A self-lubricating material, its preparation method and application

By preparing copper-based porous materials with synergistic Sn and Ni reinforcement, the problems of unstable lubrication and corrosion in sliding bearings were solved, achieving self-lubrication and corrosion resistance, thus meeting the high reliability and long service life requirements of wind turbine units.

CN123102980APending Publication Date: 2026-11-17SUZHOU XINTAI SPACE-TIME OPTOELECTRONICS TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611415914.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-11
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing sliding bearing materials in wind turbines suffer from unstable lubrication, high friction coefficient, and easy corrosion. They are particularly difficult to achieve self-lubrication and have insufficient corrosion resistance in marine environments, which cannot meet the requirements of large-scale and high reliability.

Method used

A copper-based alloy material with Sn 11.0%~13.0%, Ni 1.5%~2.5%, and the balance Cu was used to prepare a porous material by powder metallurgy. Combined with vacuum or hydrogen atmosphere protected sintering and oil immersion treatment, interconnected pores were formed to store lubricating oil, and a self-lubricating regulation mechanism of temperature-load-oil release was constructed.

Benefits of technology

It achieves sufficient lubrication of the bearing interface under harsh working conditions, improves the comprehensive mechanical properties and wear resistance of the material, is suitable for marine high-salt and high-humidity corrosive environments, and extends the service life and operational reliability of wind turbine units.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This invention discloses a self-lubricating material, its preparation method, and its application. The preparation method of the self-lubricating material includes: by mass fraction, the raw material composition is: Sn 11.0%~13.0%, Ni 1.5%~2.5%, with the balance being Cu, and the total mass fraction of impurities ≤1.0%; weighing each raw material powder according to the ratio, mixing them evenly, and then sequentially subjecting the resulting mixed powder to molding, sintering, and oil impregnation to obtain the self-lubricating material. This invention utilizes a dual-drive mechanism of thermo- and pressure-induced lubrication to release the lubricating oil stored inside the porous matrix to the actual contact area of ​​the micro-protrusions, eliminating the lubrication blind zone present in traditional external oil supply methods; it constructs a closed-loop self-lubricating control mechanism of temperature-load-oil release, ensuring sufficient lubrication at the bearing interface of wind turbine units under harsh operating conditions, and is suitable for high-salt and high-humidity corrosive conditions such as marine and tidal environments.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of lubrication materials technology, specifically to a self-lubricating material and its preparation method. Background Technology

[0002] As wind turbines become larger and more offshore, rolling bearings, due to their complex structure, high cost, and limited load-bearing capacity, can no longer meet the demands for high single-unit capacity, high reliability, and long service life. Sliding bearings, with their advantages of simple structure, high load-bearing capacity, low coefficient of friction, and good adaptability, are gradually becoming the alternative to main shaft bearings in wind turbines, forming a development trend of "sliding bearings replacing rolling bearings".

[0003] In sliding bearings, lubrication directly determines their friction performance and lifespan. Oil lubrication has a friction coefficient only on the order of 0.1 that of solid lubrication, offering significant advantages. Therefore, designing a sliding bearing material capable of self-lubrication has become a key technological path to improve the operating efficiency and reliability of wind turbine units.

[0004] The contact surface between the shaft and the bearing is composed of micro-protrusions, resulting in an extremely small actual contact area. External lubricating oil has difficulty penetrating the contact area of ​​these micro-protrusions, leading to insufficient lubrication at the most critical points and hindering the lubricating medium from reaching the actual contact surface. The micro-protrusion contact points are subjected to extremely high stress and heat, easily causing material softening, welding, and accelerated wear, severely impacting bearing life. Concentrated frictional heat can also lead to material failure.

[0005] On the other hand, while solid lubricants (such as graphite) have a certain degree of self-lubrication, their coefficient of friction is much higher than that of oil lubrication, and they are prone to electrochemical corrosion in marine environments. Existing materials do not have the ability to automatically adjust the supply of lubricating oil according to friction conditions (such as temperature and load), resulting in unstable lubrication effects and a lack of self-feedback lubrication mechanisms. Summary of the Invention

[0006] Therefore, embodiments of the present invention provide a self-lubricating material, its preparation method, and its application.

[0007] To achieve the above objectives, the embodiments of the present invention provide the following technical solutions:

[0008] According to a first aspect of the present invention, the present invention provides a method for preparing a self-lubricating material, the method comprising:

[0009] The raw material composition by mass fraction is: Sn 11.0%~13.0%, Ni 1.5%~2.5%, with the balance being Cu, and the total mass fraction of impurities ≤1.0%. The raw material powders are weighed according to the proportions, mixed evenly, and the resulting mixed powder is sequentially subjected to molding, sintering, and oil impregnation to obtain the self-lubricating material.

