After heat preservation, the copper liquid is sent into the semi-continuous casting crystallizer through a closed transfer channel. The transfer and the liquid surface of the crystallizer are isolated from air by high-purity argon. The outer diameter of the casting ingot is set to 370 mm and the initial casting speed is 40 mm / min. The inlet temperature of the cooling water is controlled at 20-30℃ according to the crystallizer specifications. The operating conditions are that the outlet temperature does not exceed 45℃ and there is no flow interruption. The actual casting speed, cooling water flow rate and inlet and outlet temperatures are recorded. The stable casting section and the start and stop section are numbered separately. The start and stop ends and the sections found to have shrinkage cavities or porosity by ultrasonic inspection are cut off. The quality of the ingot is not estimated based on the casting set values.

[0060] Before extrusion, the round ingots are homogenized at 600℃. The temperature of the central thermocouple of the same specification is measured and timed for 3 hours after reaching the temperature. The temperature inside the furnace is controlled at 580-620℃, and the holding time after the center reaches the temperature is maintained at 2.5-3.5 hours. After treatment, the ingots are cooled in the furnace to a temperature suitable for finishing. The oxide layer and surface defects are then removed. The ingots are machined to form a perforated billet with a nominal outer diameter of 350mm, a through hole diameter of 105mm, and a length of 500mm. The deviation between the through hole axis and the outer circle axis is controlled within 0.5mm. The end face is deburred. The measured outer diameter, hole diameter, length, and circumferential dimensional difference are recorded in the billet record.

[0061] Samples from the same batch of ingots, including the first, middle, and last parts, were retained, and samples that underwent the same homogenization treatment as the production billets were retained. Samples were taken from the near outer side, the middle of the wall thickness, and the near hole side at each axial position. After removing the surface oxide layer, the contents of lanthanum, yttrium, and oxygen were determined. Lanthanum and yttrium were detected by inductively coupled plasma mass spectrometry with copper matrix matching calibration and blank subtraction. Oxygen was detected by inert gas melting method. Two parallel measurements were performed at each position, and the detection limit, calibration, and repeatability records were retained. Results below the detection limit were also retained and not treated as zero content.

[0062] The acquisition module aligns the weighing and testing data by furnace batch number, ingot number, and sampling location index, and saves the weighing resolution, valid test mark, and original record link. Parallel measurements at the same location are not deleted as duplicate samples. When test data is missing or the instrument quality control sample exceeds the allowable range of laboratory validation, the corresponding record is marked as abnormal and the output of the furnace batch status is paused. After the retest is passed, the relationship between the original record and the replacement record is retained.

[0063] The material structure and composition records are compared according to the sampling location. Only material records that can be traced by raw material batch, heat treatment furnace number and sampling location are retained as candidate inputs. When the same perforated billet corresponds to multiple inconsistent sources, it is removed from the candidate set and the physical object is isolated. A unique furnace batch status version is formed by the combined valid results of composition detection and metallographic detection. Subsequent window screening is performed by S2. The casting station does not lower the acceptance standard on its own.

[0064] After adjacent samples are polished and crystallized, the initial grains are recorded in the axial and transverse sections. The average value, quantile value and grain distribution of each sampling position are obtained using the equivalent circle diameter statistical aperture specified in S5. The quantile values ​​are taken as the dimensions where the cumulative number of grains reaches 10%, 50% and 90%, respectively. The furnace batch material status record simultaneously saves the minimum and maximum values ​​of lanthanum, yttrium, oxygen content and grain statistics at each position. The spatial distribution range is used for matching, and not just a single furnace average is saved. Items with missing test items, repeated measurements that cannot meet the laboratory validity rules or mixed materials with holes are not selected in the window. Qualified data are transmitted to S2 after being bound with the furnace batch number, ingot number and billet number.

[0065] In this specific embodiment, S2 includes:

[0066] The process station reads the measured material state and perforated billet size of the S1 furnace batch. The target outer diameter of 120mm, wall thickness of 8mm, corresponding effective metal cross-sectional area and equipment tooling number are registered as a verification object. First, a hot deformation test is carried out on the material after the same furnace batch is processed. Then, a full-size trial extrusion and natural air cooling test are carried out on the perforated billet of the same size. The hot deformation test is only used to exclude obvious cracks or unstable temperature and deformation rate combinations. It cannot directly replace the load and final structure verification of the full-size trial extrusion.

[0067] The heat deformation specimens are cylindrical specimens with a diameter of 8 mm and a height of 12 mm. They are compressed and screened at true strain rate levels of 650℃, 680℃, 700℃ and 720℃ and the reciprocals of 0.1, 1 and 10s. After the temperature reaches the set value, it is held for 3 minutes and then compressed to a true strain of 1.0. The load, displacement, temperature and crack location are recorded. The above are the screening conditions. The strain of the small-scale compression is not equivalent to the cumulative deformation of the pipe in a single extrusion. If a crack appears in the same level, it is disqualified as the starting point of the first extrusion test. Other levels still need to be judged by full-size test.

[0068] Full-scale tests were conducted on a forward extrusion press with a nominal capacity of 6000 tons. The test nodes for the perforated billet temperature were 660℃, 680℃, and 700℃; the die temperature nodes were 640℃, 660℃, and 680℃; and the extrusion barrel temperature nodes were 650℃, 670℃, and 690℃. Each preheating node was recorded based on the actual temperature reached and the temperature difference. The nominal set temperature was not taken as the full billet temperature. The bar speed was set at the beginning, middle, and end of the effective extrusion stroke. The initial test trajectories were set to 0.5, 0.5, 0.4 mm / s, 0.8, 0.7, 0.5 mm / s, and 1.0, 0.8, 0.5 mm / s, respectively. A continuous linear transition was adopted between adjacent nodes. The segment nodes were located at 20% and 80% of the effective stroke. The entire trajectory and its acceleration and deceleration process were saved for each test.

