A process for controlling the wall thickness uniformity of centrifugal castings

By detecting and compensating for mold rotation eccentricity before centrifugal casting, controlling the rotational speed stability during pouring, and adjusting process parameters based on casting wall thickness detection results, the problem of casting wall thickness uniformity control was solved, improving the consistency and repeatability of casting production.

CN123102956APending Publication Date: 2026-11-17XINGGUO TECHNOLOGY (WUXI) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611501424.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-24
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies lack the ability to detect and adjust the eccentricity of the mold rotation during centrifugal casting, making it difficult to control the uniformity of the casting wall thickness. Furthermore, fluctuations in the rotation speed during pouring affect the uniformity of the casting wall thickness.

Method used

Before pouring the molten metal, the rotational eccentricity of the mold is detected and compensated. During the pouring process, the rotational speed is kept stable, and the process parameters are adjusted based on the feedback from the casting wall thickness detection to control the difference in casting wall thickness.

Benefits of technology

By pre-compensating for mold rotation eccentricity and stabilizing rotation speed, the unevenness of casting wall thickness is reduced, thereby improving the consistency and repeatability of casting production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102956A_ABST
    Figure CN123102956A_ABST
Patent Text Reader

Abstract

This invention relates to the field of centrifugal casting technology, specifically to a process for controlling the wall thickness uniformity of centrifugal castings. The process includes: detecting the rotational eccentricity and offset direction of the actual center of rotation of the mold relative to the target center of rotation before pouring the molten metal, and compensating for the mold installation position based on the offset direction; continuously detecting and adjusting the actual rotational speed of the mold during the pouring and initial solidification processes to control speed fluctuations; and combining pre-pouring eccentricity compensation, stable speed control during the pouring process, and post-pouring wall thickness spatial distribution feedback to reduce the impact of mold rotational eccentricity and speed fluctuations on the wall thickness uniformity of the casting, thereby improving the wall thickness consistency and production stability of centrifugal castings.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of metal centrifugal casting technology, and specifically to a process for controlling the wall thickness uniformity of centrifugal castings. Background Technology

[0002] Centrifugal casting utilizes the centrifugal force generated by the rotation of the mold to cause molten metal to spread and solidify along the inner wall of the mold, and is widely used in the manufacture of cylindrical, ring-shaped, and other metal castings. For centrifugal castings with high wall thickness requirements, the rotational state of the mold and the working speed during the pouring process directly affect the distribution of molten metal and the uniformity of the casting wall thickness.

[0003] In actual production, the mold is subjected to high-temperature thermal cycling and mechanical loads for a long time, which can easily lead to thermal deformation, assembly errors, or changes in support clearances. This causes the actual rotation center to deviate from the target rotation center, resulting in rotational eccentricity. When the mold is eccentric, the centrifugal force on the molten metal at different circumferential positions is different, which can easily lead to circumferential wall thickness differences. At the same time, the actual working speed may fluctuate due to factors such as load changes during the pouring process, causing the incompletely solidified molten metal to redistribute, further affecting the uniformity of the casting wall thickness.

[0004] Existing technologies typically pre-set the working speed and pouring parameters according to the casting specifications. Before pouring, there is a lack of detection and adjustment of the actual rotational eccentricity of the mold, and there is also a lack of continuous control over the fluctuation of the actual speed during the pouring process. For the wall thickness deviation after forming, the process is usually adjusted or mechanically repaired only based on the detection results. It is difficult to determine the main influencing factors based on the distribution characteristics of the wall thickness deviation in the circumferential and axial directions of the casting, and to provide targeted process feedback.

[0005] Therefore, how to control the actual rotational eccentricity of the mold before casting, maintain a stable working speed during casting, and use the casting wall thickness distribution results to judge and adjust the main sources of deviation, so as to reduce wall thickness differences and improve the wall thickness uniformity of centrifugal castings, has become a technical problem that needs to be solved in this field. Summary of the Invention

[0006] To address the shortcomings of existing technologies, this invention provides a process for controlling the wall thickness uniformity of centrifugal castings, which overcomes the deficiencies of existing technologies, has a reasonable design, a compact structure, and solves the problems mentioned in the background art.

[0007] To achieve the above objectives, the present invention provides the following technical solution:

[0008] A process for controlling the wall thickness uniformity of centrifugal castings includes the following steps:

[0009] S1. Before pouring the molten metal, rotate the mold around the target rotation axis to obtain radial distance change data at different circumferential positions of the mold, and determine the rotational eccentricity and offset direction of the actual rotation center of the mold relative to the target rotation center based on the radial distance change data.

