A microchannel heat exchange cold plate material, its preparation method and application
By using a gradient distribution of titanium powder and diamond particles and a micron-level groove coating, combined with a specific sintering process, the heat dissipation and corrosion resistance problems of microchannel cold plates in high-temperature and high-corrosion environments have been solved, achieving a balance between high thermal conductivity and processability, making it suitable for thermal management in aerospace and deep-sea exploration.
Patent Information
- Application Number
- CN202611177123.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-05
- Publication Date
- 2026-11-17
AI Technical Summary
Existing microchannel cold plates are prone to softening and corrosion failure under high temperature, high corrosion and strong vibration conditions, making it difficult to achieve both high thermal conductivity and excellent processability at the same time. In addition, the heat exchange interface has high thermal resistance and insufficient corrosion resistance.
Microchannel heat exchange cold plate material is prepared by using gradient-distributed titanium powder and diamond particles. The inner wall of the microchannel is provided with micron-level grooves and coated with a microcrystalline carbon coating. The material achieves high thermal conductivity and corrosion resistance through a two-stage stepped vacuum sintering and hot rolling process combined with cold isostatic pressing technology.
It achieves efficient heat dissipation of cold plate materials in high temperature and high corrosion environment, with thermal conductivity increased to 300~450W/(m·K), salt spray corrosion resistance time exceeding 500h, and compressive strength retention rate ≥90%, making it suitable for thermal management of aerospace and deep-sea exploration.
Smart Images

Figure CN123102985A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of thermal management materials technology, specifically relating to a microchannel heat exchange cold plate material, its preparation method, and its application. Background Technology
[0002] In aerospace, industrial manufacturing, and deep-sea exploration, equipment often operates under complex conditions of high temperature, high corrosion, and strong vibration. The heat flux density of its internal heat-generating components (such as aero-engine control system chips, industrial high-temperature sensors, and deep-sea probe circuit modules) is extremely high, and stringent requirements are placed on the structural stability and corrosion resistance of heat dissipation components. Traditional microchannel cold plates are mostly made of aluminum, copper, or their alloys. Although they have certain thermal conductivity, they are prone to softening in high-temperature environments (such as above 200°C), resulting in a significant decrease in structural strength. In corrosive environments (such as deep-sea salt spray and industrial acid / alkali atmospheres), they are susceptible to corrosion failure, leading to cold plate leakage and affecting the normal operation of the equipment. To improve the high temperature resistance and corrosion resistance of cold plates, researchers have tried to use titanium alloys to prepare microchannel cold plates. Titanium alloys have excellent high temperature resistance (melting point of about 1668℃) and corrosion resistance (strong stability in seawater and acid and alkaline environments), but their thermal conductivity is low (about 17-21 W / (m·K)), which is only about 1 / 10 of that of pure aluminum, and the heat dissipation efficiency is difficult to meet the requirements of high power density equipment.
[0003] In other words, existing uniform titanium / diamond composite materials, if the diamond content is low, have limited improvement in thermal conductivity and cannot meet the heat dissipation requirements of high heat flux density components. If the overall diamond content is increased, the material's brittleness increases significantly, making it difficult to complete forming processes such as rolling and etching. The sintering process is prone to generating pore defects, posing a risk of coolant leakage. Conventional titanium alloy microchannels lack reinforced thermal conductivity and corrosion protection structures on their inner walls, resulting in high thermal resistance at the heat exchange interface and susceptibility to corrosion failure under salt spray and high-temperature conditions.
[0004] Therefore, how to simultaneously achieve high thermal conductivity and excellent processability in titanium-based cold plates, while improving the heat exchange efficiency of the microchannel inner wall and enhancing the corrosion resistance and high temperature resistance of the substrate, has become a technical problem that urgently needs to be solved in this field. Summary of the Invention
[0005] The purpose of this section is to outline some aspects of embodiments of the present invention and to briefly describe some preferred embodiments. Simplifications or omissions may be made in this section, as well as in the abstract and title of this application, to avoid obscuring the purpose of these documents; however, such simplifications or omissions should not be construed as limiting the scope of the invention.
[0006] In view of the problems existing in the above and / or prior art, the present invention is proposed.
[0007] Therefore, the purpose of this invention is to overcome the shortcomings of the prior art and provide a microchannel heat exchange cold plate material.