[0069] The test station first selects 680℃ billet temperature, 660℃ mold temperature and 670℃ barrel temperature with the lowest speed trajectory as candidate test starting points. The test is carried out step by step according to the equipment capacity. The combination of preheating and trajectory is repeatedly verified using at least three full-size perforated billets in the same state. Before the actual records meet the judgment rules, all combinations are marked as pending verification and are not included in the production usable set. The extrusion pressure, inner and outer wall temperature history, forming crack and room temperature detection results generated during the test are all saved in association with the pipe section position. The grain results of one pipe and the conductivity results of another pipe cannot be combined into the same successful sample.

[0070] The production window adopts a discrete, validated combination and its clearly validated tolerance range. The window record includes the window number, version, effective time, original test number, coverage range of each material state component, effective metal cross-sectional area of ​​the billet, target outer diameter and wall thickness, preheating conditions, complete rod speed trajectory and allowable transition, load limit, demolding temperature limit, high temperature dwell time limit, cumulative temperature limit and natural air cooling environment. The coverage range of the material state comes from the measured range of each location of the material participating in the validation. Preheating deviation, dimensional deviation and speed deviation must be covered by supplementary tests of boundary and intermediate conditions. Unvalidated ranges are left blank or only actual test points are registered. Multidimensional usable intervals cannot be arbitrarily pieced together from the extreme values ​​of each component of several boundary samples.

[0071] After trial extrusion, the forming cracks, final grain size, and conductivity are tested. Crack inspection covers the inner and outer walls and ends. Final state testing follows the S5 rules for the first, middle, and last sections, as well as the circumferential and wall thickness directions. Only repeated test combinations that result in crack-free forming, with average grain size at each test location of the same final state pipe not exceeding 15 μm and conductivity not less than 100% IACS can establish a qualified window. The upper limit of the crack-free forming extrusion pressure of the window is taken as the maximum measured extrusion pressure in the repeated tests of this combination, along with the force measurement expansion uncertainty. Supplementary tests are conducted near this load boundary for verification. If the supplementary test results in cracking, the boundary is invalid and the applicable combination is reduced. The upper limit of the actual usable extrusion pressure of the extruder is determined by the lowest value among the hydraulic system calibration, the current tooling load-bearing capacity, and the equipment limitations of the day. The upper limit of the actual extrusion pressure used in production is then taken as the lower limit of the value between the crack-free boundary and the actual usable upper limit of the equipment.

[0072] In the natural air cooling test, the inner and outer wall temperatures are measured simultaneously and the complete process until room temperature is retained. 450℃, 500℃, and 550℃ are successively used as the cumulative temperature limits to be verified. For each limit, the total time for the corresponding qualified pipe section to reach the limit is calculated. The maximum ex-mold temperature plus the temperature measurement uncertainty of the qualified repeated samples of the same complete process combination is used as the candidate ex-mold upper limit. The longest cumulative time plus the sampling time uncertainty is used as the candidate residence upper limit. Natural air cooling tests are carried out near the boundary defined by the candidate limits and the two candidate upper limits. The three items are released as a group only after the boundary is confirmed to be usable by the same final state detection rule. The lowest cumulative temperature limit that can retain the qualified combination and pass the supplementary test is selected. If there is no group boundary that passes the verification, the window is not released.

[0073] The demolding temperature and residence time thresholds are empirical constraints of this combination and do not mean that a fine-grained structure will necessarily be obtained below a certain single temperature. If a non-conforming sample in a repeated test cannot be distinguished from a candidate window in terms of material state, equipment tooling, temperature history, and trajectory error range, the candidate window will be cancelled without hiding the sample by adjusting the threshold. All preheating, trajectory, force, and temperature upper limits are stored together with the same window number. When selecting a process window, the group parameters are checked at the same time, and the upper limit values ​​of different process windows are not combined for use.

[0074] Window library, inner wall calibration record and candidate trajectory response record are uniformly stored in the process database. The test tube number and window version are used as the association key. The record of nominal wall thickness 8mm, target outer diameter 120mm, billet preheating 680℃, die 660℃, extrusion cylinder 670℃, bar speed of 0.5mm / s in the beginning and middle sections and 0.4mm / s in the end section only represents one combination to be tested. Its material coverage, three upper limits and compensation amount must be written by the corresponding test before it becomes valid. When the material treatment, tooling, temperature measurement arrangement, air-cooled support or environmental range is changed, a new version is created and the affected items are re-verified.

[0075] After verifying that the measured material state and pipe specifications of the production batch fall within the corresponding applicable parameter range, when selecting the process window, the controller checks the location range of lanthanum, yttrium, oxygen content and initial grain distribution, billet area, pipe specifications and environmental conditions item by item. Only when all fall within the coverage range of the same valid record will the window be retained. When multiple windows match, the latest version that has been verified by the current equipment tooling and has not been shrunk and deleted will be selected first. Within the same version, the window number will be selected in order. The controller will not push outward to material states, cross sections, wall thicknesses or rod speed trajectories that have not been covered by the test. When there is no matching record, the corresponding batch and specification will be marked as paused. The selected complete window, along with the original test index, will be written into the billet process execution record for S3 and S4 to read.