[0010] S2. Compare the rotational eccentricity with the preset control threshold. When the rotational eccentricity exceeds the preset control threshold, adjust the mold installation position according to the offset direction so that the actual rotational center of the mold moves toward the target rotational center. After adjustment, re-detect the rotational eccentricity until the rotational eccentricity does not exceed the preset control threshold.

[0011] S3. After completing the eccentricity compensation, the mold speed is increased to the set working speed, and the actual speed of the mold is continuously detected during the pouring and initial solidification of the molten metal. The mold drive is adjusted according to the deviation between the actual speed and the set working speed so as to control the actual speed deviation within the preset allowable range.

[0012] S4. Pour molten metal into the mold according to the set pouring parameters, and keep the mold rotating after pouring to allow the molten metal to undergo initial solidification.

[0013] S5. After the casting is demolded, multiple circumferential detection points are set on multiple axial detection sections of the casting to obtain the actual wall thickness value of each detection point. The maximum wall thickness difference is determined based on the actual wall thickness value of each detection point. Based on the distribution characteristics of the maximum and minimum wall thickness points in the axial and circumferential directions of the casting, it is determined that the wall thickness difference is mainly manifested as circumferential difference, axial difference, or a composite difference that exists simultaneously in the circumferential and axial directions.

[0014] S6. Adjust the corresponding process factors according to the determined wall thickness difference type. When the wall thickness difference is mainly manifested as circumferential difference, prioritize checking the rotational eccentricity; when the wall thickness difference is mainly manifested as axial difference, prioritize checking the casting quality and filling time; when the wall thickness difference is a composite difference that exists in both circumferential and axial directions, check the rotational eccentricity, actual rotational speed stability, and casting parameters in sequence, and use the adjusted process parameters for subsequent centrifugal casting of castings of the same specification.

[0015] Preferably, the outer periphery of the mold is provided with a first radial detection position, a second radial detection position, a third radial detection position and a fourth radial detection position distributed at 90° intervals along the circumference. The first radial detection position and the third radial detection position are arranged opposite each other, the second radial detection position and the fourth radial detection position are arranged opposite each other, and the directions of the first radial detection position and the third radial detection position are perpendicular to the directions of the second radial detection position and the fourth radial detection position.

[0016] Preferably, the offset of the actual rotation center of the mold in the first orthogonal direction is determined based on the change in radial distance between the first and third radial detection positions, the offset of the actual rotation center of the mold in the second orthogonal direction is determined based on the change in radial distance between the second and fourth radial detection positions, and the rotational eccentricity is determined based on the offsets in both orthogonal directions.

[0017] Preferably, the offset in the first orthogonal direction is set as The offset in the second orthogonal direction is Then the eccentricity e is determined according to the following formula: , And according to and Determine the offset direction.

[0018] Preferably, the mold is rotated at a speed of 50 r / min for at least three rotation cycles to obtain radial distance change data, and the detection results corresponding to multiple rotation cycles are averaged to obtain rotational eccentricity.

[0019] Preferably, the preset control threshold is 0.10 mm, the set working speed is 700-800 r / min, and the actual speed deviation during the pouring process is controlled within ±2% of the set working speed.

[0020] Preferably, the molten metal is aluminum alloy molten metal, the pouring temperature is 720~740℃, the actual pouring quality is controlled within ±1.0% of the target pouring quality, and the filling time is 9~12s.

[0021] Preferably, after pouring, the mold continues to rotate at a set working speed for 70 to 100 seconds to allow the molten metal to undergo initial solidification.

[0022] Preferably, three inspection sections are set along the axial direction of the casting, and eight inspection points are evenly set along the circumference of each inspection section, for a total of 24 inspection points. The maximum wall thickness difference is determined based on the actual wall thickness values ​​of the 24 inspection points. The maximum wall thickness difference is calculated according to the following formula: , in, This represents the maximum wall thickness value among the 24 detection points. This is the minimum wall thickness value among the 24 detection points.

[0023] Preferably, when the maximum wall thickness difference When the difference is less than 0.80mm, the current rotational eccentricity control parameters, operating speed, and pouring parameters will be used as the basic process parameters for subsequent castings of the same specifications; when the maximum wall thickness difference... When the thickness exceeds 0.80 mm, the corresponding process parameters are adjusted based on the distribution characteristics of the maximum and minimum wall thickness points.