[0008] To solve the above technical problems, the present invention provides the following technical solution: the microchannel heat exchange cold plate material body is prepared by powder metallurgy from titanium powder and diamond particles, the body thickness is 0.5-2mm, the surface of the body is etched with microchannels, the inner wall of the microchannel is provided with micron-level groove structure, and the surface of the micron-level groove is coated with microcrystalline carbon coating. The diamond particles are distributed in a gradient within the titanium powder matrix, with the volume fraction of diamond increasing from the outer surface of the cold plate to the inner wall of the microchannel in the range of 10%-40%, and the particle size decreasing in the range of 5μm-1μm.
[0009] As a preferred embodiment of the microchannel heat exchange cold plate material of the present invention, the microchannel has a cross-section including a regular hexagon, a rectangle or an inverted trapezoid, a width of 0.8-2mm, a height of 1.5-2mm, a spacing of 0.5-1.5mm between adjacent microchannels, and a surface roughness Ra≤1.6μm.
[0010] As a preferred embodiment of the microchannel heat exchange cold plate material of the present invention, the titanium powder has a purity of ≥99.5% and a particle size of 10-50μm; the diamond particles are high-temperature high-pressure synthetic diamond or chemical vapor deposition diamond, with a purity of ≥99.9%.
[0011] As a preferred embodiment of the microchannel heat exchange cold plate material of the present invention, the microcrystalline carbon coating is obtained by coating and immersing the microcrystalline carbon paint for 20 seconds, suspending and leveling it, and drying it at 120°C for 30 minutes, with a thickness of 8-30 μm; wherein the microcrystalline carbon paint is obtained by compounding polyacrylic acid, microcrystalline graphite and CNT in a mass ratio of 6:3:2, using water as the dispersion medium, and has a solid content of 11%.
[0012] As a preferred embodiment of the microchannel heat exchange cold plate material of the present invention, wherein: the bonding strength between the microcrystalline carbon coating and the inner wall of the microchannel is ≥10MPa, and the thermal conductivity is ≥200W / (m·K).
[0013] Another objective of this invention is to provide a method for preparing a microchannel heat exchange cold plate material.
[0014] To solve the above-mentioned technical problems, the present invention provides the following technical solution: including, Titanium powder and diamond particles of different volume fractions are ultrasonically mixed at an ultrasonic power of 300-500W for 30-60 minutes to obtain mixed powders with different diamond contents. Sintering aids of 0.5%-2% of the total mass of the mixed powder are added, and the mixture is wet ball-milled with alcohol at a speed of 200-300r / min for 4-8 hours. After ball milling and drying, titanium / diamond composite powders with different diamond mass fractions are obtained. Titanium / diamond composite powders with different diamond volume fractions were layered and loaded into a mold, and then pressed using a cold isostatic pressing process. The pressing pressure was 80-120 MPa and the holding time was 5-10 min to obtain cold plate blanks with different diamond volume fractions. The cold-rolled steel blanks were placed into a vacuum sintering furnace for sintering in descending order of diamond volume fraction and diamond particle size, starting from the outer surface of the cold-rolled steel blank and moving towards the inner wall of the microchannel. The pressure was 10 MPa and the vacuum degree was ≤1×10⁻⁶. -3 Under the conditions of Pa, the temperature is first raised to 800-900℃ at a rate of 5-10℃ / min and held for 2-3 hours. Then, the temperature is raised to 1200-1400℃ at a rate of 3-5℃ / min and held for 4-6 hours. After sintering, the plate is hot rolled at 800-1000℃ for 15-20 minutes to obtain the cold plate body. The cold plate body is etched with microchannels with micron-level grooves using precision etching technology, and then a microcrystalline carbon coating is applied to the surface of the micron-level groove structure to obtain the microchannel heat exchange cold plate material.
[0015] In a preferred embodiment of the preparation method of the microchannel heat exchange cold plate material of the present invention, the sintering aid is obtained by mixing titanium boron alloy powder and phenolic resin in a mass ratio of 1:1.
[0016] As a preferred embodiment of the preparation method of the microchannel heat exchange cold plate material of the present invention, wherein: the spray pressure of the precision etching is 3MPa, the temperature is 40-50℃, and the etchant comprises 10 parts ammonium bifluoride, 5 parts sodium nitrate, 15 parts nitric acid, and 1 part ethylenediaminetetraacetic acid by mass.
[0017] Another objective of this invention is to provide an application of a microchannel heat exchange cold plate material for efficient heat dissipation of heating elements under harsh operating conditions of high temperature, high corrosion, and high vibration.