[0076] In this specific embodiment, S3 includes:

[0077] The extrusion station reads the applicable window written by S2 and the perforated billet record of S1, and checks the ratio of the effective metal cross-sectional area of ​​the perforated billet to the annular cross-sectional area of ​​the finished product according to the nominal dimensions. Calculate, where The nominal extrusion ratio is a dimensionless positive number, and this embodiment requires it to be between 25 and 40. This indicates the outer diameter of the finished blank with holes, in mm, obtained from the actual measured dimensions of the blank. This indicates the diameter of the through hole in the perforated blank, in mm, obtained from the same record and smaller than the outer diameter of the blank; The outer diameter of the finished product at room temperature is expressed in mm. In this embodiment, it is set to 120 mm. The inner diameter of the finished product at room temperature is indicated in mm. It is determined to be 104 mm by subtracting twice the wall thickness from the outer diameter. All four diameters are greater than zero. The subscripts b and p respectively identify the perforated blank and the finished product. The superscript 2 indicates the square. The nominal extrusion ratio corresponding to the 350 mm outer diameter and 105 mm hole diameter is approximately 31.10, which meets the specification conditions that the outer diameter of the finished product is not less than 100 mm and the wall thickness is not less than 5 mm.

[0078] The mold and mandrel are coaxially positioned to form an annular outlet. The target size at room temperature is only used as a design reference. The tooling station corrects the mold hole and mandrel working zone size based on the hot outer diameter, hot wall thickness and shrinkage after cooling of the same specification trial extrusion, so that the air-cooled finished product reaches a 120mm outer diameter and 8mm wall thickness. Before loading the blank, check that there is an assembly gap between the hot mandrel and the through hole of the blank. The mandrel support and centering position are consistent with the verification test. If there is eccentricity, working zone wear or mold number change, the original window cannot be used without verification.

[0079] For a perforated billet with a nominal length of 500 mm, the equipment retains the residual length determined by trial extrusion, nominally set at 30 mm at the end, and records the actual residual under the billet number. The extrusion ratio is not calculated using the outer circle area including the through hole. Subsequent volume alignment only includes the metal entering the effective extrusion stage. The filling, upsetting, die filling stages and the end residual are identified separately. The test verification should cover the impact of this residual setting on the final load and pipe quality.

[0080] The controller selects a record that matches the mounting fixture from the valid combination output by S2 according to the billet number. When the measured diameter, through hole, eccentricity, or hot finished product cross section deviates from the test coverage of the combination, the record is removed and the billet loading is paused. Only when the size and the actual available extrusion pressure of the equipment meet the window simultaneously will an extrusion execution command be generated, and the window number, fixture number, and screening result will be written into the execution record.

[0081] Within the applicable window, the heating station preheats the perforated billet to 650-720°C, the mold to 630-680°C, and the extrusion cylinder to 640-690°C. The executed values ​​can only be the combinations that have been verified within the window. The candidate combinations of 680°C, 660°C, and 670°C in this embodiment are only used for production after verification within this window. The perforated billet uses the near-surface and center thermocouples of the same specification witness billet to determine the temperature and heat preservation procedures. Before the heat preservation ends, each measuring point is within 5°C above or below the set value for 15 minutes as the heat homogenization rule for the test. The transportation time, surface heat dissipation, and cylinder loading waiting time are all included in the preheating verification.

[0082] The pipe is extruded in a single pass using a forward extrusion press with a nominal capacity of not less than 5000 tons of force. In this embodiment, the nominal capacity is set to 6000 tons of force. The ton-force conversion is based on approximately 9.80665 kN per ton of force. However, the actual force applied by the controller is based on the extrusion force obtained by converting and verifying the calibrated main cylinder pressure and effective pressure area. The pressure on the reversing side, no-load friction, and sensor zero point are corrected according to the equipment calibration records. Before starting work, it is verified that the upper limit of the actual available force meets the window, and the load-bearing capacity of the mandrel, die, and extrusion cylinder is also verified. A nominal capacity of 5000 tons of force or more is not used as a basis for judging whether any combination can be extruded.

[0083] During extrusion, the tube is formed by passing through the annular gap in one pass along the verified rod speed trajectory. The tube enters the online guiding finishing device with low contact load, and only the straightness and direction are adjusted. No additional reduction passes for diameter or wall reduction are added to change the microstructure. Afterward, the tube is naturally air-cooled on fixed-gap support rollers. Water spraying, forced air cooling, and heat insulation coating are cancelled. The initial verification range of the air-cooling environment is set at room temperature of 20-30℃ and airflow velocity not exceeding 0.3m / s. The actual environmental range used in production shall be based on the test coverage records. The extruded tube is not annealed, solution treated, or aged.

[0084] The acquisition module collects the displacement of the extrusion rod and the actual extrusion force every 10ms using a unified hardware clock, and collects the temperature every 20ms. The temperature measurement spot after demolding is placed within 20mm behind the mold opening. Downstream fixed temperature measurement sections are 1m, 3m and 6m away from the mold opening. Four temperature measurement directions are arranged along the circumference of each section and the maximum value of the effective reading is taken. During the test, contact thermocouples of copper tubes with the same surface condition are used to check the optical temperature measurement parameters and instrument response delay. Invalid temperature data caused by specular reflection, oxidation and field of view obstruction are not supplemented with lower values.

[0085] For pipe sections that have left the fixed temperature measurement section, the infrared imaging equipment along the air-cooling roller conveyor continues to record the outer wall temperature. The position encoder and the pipe markings in the image are matched with the original axial material coordinates. The temperature measurement coverage continues until the temperature is below the cumulative temperature limit and is confirmed by test to no longer rise. The final state of air cooling to room temperature is still recorded separately. Each frame of data is written with a timestamp, sensor position, billet number, extrusion rod displacement, actual extrusion pressure, temperature in each direction, ambient temperature, and valid measurement mark. If the clock is out of sync for more than one sampling interval or a key temperature measurement is missing, the production rod speed command is paused and the missing interval is transmitted to S4 as the range to be isolated. The original data is retained for reconstructing the temperature history.