[0024] This invention provides a process for controlling the wall thickness uniformity of centrifugal castings. It has the following beneficial effects:

[0025] 1. This invention detects the actual rotation center of the mold before pouring molten metal, obtaining the rotational eccentricity and offset direction. When the rotational eccentricity exceeds a preset control range, the mold installation position is compensated according to the offset direction, ensuring the mold is in a controlled rotational state before pouring begins. Simultaneously, the actual rotational speed of the mold is continuously detected and adjusted during pouring to reduce the impact of operating speed fluctuations on molten metal distribution and the initial solidification process. This reduces wall thickness unevenness caused by mold rotational eccentricity and speed fluctuations.

[0026] 2. This invention uses multiple axial sections and multiple circumferential detection points to detect the wall thickness after the casting is demolded. Based on the spatial distribution characteristics of the maximum and minimum wall thickness points, wall thickness differences are classified circumferentially and axially. When the wall thickness difference is mainly circumferential, the mold rotational eccentricity is checked first; when it is mainly axial, the pouring quality and filling time are checked first; when both circumferential and axial differences exist simultaneously, the rotational eccentricity, working speed stability, and pouring parameters are checked sequentially. This avoids blindly adjusting multiple process parameters without clearly identifying the main source of error, thus improving the targeted nature of process adjustments.

[0027] 3. This invention combines the detection and compensation of mold rotation eccentricity before casting, the monitoring and adjustment of working speed during casting, and the detection and process feedback of wall thickness after casting. This establishes a correspondence between the initial rotation state of the mold, the rotational stability during casting, and the final casting wall thickness. The process parameters that currently meet the wall thickness uniformity requirements are used as the basic process parameters for subsequent castings of the same specification, thereby improving the consistency and repeatability of the process in the production of castings of the same specification. Attached Figure Description

[0028] Figure 1 This is a schematic flowchart of the process for controlling the wall thickness uniformity of centrifugal castings in an embodiment of the present invention. Detailed Implementation

[0029] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions of this invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, what is described is only a part of this invention, not all of it. All other works obtained by those skilled in the art based on this invention without inventive effort are within the scope of protection of this invention.

[0030] Reference Figure 1 This embodiment provides a centrifugal casting wall thickness uniformity control process, which is applicable to the centrifugal casting of cylindrical, annular or other near-rotational metal castings with rotational forming characteristics.

[0031] The control process of this embodiment includes: detecting the actual rotation center of the mold and performing position compensation before pouring; monitoring and adjusting the actual rotation speed of the mold in a closed loop during pouring; obtaining the spatial distribution of wall thickness through multiple axial sections and circumferential detection points of the casting after pouring, and determining the process factors to be adjusted preferentially according to the circumferential or axial distribution characteristics corresponding to the wall thickness difference, thereby forming a closed-loop control process before, during and after pouring.

[0032] Target casting and wall thickness evaluation method

[0033] This embodiment focuses on a cylindrical aluminum alloy centrifugal casting with an outer diameter of 400 mm and a target wall thickness of 50 mm.

[0034] After the casting is demolded, three inspection sections—the front, middle, and rear—are selected along the axial direction of the casting. Eight inspection points are evenly set along the circumference of each inspection section, for a total of 24 inspection points. The actual wall thickness value at each inspection point is measured using an ultrasonic thickness gauge, and the average wall thickness, maximum wall thickness, and minimum wall thickness are obtained based on the inspection results of the 24 inspection points.

[0035] Maximum wall thickness difference Calculate according to the following formula: , in, This represents the maximum wall thickness value among the 24 detection points. This is the minimum wall thickness value among the 24 detection points.

[0036] This implementation method uses the maximum wall thickness difference As the main indicator for evaluating the uniformity of casting wall thickness, and ≤0.80mm is used as the process evaluation condition for this embodiment.

[0037] To further distinguish the spatial distribution characteristics of uneven wall thickness, three axial detection sections were designated Z1, Z2, and Z3, and eight circumferential detection points on each section were designated P1 to P8. For each axial detection section, the difference between the maximum and minimum wall thickness was calculated to obtain the circumferential wall thickness difference of the corresponding section. Simultaneously, the wall thickness values ​​at the same circumferential detection position in the three sections Z1, Z2, and Z3 were compared to obtain the axial wall thickness difference at the corresponding position.