[0010] Furthermore, the raw material composition is: Sn 12.0%, Ni 2.0%, balance Cu, and total impurity mass fraction ≤1.0%.

[0011] Furthermore, the particle size of the raw material powder is 12-23 μm; the particle size of the mixed powder is 50-100 μm.

[0012] Furthermore, the molding conditions are: molding pressure 400~600 MPa, holding time 30~60 seconds; zinc stearate or graphite emulsion is used as mold lubricant.

[0013] Furthermore, the sintering process employs vacuum sintering or hydrogen atmosphere-protected sintering, wherein...

[0014] The vacuum sintering conditions are as follows: sintering temperature 800~850℃, holding time 2~3 hours, heating rate 5~10℃ / min, furnace cooling, and vacuum degree ≤10. -3 Pa;

[0015] The conditions for hydrogen atmosphere-protected sintering are: sintering temperature 820~870℃, holding time 2~2.5 hours, heating rate 5~10℃ / min, furnace cooling, and hydrogen flow rate 0.5~1.0 L / min.

[0016] Furthermore, the conditions for the oil immersion treatment are as follows: In an environment with a vacuum degree ≤100 Pa, the sintered material is immersed in lubricating oil at an immersion temperature of 80~120℃ for 2~6 hours. After immersion, the surface oil is cleaned. Preferably, the immersion temperature is 100℃ and the immersion time is 4 hours. Performing the oil immersion treatment under vacuum conditions allows the lubricating oil to fully penetrate the interconnected pores of the porous matrix, improving oil storage capacity and lubrication effect.

[0017] Furthermore, before mixing, the method further includes adding graphite with a mass fraction of 1% to 5%, wherein the graphite has a particle size of 10-30 μm.

[0018] According to a second aspect of the present invention, the present invention provides a self-lubricating material, which is made by the preparation method described in any of the preceding claims.

[0019] According to a third aspect of the present invention, the present invention provides the application of the self-lubricating material as described above in the preparation of sliding bearings for offshore wind turbines.

[0020] Wind turbine shafts are generally designed to be made of steel or alloy steel. Based on the principles of friction and wear, bearing materials should not use the same material system, i.e., iron-carbon alloys are not suitable. Therefore, a copper-based alloy was chosen. After comparison and screening, the material composition was determined to be: Sn 11.0%~13.0%, Ni 1.5%~2.5%, with the balance being Cu. Sn and Ni are mainly used to enhance the overall performance of the copper alloy through solid solution strengthening, improved corrosion resistance, and adjustment of mechanical properties.

[0021] Sn dissolves in the copper matrix to form an α-solution, significantly improving the alloy's strength and hardness, as well as its wear resistance and castability. Sn can also form an oxide film (such as SnO2) on friction surfaces, reducing wear (used in bearings and gears). SnO2 is a dense oxide film that resists chloride ion corrosion, enhancing the corrosion resistance of copper alloys.

[0022] Ni dissolves infinitely in copper, increasing its strength while maintaining good ductility, thus comprehensively strengthening the copper alloy. The mechanism is solid solution strengthening combined with grain refinement strengthening. Ni also promotes the formation of a passivation film in copper alloys, significantly improving corrosion resistance and heat resistance.

[0023] Porous materials are prepared using powder metallurgy. First, pre-alloyed powders are prepared, then molded, and subsequently sintered under vacuum or H2 atmosphere protection. By controlling the process, alloy materials with interconnected pores at the micrometer scale are obtained.

[0024] The embodiments of the present invention have the following advantages:

[0025] This invention utilizes a dual-drive mechanism of thermal and pressure to release the lubricating oil stored inside the porous matrix to the actual contact area of ​​the micro-protrusions, eliminating the lubrication blind spots present in traditional external oil supply methods; and constructs a closed-loop self-lubricating control mechanism of temperature-load-oil release to ensure sufficient lubrication of the wind turbine bearing interface under harsh operating conditions.

[0026] This invention uses powder metallurgy to prepare copper-based porous materials. Under the synergistic strengthening effect of Sn and Ni, the comprehensive mechanical and wear resistance properties of the matrix are superior to those of conventional copper-based alloys, making it suitable for high-salt and high-humidity corrosion conditions such as marine and tidal environments. Detailed Implementation

[0027] The following specific embodiments illustrate the implementation of the present invention. Those skilled in the art can easily understand other advantages and effects of the present invention from the content disclosed in this specification. Obviously, the described embodiments are only some, not all, of the embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0028] The following instructions recommend using fully synthetic gear oil (such as ISO VG 460 grade), such as Mobil SHC 600 series or Shell Omala S4 GX 460 or equivalent products.