[0086] In this specific embodiment, S4 includes:

[0087] The controller reads the synchronous acquisition record from S3, taking the first continuous passage of the pipe head over the die orifice as the effective extrusion start point. Simultaneously, it records the reference position of the extrusion rod, excluding pre-filling displacement, and proceeds according to... The formula is used to convert the extruded metal volume into the additional pipe length required for the axial position of the pipe. This indicates the axial length of the hot-state pipe formed in this section, in mm; This represents the effective metal cross-sectional area of ​​the perforated billet inside the extrusion cylinder in this section, expressed in square millimeters. It is obtained by subtracting the area of ​​the hole occupied by the mandrel from the area of ​​the hot outer contour. This indicates the effective advance displacement increment of the extrusion rod after the mold filling is completed, in mm, and is obtained by the displacement sensor after elastic compression correction by the equipment. This represents the hot annular cross-sectional area of ​​the tube material in the demolding section, in square millimeters. It is obtained by measuring the hot outer and inner diameters or by dimensional conversion verified with the same tooling. Both areas are positive and correspond to the same hot volume reference. The subscript 'b' indicates the blank material, and 'e' indicates the demolding state. It represents the increment between adjacent valid sampling times, and does not directly use the room temperature nominal compression ratio as the hot position conversion factor;

[0088] The effective billet area is obtained after the upsetting fills the extrusion cylinder according to the actual cylinder cavity and mandrel size. During the test, the volume conversion is verified by the laser speed measurement of the demolding and the cumulative tube length. The length error caused by elastic compression, changes in mold material storage and changes in hot cross section is stored in the position calibration record. Cooling shrinkage is corrected by the actual measurement correspondence between the demolding and the downstream length mark. Data exceeding the position calibration error range is not forcibly aligned. In this embodiment, a tube segment is divided for every 100mm increase in the hot cumulative length, and the short sections at the beginning and end are retained. Correspondence records are established for billet number, tube segment number, upper and lower limits of hot length, upper and lower limits of room temperature length and formation time interval.

[0089] Downstream fixed temperature measurement records are located by subtracting the real-time axial transport distance from the temperature measurement section to the die opening from the cumulative demolding length, and positioning the material coordinates that have passed the light spot. The transport distance is integrated by the speed encoder and corrected by the pipe section mark. After the extrusion is paused, the movement and cooling of the demolded pipe are still tracked. Fixed time delay is not used to replace material position alignment. The demolding light spot time is back-calculated to the demolding time based on its distance from the die opening and the measured pipe speed. The temperature of the back-calculated period is taken as the upper limit obtained by calibration and included in the cumulative time. The temperature and force records in the two boundary uncertainty areas are simultaneously assigned to the two adjacent segments. The boundary margin is not less than the measured maximum position error.

[0090] Before production, the inner wall is estimated to be calibrated using a test tube with an 8mm wall thickness, the same outer diameter, and the same surface condition. During natural air cooling, small-diameter thermocouples are installed on the inner and outer walls of the same axial section and recorded simultaneously, covering the range of the intended demolding temperature, room temperature, airflow, support, and air cooling duration. The installation method and thermocouple response compensation are recorded. At least three tubes are used to establish the mapping, and another three independent tubes are used for verification. The data is divided according to the entire test tube. Adjacent moments on the same tube cannot be included in the fitting and verification data at the same time.

[0091] The calibration table uses window version, actual wall thickness coverage range, demolding temperature range, air cooling condition range, outer wall temperature, and time elapsed after demolding as search keys. The temperature axis is divided into grids of 10℃ and the time axis of 1s. For the four corner grids with actual measurement coverage, bilinear interpolation is performed using the average inner wall temperature. If any corner point is missing or exceeds the coverage boundary, the grid is invalid. The interpolated temperature is subtracted from the actual inner wall temperature of each point of the independent verification tube. The maximum value of all positive differences is taken and the combined uncertainty of the inner and outer wall temperature measurements is added as the upward compensation amount for the applicable zone. Negative differences are counted as zero, and the compensation amount is non-negative. Records with 8mm wall thickness, 680℃ demolding temperature range, 500℃ outer wall temperature, and 10s after demolding as keys are filled in with the corresponding actual measurement records and are not replaced by preset constants.

[0092] Controller calculation In the formula The temperature used to determine the cumulative residence time in the same pipe section at the same time is expressed in °C. This indicates the maximum effective measured temperature of the outer wall of the pipe section in multiple directions, in °C. This represents the uncompensated inner wall temperature obtained by interpolation from the calibration table, in °C. This indicates that the underestimation compensation amount of the inner wall obtained from the above independent verification is a non-negative temperature difference, expressed in °C, and read from the same calibration zone. This function takes the larger of the two temperatures within the parentheses. The function itself is not applicable to independent physical units. Its input and output units are both ℃. The subscripts j, o, and i identify the judgment temperature, outer wall temperature, and inner wall estimated temperature, respectively. If the wall thickness, demolding temperature, or air cooling conditions exceed the calibration coverage range, the judgment temperature that can be used for release will not be output and the route will be paused.

[0093] Each pipe section starts from demolding... The cumulative time spent in high-temperature environments is given by the formula. This indicates the cumulative time spent in high-temperature environments, expressed in seconds (s). The subscript "h" indicates the cumulative high-temperature duration. This represents the sampling interval number arranged chronologically from the time of model departure, and is a dimensionless positive integer starting from 1; This represents the total number of intervals currently included, and is a dimensionless non-negative integer. The sum is zero when no intervals have been formed yet. Indicates the first The actual duration of each interval, in seconds, is obtained from the difference between adjacent timestamps and is greater than zero; This indicates the dimensionless timing indication value for the interval. It is set to 1 when the maximum of the two ends of the interval plus the upper limit of the change within the interval reaches or exceeds the cumulative temperature limit of the window; otherwise, it is set to 0. The upper limit of the change within the interval is determined by the maximum unsampled peak value of the high-frequency calibration temperature record under the same conditions. The peak value of the interval must not be missed based solely on the low temperature at the two ends.