[0038] Among them, the circumferential wall thickness difference is mainly used to characterize the circumferential thickness difference caused by the offset of the mold rotation center, while the axial wall thickness difference is mainly used to characterize the wall thickness change caused by the differences in pouring quality, filling process and axial molten metal distribution.

[0039] Detection and compensation of eccentricity of casting rotation

[0040] Before pouring the molten metal, the mold is mounted on the rotating support mechanism of the centrifugal casting equipment, so that the mold rotates around the target rotation axis.

[0041] Four radial displacement detection positions, A, B, C, and D, are set on the outer periphery of the mold. The four detection positions are set at 90° intervals along the circumference, with A and C opposite each other, B and D opposite each other, and the AC direction and the BD direction perpendicular to each other.

[0042] This embodiment uses a non-contact laser displacement sensor to detect the radial distance change on the outer surface of the mold. The mold is rotated 3 times at a speed of 50 r / min, and radial distance data at four detection positions A, B, C, and D are continuously collected. The rotation angle position corresponding to each detection data is determined based on the encoder or rotation position detection signal.

[0043] The radial distance changes between the two relative detection positions A and C are used to determine the rotation center offset in the first orthogonal direction, and the radial distance changes between the two relative detection positions B and D are used to determine the rotation center offset in the second orthogonal direction. The detection results over three rotation cycles are averaged to reduce the impact of instantaneous measurement fluctuations on the eccentricity calculation.

[0044] Let the offset of the rotation center in the first orthogonal direction be... The offset of the rotation center in the second orthogonal direction is Then the eccentricity of the mold rotation Determined according to the following formula: , The offset direction is based on Harmony Once determined, when an angle representing the offset direction is needed, the corresponding direction angle can be determined according to the mold installation coordinate system. This yields the offset and direction of the actual rotation center relative to the target rotation center.

[0045] For the aluminum alloy cylindrical casting used in this embodiment, the threshold for controlling the rotational eccentricity before pouring is set to 0.10 mm.

[0046] When the rotational eccentricity When the offset is greater than 0.10mm, the mold mounting position is changed by the adjustment structure on the mold mounting base according to the offset direction, so that the actual rotation center moves toward the target rotation center.

[0047] The adjustment structure can employ fine-tuning mechanisms in two mutually perpendicular directions to adjust the mold mounting position in the first and second orthogonal directions, respectively. The compensation direction is opposite to the detected actual rotation center offset direction, and the compensation amount is determined based on Δx and Δy, respectively.

[0048] This implementation method adopts a step-by-step compensation approach. After completing one position compensation, the mold is rotated 3 times at 50 r / min again, and the rotational eccentricity and offset direction are re-checked. Compensation continues when the rotational eccentricity is still greater than 0.10 mm, and compensation stops when the rotational eccentricity is no greater than 0.10 mm.

[0049] Through repeated testing and step-by-step compensation, it is possible to avoid the actual rotation center from exceeding the target rotation center due to excessive adjustment at one time, thereby keeping the mold rotation state within a controlled range before pouring begins.

[0050] Operating speed control and molten metal pouring

[0051] After completing the rotational eccentricity compensation, determine the working speed according to the casting specifications and materials, and gradually increase the speed of the mold to the set working speed.

[0052] For the castings used in this embodiment, the working speed is 700-800 r / min, and the speed is maintained for 20 seconds after reaching the set working speed.

[0053] During the pouring process, the actual rotational speed of the mold is continuously monitored and compared with the set operating speed. When the actual rotational speed deviates from the set operating speed by more than the allowable fluctuation range, the rotational drive mechanism is used to adjust the actual rotational speed back to the allowable range.

[0054] This embodiment controls the actual rotational speed deviation during the pouring process to within ±2% of the set working speed.

[0055] The actual rotational speed deviation can be determined as a percentage of the difference between the actual rotational speed and the set operating speed relative to the set operating speed. During the pouring process, the actual rotational speed is acquired through continuous sampling, and the output of the drive mechanism is adjusted in real time based on the actual rotational speed deviation, thereby reducing rotational speed fluctuations during pouring and initial solidification.

[0056] In this embodiment, aluminum alloy molten metal is used for casting, the casting temperature is controlled at 720-740℃, the actual casting quality is controlled within ±1.0% of the target casting quality, and the filling time is controlled at 9-12s.