[0029] Example 1

[0030] This embodiment provides a self-lubricating material, the raw materials of which are: Sn 12.0%, Ni 2.0%, Cu 86.0%.

[0031] Its preparation method includes the following steps:

[0032] (1) Weigh each raw material according to the ratio, grind them, and obtain powder with a particle size of 12-23μm;

[0033] (2) Mix the powder obtained in step (1) and place it in the mold (the mold lubricant is zinc stearate), and hold it under a molding pressure of 450 MPa for 60 seconds;

[0034] (3) Vacuum sinter the material obtained in step (2) under the following conditions: control the vacuum degree ≤ 10. -3 Pa, heated to the sintering temperature of 850°C at a heating rate of 10°C / min, held at that temperature for 2 hours, and then cooled with the furnace;

[0035] (4) Under a vacuum of ≤100 Pa, the material obtained in step (3) is immersed in lubricating oil at a temperature of 100°C for 4 hours. After immersion, the surface oil of the material is cleaned to obtain a self-lubricating material.

[0036] Example 2

[0037] This embodiment provides a self-lubricating material, the raw materials of which are: Sn 11.0%, Ni 1.5%, Cu 87.5%.

[0038] Its preparation method includes the following steps:

[0039] (1) Weigh each raw material according to the ratio, grind them, and obtain powder with a particle size of 12-23μm;

[0040] (2) Mix the powder obtained in step (1) and place it in the mold (the mold lubricant is zinc stearate), and hold it under a molding pressure of 600 MPa for 30 seconds;

[0041] (3) Vacuum sinter the material obtained in step (2) under the following conditions: control the vacuum degree ≤ 10. -3 Pa, heated to the sintering temperature of 830℃ at a heating rate of 6℃ / min, held at that temperature for 2 hours, and then cooled with the furnace;

[0042] (4) Under a vacuum of ≤100 Pa, the material obtained in step (3) is immersed in lubricating oil at a temperature of 100°C for 4 hours. After immersion, the surface oil of the material is cleaned to obtain a self-lubricating material.

[0043] Example 3

[0044] This embodiment provides a self-lubricating material, the raw materials of which are: Sn 13.0%, Ni 2.5%, Cu 84.5%.

[0045] (1) Weigh each raw material according to the ratio, grind them, and obtain powder with a particle size of 12-23μm;

[0046] (2) Mix the powder obtained in step (1) and place it in the mold (the mold lubricant is zinc stearate), and hold it under a molding pressure of 450 MPa for 60 seconds;

[0047] (3) The material obtained in step (2) is sintered under hydrogen atmosphere protection. The conditions are: control the H2 flow rate to 1.0 L / min, raise the temperature to 850℃ at a heating rate of 10℃ / min, hold for 2.5 hours, and cool with the furnace.

[0048] (4) Under a vacuum of ≤100 Pa, the material obtained in step (3) is immersed in lubricating oil at a temperature of 100°C for 4 hours. After immersion, the surface oil of the material is cleaned to obtain a self-lubricating material.

[0049] Comparative Example 1

[0050] This comparative example provides a material whose raw materials are: Sn 12.0% and Cu 88.0%. The preparation method of this comparative example material is the same as that in Example 1.

[0051] Comparative Example 2

[0052] This comparative example provides a material whose raw materials are: Ni 2.0% and Cu 98.0%. The preparation method of this comparative example material is the same as that in Example 1.

[0053] Comparative Example 3

[0054] This comparative example provides a material, the raw materials of which are the same as in Example 1. The preparation method of this comparative example material is gravity casting, specifically including:

[0055] (1) Weigh each raw material (Sn 12.0%, Ni 2.0%, Cu 86.0%) according to the ratio, place them in a medium frequency induction melting furnace for melting, melt at 1200℃, and hold for 30 minutes to ensure that the alloying elements are fully melted and uniform;

[0056] (2) The molten metal is poured into a metal mold at a casting temperature of 1150℃ and allowed to cool and solidify naturally.

[0057] (3) After demolding, the casting is machined to obtain a sample of the required size for testing.

[0058] Test Example 1: Pore Structure

[0059] The pore structure of the materials obtained in step (3) of Examples 1-3 and Comparative Examples 1-3 was tested, and the results are shown in Table 1 below.