[0018] Beneficial effects of this invention: (1) The invention utilizes a diamond gradient distribution design. The outer layer relies on large-particle-size, low-filling diamonds to retain the plasticity of the titanium matrix, enabling the smooth completion of the entire processing cycle, including cold isostatic pressing, hot rolling, and precision etching. The high proportion of fine diamonds is concentrated at the heat exchange interface, significantly reducing the interface thermal resistance. At the same time, the fine particles fill the sintering pores, eliminating leakage defects in the flow channels. The final overall thermal conductivity of the cold plate reaches 300~450W / (m·K), and there is no cracking during rolling, solving the technical defect that traditional materials cannot simultaneously achieve both thermal conductivity and processing performance.
[0019] (2) This invention prepares micron-level grooves by precisely etching the inner wall of the flow channel, thereby increasing the heat exchange contact area of the fluid by a factor of two. The matching microcrystalline carbon coating can not only fill the micropores of the grooves to block the corrosive medium from penetrating into the titanium substrate, but also further reduce the solid-liquid heat exchange thermal resistance. It is suitable for harsh corrosive conditions such as deep-sea salt spray, industrial acid and alkali, and high temperature in aviation, and overcomes the defects of ordinary titanium cold plates that are easy to corrode and have low heat exchange efficiency.
[0020] (3) The present invention adopts a two-stage stepped vacuum sintering process. The low temperature of 800~900℃ fully removes the adsorbed gas of the powder, and the high temperature of 1200~1400℃ achieves a dense bond between the titanium and diamond interface. At the same time, combined with the hot rolling process, the bonding between the composite layers of each gradient is tight and there is no delamination. It has excellent compressive strength and is not easy to deform and crack under strong vibration conditions, thus meeting the long-term vibration service requirements of aero-engines and deep-sea probes. Attached Figure Description
[0021] To more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings used in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort. Wherein: Figure 1 This is a schematic diagram of different cross-sections of the microchannel etched on the surface of the microchannel heat exchange cold plate material according to the present invention.
[0022] Figure 2 This is a schematic diagram of the layered structure of the gradient titanium / diamond composite cold plate body in Embodiment 1 of the present invention.
[0023] Figure 3 This is a physical image of the single heat exchange plate material obtained in Embodiment 1 of the present invention.
[0024] Figure 4 This is a magnified view of the titanium and diamond interface inside the flow channel after cross-sectional structure of the microchannel inner wall in Embodiment 1 of the present invention. Detailed Implementation
[0025] To make the above-mentioned objects, features and advantages of the present invention more apparent and understandable, the specific embodiments of the present invention will be described in detail below with reference to the examples in the specification.
[0026] Many specific details are set forth in the following description in order to provide a full understanding of the invention. However, the invention may also be practiced in other ways different from those described herein, and those skilled in the art can make similar extensions without departing from the spirit of the invention. Therefore, the invention is not limited to the specific embodiments disclosed below.
[0027] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The phrase "in one embodiment" appearing in different places in this specification does not necessarily refer to the same embodiment, nor is it a single or selective embodiment that is mutually exclusive with other embodiments.
[0028] Unless otherwise specified, all raw materials used in this invention are commercially available in the field. Among them, microcrystalline graphene was purchased from Hunan Runzhong New Materials Co., Ltd., model TT-99Ultral; polyacrylic acid PAA was purchased from Hunan Linte Technology Co., Ltd., model 9102; and CNTs were short carboxylated multi-walled carbon nanotubes, purchased from Maclean, CAS number 308068-56-6.
[0029] The relevant properties of the microchannel heat exchange cold plate material prepared by this invention were determined using the following method: The flow channel dimensions were measured using a 2D measuring instrument. Thermal conductivity was determined by laser scintillation method, referring to national standard GB / T231.1. Powder particle size was measured using a laser particle size analyzer. The tensile strength is in accordance with GB / T 228.1 standard.
[0030] The present invention relates to microchannels etched on the surface of a microchannel heat exchanger cold plate material, the cross-section of which includes regular hexagons, rectangles, or inverted trapezoids. The width of each microchannel is 0.8-2 mm, the height is 1.5-2 mm, and the spacing between adjacent microchannels is 0.5-1.5 mm. Schematic diagrams of each shape are shown below. Figure 1 As shown.