[0057] After pouring, the mold continues to rotate to allow the molten metal to initially solidify. In this embodiment, after pouring, the mold continues to rotate at the set operating speed for 70-100 seconds, then gradually decreases the speed until it stops, and is demolded after the casting cools to the predetermined demolding temperature.

[0058] Spatial distribution detection of casting wall thickness and process feedback

[0059] After the casting is demolded, the wall thickness is measured at the aforementioned 24 inspection points, and the maximum wall thickness difference is calculated. .

[0060] When the maximum wall thickness difference does not exceed 0.80 mm, the current rotational eccentricity control parameters, working speed, and pouring parameters are used as the basic process parameters for subsequent castings of the same specification.

[0061] When the maximum wall thickness difference exceeds 0.80 mm, the mold rotation eccentricity, working speed, pouring quality and filling time are checked based on the distribution of the maximum and minimum wall thickness points, and the corresponding process parameters are adjusted.

[0062] Specifically, the wall thickness values ​​obtained from the 24 detection points were reorganized according to "axial position" and "circumferential position". When the maximum and minimum wall thickness points are mainly located at different circumferential positions on the same axial section, the wall thickness difference is determined mainly by the circumferential difference; when the maximum and minimum wall thickness points are mainly distributed on different axial sections and the corresponding circumferential position differences are small, the wall thickness difference is determined mainly by the axial difference.

[0063] When further quantification is required, the circumferential wall thickness differences of the three axial sections are compared, and the wall thickness differences between different axial sections at each circumferential detection position are compared; the larger difference between the two types of differences is taken as the priority for verification.

[0064] When the wall thickness deviation is mainly manifested as circumferential difference, the eccentricity of the mold rotation should be checked first; when it is mainly manifested as axial difference, the pouring quality and filling time should be checked first; when both circumferential and axial differences exist, the eccentricity of the rotation, the stability of the working speed, and the pouring parameters should be checked in turn.

[0065] When providing process feedback, first determine whether the eccentricity exceeds 0.10mm again; if the eccentricity is within the control range, further check whether the actual rotation speed deviation during the casting process is within ±2%; if the eccentricity and rotation speed are both within the corresponding control range but there is still a significant difference in axial wall thickness, then recheck the casting quality and filling time.

[0066] This avoids making large adjustments to multiple process parameters simultaneously without identifying the main source of error, ensuring that each process adjustment is clearly targeted.

[0067] This forms a control process that combines pre-pouring eccentricity detection and compensation, pouring speed control, and post-pouring wall thickness spatial distribution detection and process feedback.

[0068] The key technical focus of this implementation method is not to control the mold eccentricity, working speed, or pouring parameters individually, but to establish a correspondence between the mold rotation state before pouring, the rotational stability during pouring, and the wall thickness spatial distribution after pouring, and to use the wall thickness spatial distribution results to determine the process factors that should be prioritized for adjustment in the next round.

[0069] Example 1

[0070] This embodiment prepares a cylindrical aluminum alloy centrifugal casting with an outer diameter of 400 mm and a target wall thickness of 50 mm.

[0071] The mold was mounted on a centrifugal casting machine, and four laser displacement sensors (A, B, C, and D) were installed on the outer circumference of the mold. The mold was rotated 3 times at 50 r / min, and the initial rotational eccentricity was measured to be 0.32 mm.

[0072] The mold installation position was compensated for for the first time based on the detected offset direction. After compensation, the remaining rotational eccentricity was measured again and found to be 0.08 mm. Therefore, compensation was stopped.

[0073] The casting speed was then increased to 750 r / min and stabilized for 20 s. Molten aluminum alloy at 730℃ was quantitatively added to the mold, and the actual casting mass was controlled within ±1.0% of the target casting mass. The filling time was 10 s.

[0074] During the pouring process, the actual rotational speed of the mold is detected and adjusted to ensure that the maximum deviation of the actual rotational speed is 1.3%.

[0075] After pouring, maintain a rotation speed of 750 r / min for 90 seconds, then gradually reduce the speed until it stops. After the casting cools to the predetermined demolding temperature, demold it and use an ultrasonic thickness gauge to check 24 inspection points.

[0076] The test results are as follows: average wall thickness 50.02 mm, maximum wall thickness 50.31 mm, minimum wall thickness 49.75 mm, and maximum wall thickness difference 0.56 mm.