[0060] Detection method:

[0061] Porosity: Archimedes drainage method (GB / T 5163);

[0062] Pore ​​size distribution: Mercury porosimetry (GB / T 21650.1);

[0063] Pore ​​connectivity: fluid permeation method;

[0064] Specific surface area: BET method (GB / T 19587).

[0065] Table 1

[0066]

[0067] Note: Comparative Example 3 is a gravity-cast dense material with no interconnected pore structure, therefore, related items are not tested.

[0068] The results show that: Examples 1-3 of the present invention obtained copper-based alloy materials with high interconnected pores through powder metallurgy process, with a porosity of 20.8%-25.3% and pore connectivity of over 90%; compared with Comparative Example 1 (without Ni) and Comparative Example 2 (without Sn), the alloy system with the addition of both Sn and Ni can obtain higher pore connectivity and specific surface area, which is beneficial for storing lubricating oil; Comparative Example 3, which was gravity cast, is a dense alloy without interconnected oil storage pores and cannot achieve oil immersion self-lubrication.

[0069] Test Example 2: Mechanical Property Testing

[0070] The mechanical properties of the materials obtained in step (3) of Examples 1-3 and Comparative Examples 1-3 were tested and compared with elemental Cu. The results are shown in Table 2 below.

[0071] Detection method:

[0072] Tensile strength: GB / T 228.1;

[0073] Yield strength: GB / T 228.1;

[0074] Elongation: GB / T 228.1;

[0075] Hardness: GB / T 231;

[0076] Elastic modulus: GB / T 223.15.

[0077] Table 2

[0078]

[0079] The results show that, compared with elemental copper, the materials in Examples 1-3 of this invention exhibit significantly improved tensile strength and hardness under the solid solution strengthening effect of Sn and Ni; compared with Comparative Example 1 containing only Sn, the introduction of Ni further enhances the matrix strength and hardness; compared with Comparative Example 2 containing only Ni, Sn can significantly improve the alloy's hardness and wear resistance. Comparative Example 3, prepared by gravity casting, has the highest mechanical properties, but lacks oil-retaining pores and does not meet the self-lubricating requirements. The porous material prepared by powder metallurgy in this invention balances suitable pore size for oil storage with sufficient mechanical strength, meeting the load-bearing requirements of wind turbine bearings.

[0080] Test Example 3: Corrosion Resistance Test

[0081] Corrosion resistance tests were conducted on the materials prepared in Examples 1-3 and Comparative Examples 1-3.

[0082] Test methods

[0083] Salt spray test: GB / T 10125 (neutral salt spray, 5% NaCl, 35℃);

[0084] Immersion test: GB / T 10124 (Seawater / Artificial Seawater);

[0085] Electrochemical testing: GB / T 24196 (polarization curves, electrochemical impedance spectroscopy).

[0086] The results are shown in Table 3 below.

[0087] Table 3

[0088]

[0089] The results showed that the samples in Examples 1-3 of this invention exhibited lower salt spray corrosion and seawater immersion corrosion rates, more positive corrosion potentials, and superior resistance to marine salt spray corrosion compared to Comparative Example 1 (without Ni) and Comparative Example 2 (without Sn). The synergistic effect of Sn and Ni promoted the formation of a dense passivation film and SnO2 oxide film on the alloy surface, resisting chloride ion corrosion and making it suitable for high-salt and high-humidity marine conditions. Comparative Example 3, using gravity casting, showed the best corrosion resistance, but its lack of interconnected pores prevented self-lubrication.

[0090] Test Example 4: Heat Resistance Test

[0091] The heat resistance of the self-lubricating materials of Example 1 and Comparative Example 1 was tested, and the results are shown in Table 4 below.

[0092] Test methods

[0093] High-temperature tensile testing: GB / T 4338;

[0094] High-temperature hardness: GB / T 4342;

[0095] Thermogravimetric analysis: GB / T 27761.

[0096] Table 4

[0097]

[0098] The results showed that the self-lubricating material provided by this invention retained ≥75% of its tensile strength at 300℃; Ni element stabilized the grain boundaries, and its resistance to high-temperature softening was superior to CuSn12 (Comparative Example 1); the oxide film was dense, and the weight gain during high-temperature oxidation was <1.2 mg / cm³. 2 ·h.

[0099] Test Example 5: Friction Performance Testing

[0100] The frictional properties of the self-lubricating materials prepared in Examples 1-3 and Comparative Examples 1-3 were tested and compared with Cu. The results are shown in Table 5 below.