[0094] The sampling interval is timed by the actual timestamp, and the number of samples multiplied by the nominal period is not used to cover up frame loss. The interval that crosses the temperature limit is accumulated as the entire interval. When the temperature rises above the limit again, the accumulation continues without being cleared. When the sensor's effectiveness is interrupted, the missing interval is timed as if the limit has been reached, and the judgment of qualified release for that segment is stopped until a supplementary record sufficient to cover the upper limit of the missing temperature is obtained. When comparing the total accumulated time with the upper limit of the window, the same timing method and sampling uncertainty caliber are used. Different interpolation and timing rules must not be used for testing and production.

[0095] A subsequent rod speed decision is made every 100ms. The control status record includes the current effective rod displacement, measured extrusion pressure, demolding temperature, judgment temperature of each formed pipe segment, cumulative time, and current trajectory number. Candidate actions are only taken from the entire remaining trajectory that has been verified in the window and the verified switching connection segment. Different trajectories are not arbitrarily spliced ​​point by point. In this implementation method, the original trajectory is maintained first. When switching is required, only candidates whose current displacement, rod speed, and acceleration / deceleration amplitude fall within the test coverage range of the connection segment are retained. If the switching is not verified in the middle, the original trajectory can only be continued or the equipment can be shut down under control.

[0096] For each candidate, the controller searches for test records under the same conditions according to window, displacement range, current rod speed, and current temperature. The test curve is aligned according to the effective rod displacement. The maximum positive deviation of the measured force of the billet in the last 0.5s minus the corresponding test force and the measured demolding temperature minus the corresponding test demolding temperature is used as the current correction amount. Negative deviations do not reduce the upper limit of the prediction. The predicted force of the remaining trajectory is taken as the upper envelope force correction amount of the future force value of each matched test and the upper limit of the prediction underestimation independently verified. The predicted demolding temperature forms an upper envelope according to the same rules. The upper limit of the underestimation is obtained by the verification of the entire test tube that did not participate in the establishment of the response curve. The units are kN and ℃, respectively. If any corrected state exceeds the coverage of the response record, it is judged as no valid candidate.

[0097] The remaining natural air-cooling history of the candidate trajectory is based on the test records of the same window, the same pipe segment position, and the demolding temperature range. It is aligned according to the time elapsed after demolding. For the currently formed pipe segment, the future curve is corrected by the maximum positive deviation of the actual judgment temperature in the last 0.5 seconds from the test judgment temperature plus the upper limit of the temperature prediction underestimation. The remaining time is accumulated according to the aforementioned timing rules and added to the accumulated time. If no pipe segment has been formed, the entire air-cooling upper envelope covered by the predicted demolding temperature range of the candidate is used. If no calibration and air-cooling records covering the predicted demolding temperature can be found, the candidate is removed.

[0098] The remaining natural air-cooling process of the demolded pipe section is taken from a conservative upper bound applicable to all candidates. It is not assumed that the heat accumulated in the pipe section or the residence time is reduced due to the reduction of the subsequent rod speed. Only when the load and demolding thermal state of the metal that has not yet been demolded change with the candidate trajectory, all pipe sections that have not been air-cooled and the expected newly formed pipe sections are checked one by one. If the predicted extrusion pressure does not exceed the upper limit of force, the predicted demolding temperature does not exceed the upper limit of demolding, and the sum of the accumulated and the remaining accumulated does not exceed the upper limit of residence time, the candidate will be included in the executable set. When there are multiple candidates, the original trajectory is retained first, and then the selection is made from the shortest to the longest estimated completion time of the remaining effective stroke. If the time is the same, the selection is made by trajectory number.

[0099] The controller only issues commands for the selected candidate for the next 100ms and recalculates with new actual measurements in the next cycle. It does not overwrite the original measurements with the predicted values. If there is no trajectory that meets all three constraints at the same time, or if the window, calibration and batch specifications used no longer match, the corresponding batch and specification route is paused. The deceleration and unloading procedure verified by the equipment is used to end the command. During the shutdown process, force and temperature are collected and included in the relevant pipe sections. The shutdown or resumption of execution is not regarded as the temperature history restart.

[0100] When the actual extrusion pressure, demolding temperature, or cumulative high-temperature dwell time of any pipe section exceeds the window constraint, the controller immediately retains the cause of the over-limit, the time, and the axial range of the pipe section. The actual affected area, together with the position error margin, is registered as an isolation inspection area. Force over-limit is attributed to the material formed during that period and in the mold transition zone. Temperature or cumulative time over-limit is attributed to the corresponding pipe section. Over-limit markings shall not be deleted when the next cycle returns to normal. The premise for continuing to execute on the unformed part is still that there are valid candidates and the equipment protection conditions are met.

[0101] After the billet is completed, the maximum positive deviation of the measured force, demolding temperature, and cumulative time of each pipe section relative to the original test record is substituted into the verified complete preheating combination of the next billet and the corresponding trajectory record for upper limit screening. The current combination is kept first. If the current combination cannot simultaneously meet all constraints, it is selected according to the sum of the absolute differences with the current billet temperature, mold temperature, and cylinder temperature from smallest to largest. If the differences are the same, it is selected according to the combination number. Only the records that still match the other material states, dimensions, and environment are selected. Reducing the billet temperature is not regarded as necessarily reducing the load. If there is no usable combination, it is paused. The execution trajectory, measured history, isolation range, and selection of the next billet preheating are written together into the billet number history and handed over to S5 for final state association.