[0077] Based on the results of 24 testing points, the maximum wall thickness difference did not exceed 0.80 mm. Therefore, the rotational eccentricity control parameters, the working speed of 750 r / min, and the corresponding pouring parameters of this embodiment are used as the basic process parameters for subsequent castings of the same specifications.

[0078] Example 2

[0079] This embodiment uses the same casting dimensions, materials, and testing methods as Embodiment 1.

[0080] The initial rotational eccentricity was measured to be 0.45 mm. After two position compensations, the final rotational eccentricity was 0.06 mm.

[0081] The working speed was set to 800 r / min and stabilized for 20 seconds; the aluminum alloy molten metal pouring temperature was 740℃ and the filling time was 12 seconds; after pouring, the rotation was maintained at 800 r / min for 100 seconds; the maximum actual speed deviation during the pouring process was 1.1%.

[0082] The wall thickness was measured at 24 points. The average wall thickness was 49.98 mm, the maximum wall thickness was 50.27 mm, the minimum wall thickness was 49.71 mm, and the maximum wall thickness difference was 0.56 mm.

[0083] The maximum wall thickness difference in this embodiment is also less than 0.80 mm, indicating that under different working speeds and pouring conditions given in this embodiment, as long as the rotational eccentricity is effectively controlled before pouring and the speed fluctuation during pouring is within the controllable range, a small wall thickness difference can still be obtained.

[0084] Example 3

[0085] This embodiment uses the same casting dimensions, materials, and testing methods as Embodiment 1.

[0086] The initial rotational eccentricity was measured to be 0.28 mm, and the final rotational eccentricity after position compensation was 0.09 mm.

[0087] The working speed was set to 700 r / min and stabilized for 20 seconds; the aluminum alloy molten metal pouring temperature was 720℃ and the filling time was 9 seconds; after pouring, the rotation was maintained at 700 r / min for 70 seconds; the maximum actual speed deviation during the pouring process was 1.7%.

[0088] The wall thickness was measured at 24 points. The average wall thickness was 50.04 mm, the maximum wall thickness was 50.38 mm, the minimum wall thickness was 49.75 mm, and the maximum wall thickness difference was 0.63 mm.

[0089] Comparative Example 1

[0090] This comparative example uses the same mold, aluminum alloy material, pouring temperature, target pouring mass, working speed and initial solidification time as Example 1, but no rotational eccentricity compensation is performed before pouring.

[0091] The measured rotational eccentricity before pouring was 0.32 mm, and the maximum actual rotational speed deviation during pouring was 1.4%.

[0092] The wall thickness was measured at 24 points. The average wall thickness was 50.08 mm, the maximum wall thickness was 50.91 mm, the minimum wall thickness was 49.07 mm, and the maximum wall thickness difference was 1.84 mm.

[0093] Comparative Example 2

[0094] This comparative example performs rotational eccentricity detection and position compensation on the mold before casting to achieve a final rotational eccentricity of 0.08 mm, but does not perform effective working speed stabilization control during the casting process.

[0095] The working speed was set to 750 r / min, and the maximum actual speed deviation during the casting process was 4.8%. Other process conditions were the same as in Example 1.

[0096] The wall thickness was measured at 24 points. The average wall thickness was 50.03 mm, the maximum wall thickness was 50.72 mm, the minimum wall thickness was 49.30 mm, and the maximum wall thickness difference was 1.42 mm.

[0097] Comparative Example 3

[0098] This comparative example uses the same process conditions as Example 1, but the final rotational eccentricity before casting is controlled within the range of 0.15 to 0.20 mm, which is actually 0.17 mm. The maximum actual rotational speed deviation during casting is 1.5%.

[0099] The wall thickness was measured at 24 points. The average wall thickness was 50.05 mm, the maximum wall thickness was 50.55 mm, the minimum wall thickness was 49.43 mm, and the maximum wall thickness difference was 1.12 mm.

[0100] Analysis of Results from Examples and Comparative Examples

[0101] As can be seen from Examples 1-3 and Comparative Examples 1-3, under the casting specifications and process conditions of this embodiment, when the rotational eccentricity before pouring is controlled within 0.10 mm and the actual rotational speed deviation during pouring is controlled within ±2%, the maximum wall thickness difference of the resulting casting is 0.56-0.63 mm; when no eccentricity compensation is performed, the rotational speed fluctuates greatly, or the eccentricity is not sufficiently controlled, the maximum wall thickness difference reaches 1.84 mm, 1.42 mm, and 1.12 mm, respectively.