[0101] Test method: The pin-disc friction and wear tester (GB / T 12444) was used. The test conditions were: load 50 N, speed 200 r / min, temperature 90±2℃, lubrication with lubricating oil (ISO VG 460), test time 2 hours, and wear rate was calculated by measuring wear volume with a three-dimensional profilometer.

[0102] Table 5

[0103]

[0104] Note: Comparative Example 3 is a dense material formed by gravity casting. Although it was treated with oil immersion, it had no oil storage pores. The surface lubricating oil was squeezed out in the early stage of the test, and the lubrication effect decreased rapidly.

[0105] The results showed that the un-oil-impregnated sintered matrix had a high coefficient of friction and a large wear rate; the self-lubricating materials of Examples 1-3 of the present invention, after vacuum oil impregnation, had a coefficient of friction as low as 0.038-0.045, and a wear rate significantly lower than that of the comparative examples. Comparative Examples 1 and 2 alloys lacked Sn-Ni synergy, resulting in significantly worse coefficients of friction and wear rates; the densely cast Comparative Example 3 lacked oil-retaining pores, leading to easy oil loss and the worst tribological performance. This demonstrates that the components of the present invention, combined with the porous oil impregnation process, synergistically achieve excellent self-lubricating tribological performance.

[0106] Example 4

[0107] Supporting efficient power generation of large-capacity units

[0108] As wind farm development shifts towards large-capacity, offshore units, the high load-bearing capacity of sliding bearings enables them to adapt to higher loads. Self-lubricating technology ensures stable operation of these large units under full-power conditions, avoiding power reduction due to bearing overheating or wear, thus fully realizing the power generation potential of large units.

[0109] Quantitative example: Taking a 100MW wind farm as an example, if the annual downtime due to failure is reduced by 50 hours and the planned maintenance downtime is reduced by 30 hours due to improved lubrication of the main shaft bearing, the annual power generation time can be improved by about 80 hours. Based on the equivalent full-load hours of 2500h, the power generation can be increased by about 3.2%.

[0110] Although the present invention has been described in detail above with general descriptions and specific embodiments, modifications or improvements can be made to it, which will be obvious to those skilled in the art. Therefore, all such modifications or improvements made without departing from the spirit of the present invention fall within the scope of protection claimed by the present invention.

Claims

1. A method for preparing a self-lubricating material, characterized in that, The method includes: The raw material composition by mass fraction is: Sn 11.0%~13.0%, Ni 1.5%~2.5%, with the balance being Cu, and the total mass fraction of impurities ≤1.0%. The raw material powders are weighed according to the proportions, mixed evenly, and the resulting mixed powder is sequentially subjected to molding, sintering, and oil impregnation to obtain the self-lubricating material.

2. The method for preparing the self-lubricating material according to claim 1, characterized in that, The raw material composition is: Sn 12.0%, Ni 2.0%, balance Cu, and total impurity mass fraction ≤1.0%.

3. The method for preparing the self-lubricating material according to claim 1, characterized in that, The particle size of the raw material powder is 12-23 μm; The particle size of the mixed powder is 50-100 μm.

4. The method for preparing the self-lubricating material according to claim 1, characterized in that, The molding conditions are: molding pressure 400~600 MPa, holding time 30~60 seconds; zinc stearate or graphite emulsion is used as mold lubricant.

5. The method for preparing the self-lubricating material according to claim 1, characterized in that, The sintering process employs vacuum sintering or hydrogen atmosphere-protected sintering, wherein... The vacuum sintering conditions are as follows: sintering temperature 800~850℃, holding time 2~3 hours, heating rate 5~10℃ / min, furnace cooling, and vacuum degree ≤10. -3 Pa; The conditions for hydrogen atmosphere-protected sintering are: sintering temperature 820~870℃, holding time 2~2.5 hours, heating rate 5~10℃ / min, furnace cooling, and hydrogen flow rate 0.5~1.0 L / min.

6. The method for preparing the self-lubricating material according to claim 1, characterized in that, The conditions for the oil immersion treatment are as follows: under a vacuum of ≤100 Pa, the sintered material is immersed in lubricating oil for immersion at an oil immersion temperature of 80~120℃ for 2~6 hours, and the floating oil on the surface of the material is cleaned after immersion.

7. The method for preparing the self-lubricating material according to claim 1, characterized in that, Before mixing, the method further includes adding graphite at a mass fraction of 1% to 5%, wherein the graphite has a particle size of 10-30 μm.

8. A self-lubricating material, characterized in that, It is prepared by any one of the preparation methods described in claims 1-7.

9. The application of the self-lubricating material according to claim 8 in the preparation of sliding bearings for offshore wind turbines.