[0031] Example 1 This embodiment provides a method for preparing a microchannel heat exchange cold plate material, specifically: 1) Titanium powder (purity ≥99.5%, particle size 30μm) was ultrasonically mixed with 1μm diamond (40% titanium powder), 2μm diamond (30% titanium powder), 3μm diamond (20% titanium powder), and 4μm diamond (10% titanium powder) at an ultrasonic power of 450W for 50min to obtain mixed powders F1, F2, F3, and F4. Sintering aid (titanium boron alloy powder and phenolic resin, mixed in a 1:1 ratio) was added to each of the mixed powders F1, F2, F3 and F4 respectively. The powders were then subjected to alcohol wet ball milling at a speed of 250 r / min for 6 h. After drying, titanium / diamond composite powders with different volume fractions were obtained. 2) Titanium / diamond composite powders of different volume fractions were layered and loaded into a mold, and pressed using a cold isostatic pressing process. The pressing pressure was 100 MPa and the holding time was 8 min, resulting in four kinds of titanium / diamond cold plate blanks with different volume fractions. 3) Place the cold-rolled steel blanks into the vacuum sintering furnace in the order of F1, F2, F3, and F4 from top to bottom. The pressure is 10 MPa and the vacuum degree is 1×10⁻⁶. -3 P is heated to 850℃ at a rate of 8℃ / min and held for 3 hours, then heated to 1300℃ at a rate of 3℃ / min and held for 5 hours. After sintering, a titanium / diamond composite material blank is obtained. The blank is then hot rolled at 900℃ for 15 minutes to obtain a rolled plate body with a final thickness of 0.8 mm.
[0032] Figure 2 The diagram shows the layered structure of the gradient titanium / diamond composite cold plate. Figure a shows the isometric structure of the four gradient powder layers F1, F2, F3, and F4. Figure b shows a simplified schematic diagram of the diamond particle distribution in each layer. Figure c shows a metallographic micrograph of the interface between the gradient titanium matrix and the diamond particles.
[0033] 4) Microchannels are etched on the surface of the rolled plate body (F1 layer). The cross-sectional shape is rectangular. The width of the microchannel is 0.8 mm, the height is 1.5, and the spacing between adjacent microchannels is 0.5. Precision etching technology is used. The spray pressure is set to 3 MPa, the temperature is 45℃, and the etchant formula is 10 parts ammonium bifluoride, 5 parts sodium nitrate, 15 parts nitric acid, and 1 part ethylenediaminetetraacetic acid to form microchannels with a roughness of 1.6 μm.
[0034] 5) A microcrystalline carbon coating is applied to the inner wall of the microchannel. The coating formulation consists of polyacrylic acid, microcrystalline graphene, and CNT in a mass ratio of 6:3:2, with water as the dispersion medium and a solid content of 11%. After immersion in the coating for 20 seconds, it is suspended for leveling and dried at 120℃ for 30 minutes, thus forming a microcrystalline carbon coating on the inner wall of the microchannel. The bonding strength between the microcrystalline carbon coating and the inner wall of the microchannel is ≥10MPa, and the thermal conductivity is ≥200W / (m·K), resulting in a single-piece heat exchange plate material. A physical image of the material is shown below. Figure 3As shown, the surface of the cold plate body is etched with parallel linear rectangular microchannels. The cold plate is equipped with laser-welded liquid inlet and liquid outlet connectors at both ends. The welded joints are reinforced with ribs, and the inside of the joints is equipped with a filter screen for intercepting impurities. The inner wall of the microchannels is precisely etched to form a micron-level groove structure.
[0035] Figure 4 This is a magnified view of the titanium and diamond interface inside the flow channel after cross-sectional structure of the microchannel inner wall in Embodiment 1 of the present invention; the microcrystalline carbon coating covers the surface of the micron-level trench and fills the micropores of the trench, which is used to reduce the thermal resistance of the heat exchange interface and block the penetration of corrosive media into the substrate. Because the diamond particles on the F1 surface are small, there will be no large pits and protrusions caused by the diamond particles falling off due to excessively large particles during the etching process. At the same time, the graphite carbon coating is used to further smooth the surface.