[0102] Compared with Comparative Example 1, in Example 1, when the actual rotational speed deviation during the pouring process was basically the same, after reducing the pre-pouring rotational eccentricity from 0.32 mm to 0.08 mm, the maximum wall thickness difference decreased from 1.84 mm to 0.56 mm, indicating that the pre-pouring mold rotational eccentricity has a significant impact on the circumferential wall thickness uniformity.

[0103] Compared with Comparative Example 2, in Example 1, when the final rotational eccentricity was around 0.08 mm, the maximum wall thickness difference increased from 0.56 mm to 1.42 mm when the maximum actual rotational speed deviation during the casting process increased from 1.3% to 4.8%. This shows that maintaining a stable working speed during the casting process is also an important condition for obtaining uniform wall thickness.

[0104] Compared with Comparative Example 3, in Example 1, when the maximum actual rotational speed deviation during the casting process was 1.3% and 1.5% respectively, the maximum wall thickness difference increased from 0.56mm to 1.12mm when the final rotational eccentricity increased from 0.08mm to 0.17mm. This further illustrates that under the casting specifications and process conditions of this embodiment, controlling the mold rotational eccentricity within 0.10mm before casting is beneficial to reducing wall thickness unevenness.

[0105] The above results indicate that the eccentricity of the casting mold and the rotation speed fluctuation during the pouring process can affect the uniformity of wall thickness. It is difficult to obtain stable uniformity of wall thickness by relying solely on eccentricity compensation before pouring without controlling the rotation speed stability during the pouring process, or by controlling the rotation speed stability without controlling the eccentricity of the casting mold to the appropriate range.

[0106] Furthermore, by classifying the wall thickness inspection results after casting according to circumferential and axial positions, different types of wall thickness unevenness can be correlated with corresponding process factors: circumferential thickness difference primarily corresponds to mold rotation eccentricity, while axial thickness difference primarily corresponds to casting quality and the filling process. When both types of differences exist simultaneously, the mold rotation state, rotation speed stability, and casting parameters are checked sequentially. This not only allows us to determine whether the casting meets the wall thickness uniformity requirements but also provides a targeted adjustment basis for the process adjustment of the next batch of castings of the same specifications.

[0107] Therefore, this embodiment combines mold rotation eccentricity detection and compensation before casting, closed-loop control of working speed during casting, wall thickness spatial distribution detection after casting, and process feedback based on wall thickness difference type. Without significantly increasing the complexity of centrifugal casting equipment, it reduces the impact of mold rotation state and speed fluctuation on the uniformity of casting wall thickness and improves the consistency of wall thickness control between batches of castings of the same specification.

[0108] The specific parameters in the above embodiments are used to illustrate the implementation process of the present invention. For centrifugal castings of different specifications and materials, the corresponding working speed, pouring temperature, pouring quality, filling time, and rotational eccentricity control range can be determined according to the target wall thickness, mold size, molten metal density, and specific filling characteristics. The adjustment principle is to ensure that the actual rotation state of the mold and the speed fluctuation during the pouring process are both within a controlled range that can meet the requirements of target wall thickness uniformity.

[0109] It should be noted that, in this document, relational terms such as "first" and "second" are used merely to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or apparatus. Without further limitations, an element defined by the phrase "comprising one..." does not exclude the presence of other identical elements in the process, method, article, or apparatus that includes the element.

[0110] The above description is only used to illustrate the technical solutions of the present invention, and is not intended to limit them. Although the present invention has been described in detail with reference to the foregoing, those skilled in the art should understand that modifications can still be made to the foregoing technical solutions, or equivalent substitutions can be made to some of the technical features. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the present invention.