[0102] In this specific embodiment, S5 includes:

[0103] The inspection station receives the billet history of S4 and the corresponding air-cooled pipe. After the temperature at each monitoring position is no more than 2°C different from the ambient temperature and maintained for 10 minutes, the final state at room temperature is recorded. Before testing, the pipe or the sampled base material is not annealed, solution-treated or aged. Samples are taken from the head, middle and tail of the same final state pipe. The material coordinates are located according to 5%, 50% and 95% of the original total length after extrusion. Adjacent metallographic rings and electrical performance sample rings are cut at each position, and the composition analysis sample is also retained. The original total length includes the marked and isolated pipe sections. The isolated sections cannot be deleted and renumbered to make the abnormal position disappear.

[0104] Each sampling section is taken with the top of the equipment as the circumferential zero degree, and samples are taken along the 0 degree, 90 degree, 180 degree and 270 degree directions. In each direction, the thickness is divided into three layers: inner, middle and outer, from the inner wall to the outer wall. The three layers cover 0 to one-third, one-third to two-thirds and two-thirds to the full thickness of the wall, respectively. The metallographic measurement area and adjacent conductive samples are kept in the same direction and layer number. A total of 36 position records are formed from the beginning, middle and end. When the sampling ring has a length, the axial start and end coordinates are also saved. The highest demolding temperature and the longest high temperature residence time in this range are used as the process correlation values ​​for this position.

[0105] Metallographic specimens are cut under low load and continuously cooled. After removing the cutting deformation layer, they are polished and exposed to crystals. At least five non-overlapping calibration fields of view are collected at predetermined equidistant positions in each layer. Fixed grain boundary division and boundary grain counting rules are used. The equivalent circle diameter is obtained by multiplying the cross-sectional area of ​​each complete grain by four, dividing by pi, and then taking the square root. The area unit is square micrometers, and the diameter unit is micrometers. At least 300 grains are counted at each position. If the field of view is insufficient, it is expanded in a predetermined direction. The field of view position is not adjusted due to the appearance of coarse grains.

[0106] In this embodiment, the arithmetic mean of the equivalent circle diameter of the counted grains at each detection location is defined as the average grain size at that location. At the same time, the 10%, 50%, and 90% grain number quantiles, the maximum identifiable grain size, and the original image are saved. Twin boundaries are not used as new grain boundaries for repeated segmentation. The axial and transverse cross-sectional images are retained when the grains are elongated. The initial structure detection and the final state detection use the same aperture. If the grain boundary cannot be identified or there are large areas that are not included, the sample is re-prepared and the field of view is expanded. The conclusion that the 15μm target is met is not given directly.

[0107] Conductivity was determined using the four-terminal DC resistance method. Rectangular miniature samples were fabricated along the pipe axis in the region adjacent to each metallographic layer. The gauge length of the voltage terminal was set to 20 mm, and the nominal cross-section was 1 mm × 1 mm. The measured gauge length and cross-sectional area were substituted into the calculation. The sample was equilibrated in a constant temperature environment of 20 °C until the temperature fluctuation did not exceed 0.1 °C. The current terminal was placed outside the voltage terminal. The average resistance was taken by passing current in both directions to reduce the influence of thermoelectric potential. The test current was changed and the test was repeated to confirm that the sample self-heating did not change the judgment. The volume resistivity was obtained by multiplying the measured resistance by the cross-sectional area and then dividing by the gauge length of the voltage terminal. All lengths were uniformly converted to m and the area was uniformly converted to square meters. The unit of resistivity was Ω·m.

[0108] For conductivity, the reciprocal of the volume resistivity is first taken to obtain the S / m value, then divided by 58 × 10⁶ S / m and multiplied by 100. The resulting value is expressed as %IACS. The comparison benchmark of 100%IACS corresponds to 20℃. At least two parallel samples are prepared at each location and their original current, voltage, size, and temperature are preserved. The two samples are judged separately without using one high value to cancel the other low value. The measurement expanded uncertainty covers the contribution of size, resistance, and temperature control. When the measurement interval crosses 100%IACS, it is treated as pending review and is not directly confirmed as qualified.

[0109] The process window verification and production confirmation both adopt the common rule that the average grain size at each location should not be greater than 15 μm and the conductivity of each parallel conductive sample should not be less than 100% IACS. If the upper limit of the uncertainty of the grain size exceeds 15 μm or the lower limit of the uncertainty of conductivity is less than 100% IACS, the window confirmation cannot be completed. The validity should be retested and adjacent samples should be taken. The original conclusion should be retained for the actual non-conforming location. The average summary value of the whole pipe is only used for statistical description and does not replace the individual judgment of 36 locations. Visual inspection and dye penetrant testing of the inner and outer surfaces should be carried out in conjunction with ultrasonic testing to record the crack situation. Pipes with cracks are not included as qualified window samples.

[0110] When testing the lanthanum, yttrium, and copper content of the finished product, the component analysis samples are obtained from the circumferential positions of adjacent rings at the beginning, middle, and end. The lanthanum and yttrium contents of the finished product are determined separately, and the copper mass fraction is calculated based on the chemical analysis results covering the main metallic and non-metallic impurities. The difference method is only used when the uncertainty caused by impurity coverage and detection limit meets the inspection requirements of the batch. Otherwise, a validated copper major quantitative analysis method is used for verification. The lanthanum, yttrium, and copper contents, detection methods, and detection limits are recorded separately. The actual measured values ​​of the finished product are recorded in columns with the 30ppm and 25ppm addition targets, the actual feed mass, and the purity of the cathode copper. The copper content of the finished product is not estimated based on the purity of the raw materials.