[0036] Two heat exchanger plates were taken and diffused together, aligned and bonded, and fixed with a graphite limiting fixture before being placed into a vacuum diffusion welding furnace; a vacuum of 8×10⁻⁶ was then evacuated. -4 Pa, the temperature is increased to 850℃ at 6℃ / min and held for 30min, then increased to 930℃, and a pressure of 4MPa is applied and held for 100min; then the temperature is decreased to 600℃ at 5℃ / min to release the pressure, and the furnace is cooled to room temperature. The atomic diffusion at the interface of the two plates achieves metallurgical bonding, resulting in a completely sealed core plate with microchannel heat exchange cold plate material in this embodiment.
[0037] Tests have shown that the thermal conductivity of the heat exchange cold plate in this embodiment can reach 320W / (m·K), the compressive strength retention rate is ≥90% (after welding) in a high temperature environment of 300℃, and the salt spray corrosion resistance time is ≥500h. It is suitable for thermal management scenarios with high and harsh working conditions such as aerospace engines, industrial high temperature equipment, and deep-sea exploration instruments.
[0038] Example 2 The difference from Example 1 is that step 1 is adjusted. Titanium powder was ultrasonically mixed with 2μm diamond (35% titanium powder), 3μm diamond (30% titanium powder), 4μm diamond (25% titanium powder), and 5μm diamond (20% titanium powder) at an ultrasonic power of 450W for 30 minutes to obtain mixed powders F1, F2, F3, and F4. The remaining steps were carried out in accordance with Example 1 to obtain the microchannel heat exchange cold plate material of this embodiment.
[0039] Comparative Example 1 The difference between this comparative example and Example 1 is that the volume fraction of diamond in each mixed powder in step 1) is adjusted to be consistent, all being 40%, and the diamond particle size is 0.3 μm. The remaining steps are the same as in Example 1. As a result, the subsequent processing cannot be rolled.
[0040] Comparative Example 2 The difference between this comparative example and Example 1 is that step 1) is adjusted. Titanium powder was ultrasonically mixed with 5μm diamond (50% titanium powder), 4μm diamond (35% titanium powder), 2μm diamond (20% titanium powder), and 1μm diamond (5% titanium powder) at an ultrasonic power of 450W for 30 minutes to obtain mixed powders F1, F2, F3, and F4. The remaining steps were carried out in accordance with Example 1 to obtain the microchannel heat exchange cold plate material of this comparative example.
[0041] Comparative Example 3 The difference between this comparative example and Example 1 is that step 1) is adjusted. Titanium powder was ultrasonically mixed with 1μm diamond (10% of titanium powder), 2μm diamond (20% of titanium powder), 3μm diamond (30% of titanium powder), and 4μm diamond (40% of titanium powder) at an ultrasonic power of 450W for 50 minutes to obtain mixed powders F1, F2, F3, and F4. The remaining steps and processes are the same as in Example 1, resulting in the microchannel heat exchange cold plate material of this comparative example. The relevant properties of the microchannel heat exchange cold plate materials prepared in Examples 1-2 and Comparative Examples 1-3 were measured, and the results are shown in Table 1.
[0042] Table 1
[0043] As can be seen from Table 1, the microchannel heat exchange cold plate materials prepared in Examples 1 and 2 of the present invention have excellent comprehensive performance. This is because, in the gradient design concept of the present invention, the outer layer has low diamond content and large particle size, which preserves the plasticity of the titanium matrix and prevents cracking during hot rolling and etching. The inner layer of the microchannel has high diamond content and fine particle size, which is concentrated at the heat exchange interface to greatly improve the overall thermal conductivity. The fine diamond fills the sintered micropores to prevent coolant leakage, and the gradient transition eliminates interlayer stress.
[0044] In Comparative Example 1, the diamond content was 40%, and the titanium matrix completely lost its plasticity. After sintering, the composite material was extremely brittle and fractured directly under rolling stress. In Comparative Example 2, the outer layer had a diamond content of only 5%, which limited the improvement in thermal conductivity of the matrix. The inner layer had a maximum of 50% diamond, which was too brittle. Rolling produced surface through-cracks, increased sintering pores, and made it easy for corrosive media to penetrate the matrix. The strength, thermal conductivity, and corrosion resistance all declined significantly. In Comparative Example 3, the gradient order was adjusted. The outer layer had a high proportion of large diamond particles, which made it easy to crack during rolling. The heat exchange inner wall had only a low proportion of fine diamond. The high thermal conductivity reinforcing phase in the core heat dissipation area was missing, and the overall thermal conductivity plummeted. At the same time, the inner layer had many pores, which significantly deteriorated the corrosion resistance. In addition, large diamond particles were present on the surface during the etching process. After etching, a large number of pits caused by diamond particles falling off and diamond protrusions that did not fall off appeared on the surface. This directly proves that the increasing volume fraction and decreasing particle size of diamond from the outside to the inside in this invention is a necessary innovative structure that takes into account both processing and heat dissipation.