Claims

1. A process for controlling the uniformity of wall thickness in centrifugal castings, characterized in that, Includes the following steps: S1. Before pouring the molten metal, rotate the mold around the target rotation axis to obtain radial distance change data at different circumferential positions of the mold, and determine the rotational eccentricity and offset direction of the actual rotation center of the mold relative to the target rotation center based on the radial distance change data. S2. Compare the rotational eccentricity with the preset control threshold. When the rotational eccentricity exceeds the preset control threshold, adjust the mold installation position according to the offset direction so that the actual rotational center of the mold moves toward the target rotational center. After adjustment, re-detect the rotational eccentricity until the rotational eccentricity does not exceed the preset control threshold. S3. After completing the eccentricity compensation, the mold speed is increased to the set working speed, and the actual speed of the mold is continuously detected during the pouring and initial solidification of the molten metal. The mold drive is adjusted according to the deviation between the actual speed and the set working speed so as to control the actual speed deviation within the preset allowable range. S4. Pour molten metal into the mold according to the set pouring parameters, and keep the mold rotating after pouring to allow the molten metal to undergo initial solidification. S5. After the casting is demolded, multiple circumferential detection points are set on multiple axial detection sections of the casting to obtain the actual wall thickness value of each detection point. The maximum wall thickness difference is determined based on the actual wall thickness value of each detection point. Based on the distribution characteristics of the maximum and minimum wall thickness points in the axial and circumferential directions of the casting, it is determined that the wall thickness difference is mainly manifested as circumferential difference, axial difference, or a composite difference that exists simultaneously in the circumferential and axial directions. S6. Adjust the corresponding process factors according to the determined wall thickness difference type. When the wall thickness difference is mainly manifested as circumferential difference, prioritize checking the rotational eccentricity; when the wall thickness difference is mainly manifested as axial difference, prioritize checking the casting quality and filling time; when the wall thickness difference is a composite difference that exists in both circumferential and axial directions, check the rotational eccentricity, actual rotational speed stability, and casting parameters in sequence, and use the adjusted process parameters for subsequent centrifugal casting of castings of the same specification.

2. The centrifugal casting wall thickness uniformity control process according to claim 1, characterized in that, The outer periphery of the mold is provided with a first radial detection position, a second radial detection position, a third radial detection position and a fourth radial detection position distributed at 90° intervals along the circumference. The first radial detection position and the third radial detection position are arranged opposite each other, the second radial detection position and the fourth radial detection position are arranged opposite each other, and the directions of the first radial detection position and the third radial detection position are perpendicular to the directions of the second radial detection position and the fourth radial detection position.

3. The centrifugal casting wall thickness uniformity control process according to claim 2, characterized in that, The offset of the actual rotation center of the mold in the first orthogonal direction is determined based on the change in radial distance between the first and third radial detection positions. The offset of the actual rotation center of the mold in the second orthogonal direction is determined based on the change in radial distance between the second and fourth radial detection positions. The rotational eccentricity is determined based on the offsets in both orthogonal directions.

4. The centrifugal casting wall thickness uniformity control process according to claim 3, characterized in that, Let the offset in the first orthogonal direction be... The offset in the second orthogonal direction is Then the eccentricity e is determined according to the following formula: , And according to and Determine the offset direction.

5. The centrifugal casting wall thickness uniformity control process according to claim 1, characterized in that, The mold is rotated at a speed of 50 r / min for at least three rotation cycles to obtain radial distance change data, and the detection results corresponding to multiple rotation cycles are averaged to obtain the rotational eccentricity.

6. The centrifugal casting wall thickness uniformity control process according to claim 1, characterized in that, The preset control threshold is 0.10mm, the set working speed is 700~800r / min, and the actual speed deviation during the pouring process is controlled within ±2% of the set working speed.

7. The centrifugal casting wall thickness uniformity control process according to claim 1, characterized in that, The molten metal is aluminum alloy molten metal, the pouring temperature is 720~740℃, the actual pouring quality is controlled within ±1.0% of the target pouring quality, and the filling time is 9~12s.

8. The centrifugal casting wall thickness uniformity control process according to claim 1, characterized in that, After pouring, the mold continues to rotate at the set working speed for 70-100 seconds to allow the molten metal to undergo initial solidification.

9. The centrifugal casting wall thickness uniformity control process according to claim 1, characterized in that, Three inspection sections are set along the axial direction of the casting, and eight inspection points are evenly set along the circumference of each inspection section, for a total of 24 inspection points. The maximum wall thickness difference is determined based on the actual wall thickness values ​​of the 24 inspection points. The maximum wall thickness difference is calculated according to the following formula: , in, This represents the maximum wall thickness value among the 24 detection points. This is the minimum wall thickness value among the 24 detection points.

10. The centrifugal casting wall thickness uniformity control process according to claim 9, characterized in that, When the maximum wall thickness difference When the difference is less than 0.80mm, the current rotational eccentricity control parameters, operating speed, and pouring parameters will be used as the basic process parameters for subsequent castings of the same specifications; when the maximum wall thickness difference... When the thickness exceeds 0.80 mm, the corresponding process parameters are adjusted based on the distribution characteristics of the maximum and minimum wall thickness points.