[0111] To correlate the test results with the measured material condition and pipe section temperature history of the furnace batch, and to confirm or narrow the applicable window for subsequent furnace batches, the test results are written into the database using the furnace batch number, ingot number, billet number, pipe section number, axial coordinate, circumferential angle, and wall thickness layer as the association keys. At the same time, the selected window version, preheating measured value, whole rod speed trajectory, actual extrusion pressure, inner and outer wall temperature history, cumulative time, crack inspection, and composition results are associated. When there are valid records for all 36 locations and all isolation intervals and the same acceptance rules are met, the corresponding parameter combination for this run is marked as confirmed. The applicable scope of materials or processes will not be expanded due to a single confirmation.

[0112] When an actual non-conforming location is found, first check its formation time period, window number and complete process combination according to the axial coordinate. Remove the combination of material state covering unit, preheating, trajectory and air cooling conditions corresponding to the location from the subsequent available set. At the same time, retain the correspondence between the removed combination and the non-conforming result and the original test number. If the qualified and non-conforming conditions cannot be distinguished within the same covering unit, remove the entire unit. If the data is missing or the test validity has not been verified, freeze the corresponding combination and it cannot continue to be used as a usable record.

[0113] The window shrinkage adopts the new version release, while the original version and the reason for deletion are read-only retained. Before the next billet and subsequent batches begin, the controller rereads the valid sets that are not frozen or removed, and re-executes S2 matching with the measured material status and specifications of the new batch. Existing batches that have been successful do not constitute the conditions for subsequent batches to use the window. When the retained set is empty, it remains paused. To re-include the deleted combination, a new full-size test and the same inspection rules must be completed according to S2 first, so that the final inspection results actually limit the subsequent production window.

[0114] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in the present invention, based on the technical solution and inventive concept of the present invention, should be covered within the scope of protection of the present invention.

[0115] This invention uses the measured lanthanum, yttrium, and oxygen content and initial microstructure of furnace batches to correlate the extrusion process window of large-section copper tubes, thus corresponding the actual material state with the forming load and final microstructure requirements. During the extrusion process, the extrusion and downstream temperature measurement data of the same tube segment are aligned according to the metal volume relationship. Combined with the inner wall temperature estimate calibrated by actual wall thickness measurement, the extrusion temperature and the subsequent high-temperature residence time during natural air cooling are incorporated into the rod speed adjustment constraint.

[0116] Based on this, the preheating conditions for the next billet are modified according to the results of this billet, and the grain and conductivity test results at different locations of the finished product are correlated with the material state, process parameters and temperature history of the corresponding pipe section. This is used to confirm or narrow the subsequent process window, so as to coordinate the microstructure retention during large-section extrusion forming and air cooling without annealing, solution treatment or aging treatment after extrusion.

Claims

1. A method for preparing large-size, fine-grained, high-purity copper tubes with trace rare earth modification by low-temperature large deformation extrusion, characterized in that, include: S1. Using high-purity copper as raw material, with only lanthanum and yttrium as alloying additives, the billet is processed into a perforated billet through smelting, casting and extrusion pre-billet treatment, and the measured material state of the furnace batch is obtained. S2. Based on the measured material state of the furnace batch, the effective metal cross-sectional area of ​​the perforated billet, and the target tube specifications, select the applicable window from the process window verified by the test of the same material and specifications to obtain the constraints of preheating conditions, rod speed trajectory range, actual extrusion pressure, demolding temperature, and high temperature dwell time. S3. Preheat according to the applicable window and extrude the perforated billet through the annular gap formed by the mold and the mandrel, and then air cool it naturally. No annealing, solution treatment or aging treatment is performed after extrusion. Simultaneously collect the extrusion rod displacement, actual extrusion pressure, demolding and downstream temperature. S4. Align the collected data to the same pipe section according to the metal volume relationship, determine the temperature history by combining the internal wall temperature estimation applicable to the pipe material, select the subsequent rod speed trajectory that simultaneously meets all constraints from the rod speed trajectory range and execute it, and correct the preheating of the next billet with the execution result. S5. Detect the grain size and conductivity of the pipe material after it has been naturally cooled to room temperature. Correlate the test results with the measured material condition and pipe section temperature history of the furnace batch to confirm or narrow the applicable window for subsequent furnace batches.

2. The preparation method according to claim 1, characterized in that, S1 includes: using cathode copper with a purity of not less than 99.99%, vacuum induction melting at an absolute pressure of not more than 5 Pa and a temperature of 1180–1220 °C, adding 15–45 ppm of lanthanum and 15–35 ppm of yttrium to a copper-rare earth intermediate alloy, with a total of 30–80 ppm, where ppm is the ratio of the mass of the added element to the total mass of the metal charge in parts per million; semi-continuous casting of round ingots after stirring and holding at a temperature of 8–12 min; holding the round ingots at a temperature of 580–620 °C for 2.5–3.5 h, cooling them in the furnace, and finishing the surface to form a perforated billet that fits with the mandrel; the measured material state of the furnace batch includes the lanthanum content, yttrium content, oxygen content, and initial grain size and distribution of the material taken from the same furnace batch material before the billet treatment was completed.