[0045] Example 3 The difference from Example 1 is that step 2 is adjusted. Titanium / diamond composite powders of different volume fractions were layered and loaded into a mold, and then pressed using a cold isostatic pressing process. The pressing pressure was 80 MPa and the holding time was 5 min, resulting in four titanium / diamond cold plate blanks with different volume fractions. The remaining steps and processes were the same as in Example 1, thus obtaining the microchannel heat exchange cold plate material of this example.
[0046] Comparative Example 4 Titanium / diamond composite powders of different volume fractions were layered and loaded into a mold, and pressed using a cold isostatic pressing process. The pressing pressure was 50 MPa and the holding time was 15 min, resulting in four titanium / diamond cold plate blanks with different volume fractions. The remaining steps and processes were the same as in Example 1, resulting in the microchannel heat exchange cold plate material of this comparative example, which showed cracking in appearance.
[0047] Comparative Example 5 Titanium / diamond composite powders of different volume fractions were layered and loaded into a mold, and then pressed using a cold isostatic pressing process. The pressing pressure was 140 MPa and the holding time was 3 min, resulting in four titanium / diamond cold plate blanks with different volume fractions. The remaining steps were the same as in Example 1, thus obtaining the microchannel heat exchange cold plate material of this comparative example.
[0048] The relevant properties of the microchannel heat exchange cold plate materials prepared in Example 3 and Comparative Examples 4 to 5 were measured and compared with those in Example 1. The results are shown in Table 2.
[0049] Table 2
[0050] As can be seen from Table 2, the gradient powder of this invention is a four-layer powder with different components, which has strict requirements on the isostatic pressure window. 80~120MPa is the exclusive process range suitable for the gradient layered system. Unlike the pressing process of a single uniform powder, the powder of Comparative Example 4 is not compacted enough, and there are a large number of interconnected pores inside the gradient layer. After sintering, the pores cannot be eliminated and are easy to break under stress. The pores become channels for the penetration of corrosive media, and the salt spray resistance is significantly reduced. The four-layer powder of Comparative Example 5 has large differences in diamond content and particle size. Under high pressure, the plastic deformation of each layer is inconsistent, and huge internal stress is generated between the layers, which directly delaminates the layers. Subsequent sintering and rolling are completely ineffective.
[0051] Example 4 The difference from Example 1 is that step 3 is adjusted. The cold-rolled steel blanks were placed in a vacuum sintering furnace at pressures of 10 MPa (F1, F2, F3, F4). The furnace was first heated to 800℃ at a rate of 10℃ / min and held for 2 hours, then heated to 1200℃ at a rate of 5℃ / min and held for 5 hours. The vacuum degree was 1×10⁻⁶. - 3 Pa, to obtain a titanium / diamond composite material billet, the billet is hot rolled at 800℃ for a time, and the final rolled plate thickness is controlled at 0.8mm. The remaining steps and processes are the same as in Example 1, to obtain the microchannel heat exchange cold plate material of this example.
[0052] Comparative Example 6 The difference from Example 1 is that step 3 is adjusted. The cold-rolled steel blanks were placed into a vacuum sintering furnace at pressures of 10 MPa (F1, F2, F3, F4), and heated directly to 1300℃ at a rate of 10℃ / min, held for 4 hours, with a vacuum degree of 1×10⁻⁶. -3 Pa, to obtain a titanium / diamond composite material billet, the billet is hot rolled at 900℃ for a time, the final rolled plate thickness is controlled at 0.8mm, the remaining steps are the same as in Example 1, to obtain the microchannel heat exchange cold plate material of this comparative example, which has cracks in appearance.
[0053] Comparative Example 7 The difference from Example 1 is that step 3 is adjusted. The cold-rolled steel blanks are placed into the vacuum sintering furnace in the order of F1, F2, F3, and F4 from top to bottom. The pressure is 10 MPa and the vacuum degree is 1×10⁻⁶. -3P was heated to 850℃ at a rate of 8℃ / min and held for 3 hours, then heated to 1300℃ at a rate of 3℃ / min and held for 5 hours. After sintering, a titanium / diamond composite material blank was obtained. The blank was then hot-rolled at 700℃ for a time until the final rolled plate thickness was controlled at 0.8 mm. The remaining steps were the same as in Example 1. The resulting microchannel heat exchange cold plate material exhibited cracking.