3. The preparation method according to claim 1, characterized in that, S2 includes: using the measured material state of the batch, the effective metal cross-sectional area of ​​the perforated billet, and the target wall thickness as test inputs, conducting hot deformation, trial extrusion, and natural air cooling tests on the same material and specifications, recording the preheating temperature, the trajectory of the rod speed as the extrusion rod displacement changes, the actual extrusion pressure, and the temperature history of the pipe section, and detecting forming cracks, final grain size, and conductivity; saving the test parameter combinations and the range of variation covered by the test for forming without cracks and for the same final state pipe with an average grain size not greater than 15μm and conductivity not less than 100% IACS as process windows, each process window is bound to the material state range, effective metal cross-sectional area, target wall thickness, preheating conditions, rod speed trajectory range, upper limit of actual extrusion pressure, upper limit of demolding temperature, upper limit of high temperature dwell time, and temperature limit for accumulating high temperature dwell time; the process window is selected only when the measured material state and pipe specifications of the production batch fall within the corresponding applicable parameter range.

4. The preparation method according to claim 1, characterized in that, S3 includes: ensuring the ratio of the effective metal cross-sectional area of ​​the perforated billet to the annular cross-sectional area of ​​the finished product is 25-40; selecting the size of the perforated billet and the annular gap between the die and the mandrel according to the finished product's outer diameter being not less than 100 mm and wall thickness not less than 5 mm; preheating the perforated billet to 650-720℃, the die to 630-680℃, and the extrusion cylinder to 640-690℃ within the applicable window; using a forward extrusion press with a nominal capacity of not less than 5000 tons and an actual available extrusion force that meets the selected working conditions to extrude the pipe in a single pass; after online finishing, naturally air-cooling to room temperature, without annealing, solution treatment, or aging treatment after extrusion.

5. The preparation method according to claim 1, characterized in that, S4 includes: determining the corresponding extruded metal volume based on the extrusion rod displacement increment and the effective metal cross-sectional area of ​​the perforated billet; converting the extruded metal volume into the axial position of the pipe; and establishing a temperature correspondence for the same pipe segment by combining the temperature measurement position at the demolding point, the downstream temperature measurement position, and the temperature measurement time; using the upper limit of the values ​​between the outer wall temperature measurement value and the estimated inner wall temperature value of the same pipe segment as the judgment temperature; accumulating the time from demolding to the time when the judgment temperature reaches the temperature limit used for accumulating high-temperature residence time in the applicable window; and evaluating the extrusion pressure, demolding temperature, and remaining temperature history of the candidate subsequent rod speed trajectory based on the collected actual extrusion pressure, demolding temperature, and accumulated time using the test records corresponding to the applicable window, and only executing the candidate subsequent rod speed trajectories that are expected to not exceed the constraints of the applicable window.

6. The preparation method according to claim 3, characterized in that, S5 includes: sampling the head, middle and tail of the same final-state pipe, setting detection positions along the circumferential and wall thickness directions for each sampling section, detecting grain size and conductivity at the corresponding positions and maintaining the correspondence between the detection positions and the pipe section temperature history; comparing the detection results with the final-state grain size and conductivity targets according to the same sampling and judgment rules used during process window verification, confirming the applicable window if both are met, and removing the material state and process parameter combination corresponding to the non-compliant pipe section from the subsequent optional parameter combinations if non-compliance exists; detecting the lanthanum content, yttrium content and copper content of the finished product, and recording them separately with the feed amount and raw material purity.

7. The preparation method according to claim 3, characterized in that, In step S2, the upper limit of the actual extrusion pressure is taken as the lower limit of the value between the upper limit of the crack-free forming extrusion pressure verified by the test and the upper limit of the actual usable extrusion pressure of the extruder; the upper limit of the demolding temperature, the upper limit of the high temperature dwell time, and the temperature limit used for accumulating the high temperature dwell time are determined in groups based on the temperature history of the natural air cooling test and the corresponding final state grain and conductivity test results, and are saved together with the preheating conditions and bar speed trajectory range that have passed the trial extrusion; when selecting the process window, the grouped parameters are checked at the same time, and the upper limit values ​​of different process windows are not combined for use, and are not extrapolated to material states, cross sections, wall thicknesses or bar speed trajectory ranges that have not been covered by the test.

8. The preparation method according to claim 5, characterized in that, In step S4, the inner wall temperature estimation is calibrated using a test pipe with the same wall thickness as the production pipe. The correspondence between the outer wall temperature, the time elapsed after demolding, and the inner wall temperature is established by synchronously measuring the inner and outer wall temperatures during natural air cooling. The estimated inner wall temperature is compensated upward according to the upper limit of the underestimation deviation in the calibration test. The compensated inner wall temperature estimate is used only within the range of wall thickness, demolding temperature, and air cooling conditions covered by the calibration test as a candidate value for the determination temperature.

9. The preparation method according to claim 5, characterized in that, In step S4, when there is no subsequent rod speed trajectory that simultaneously meets the constraints of actual extrusion pressure, demolding temperature, and high-temperature dwell time, or when there is no applicable window for the batch and specification, the extrusion route for the corresponding batch and specification is paused and the cause of the abnormality is recorded; for pipe sections where the actual extrusion pressure, demolding temperature, or high-temperature dwell time has exceeded the applicable window constraints, the pipe sections are isolated for inspection according to their axial position; based on the rod speed trajectory, actual extrusion pressure, and temperature history executed for this billet, the preheating conditions for the next billet that simultaneously meet all constraints are selected within the range of verified preheating conditions, and the pause is maintained if no preheating conditions are available.

10. The preparation method according to claim 6, characterized in that, In step S5, corresponding identifiers are established for the batch, perforated billet, and pipe section. The measured material state, process window version, preheating conditions, rod speed trajectory, actual extrusion pressure, temperature history, and the circumferential and wall thickness direction detection positions and results of the batch are saved according to the corresponding identifiers. After the process window shrinks, the correspondence between the removed material state and process parameter combination and the non-compliant detection results is saved. Subsequent batches will only select the applicable window from the parameter combination that is retained after shrinkage and matches the measured material state and pipe specifications of the subsequent batch.