[0054] The relevant properties of the microchannel heat exchange cold plate materials prepared in Example 4 and Comparative Examples 6 to 7 were measured and compared with those in Example 1. The results are shown in Table 3.
[0055] Table 3
[0056] As can be seen from Table 3, the two-stage sintering and temperature-controlled hot rolling of the present invention is the key process to solve the problems of porosity, delamination, and insufficient plasticity of the gradient composite layer. In Comparative Example 6, without segmented sintering, the gas inside the powder cannot be discharged, and a large number of pores are closed after sintering. The pores cut off the heat conduction path and significantly reduce the tensile strength. Corrosive media tend to accumulate inside the pores, and the salt spray resistance drops sharply. In Comparative Example 7, the temperature is lower than the plasticity critical temperature of the titanium matrix. Stress concentration occurs during the deformation process of the gradient plate, resulting in irreversible through cracks and loss of usability.
[0057] In summary, this invention pioneers a diamond gradient distribution structure within a titanium matrix, limiting the diamond volume fraction to increase from 10% to 40% from the outer surface of the cold plate to the inner wall of the microchannel, and decreasing the particle size from 5μm to 1μm. This breaks through the technical bottleneck of the mutual constraint between thermal conductivity and processing plasticity in traditional uniform composites. The low content of large-particle diamonds in the outer layer ensures that the plate can be rolled and etched smoothly, while the high content of fine diamonds on the heat exchange side concentrates to improve thermal conductivity and seal sintering micropores, achieving a leapfrog improvement in the thermal conductivity of the cold plate from 300 to 450 W / (m·K). Secondly, it is equipped with a two-stage stepped vacuum sintering, limited-range cold isostatic pressing, and temperature-controlled hot rolling process to specifically solve the defects of easy porosity and interlayer delamination in multi-layer gradient powder sintering, and significantly improve the high-temperature mechanical stability of the matrix. Simultaneously, micron-sized grooves are constructed on the inner wall of the microchannel and coated with a self-developed water-based microcrystalline carbon coating, which simultaneously increases the heat exchange area and blocks corrosive media, enabling the material to withstand salt spray for over 500 hours and retain compressive strength of no less than 90% at 300℃. It can be adapted to harsh working conditions such as high temperature corrosion and strong vibration in aviation and deep sea, breaking through the single performance limitations of existing heat dissipation materials.
[0058] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the spirit and scope of the technical solutions of the present invention, and all such modifications or substitutions should be covered within the scope of the claims of the present invention.
Claims
1. A microchannel heat exchange cold plate material, characterized in that: The microchannel heat exchange cold plate material body is prepared by powder metallurgy from titanium powder and diamond particles. The body thickness is 0.5-2mm. Microchannels are etched on the surface of the body. Microchannels have micron-level groove structures on the inner wall of the microchannels. Microcrystalline carbon coating is applied to the surface of the micron-level grooves. The diamond particles are distributed in a gradient within the titanium powder matrix, with the volume fraction of diamond increasing from the outer surface of the cold plate to the inner wall of the microchannel in the range of 10%-40%, and the particle size decreasing in the range of 5μm-1μm.
2. The microchannel heat exchange cold plate material as described in claim 1, characterized in that: The cross-section of the microchannel includes a regular hexagon, a rectangle, or an inverted trapezoid. The width of the microchannel is 0.8-2mm, the height is 1.5-2mm, the spacing between adjacent microchannels is 0.5-1.5mm, and the surface roughness Ra of the microchannel is ≤1.6μm.
3. The microchannel heat exchange cold plate material as described in claim 1, characterized in that: The titanium powder has a purity of ≥99.5% and a particle size of 10-50μm; the diamond particles are high-temperature and high-pressure synthetic diamond or chemical vapor deposition diamond, with a purity of ≥99.9%.
4. The microchannel heat exchange cold plate material as described in claim 1, characterized in that: The microcrystalline carbon coating is obtained by coating with microcrystalline carbon paint, immersing for 20 seconds, suspending and leveling, and drying at 120℃ for 30 minutes, with a thickness of 8-30μm; wherein, the microcrystalline carbon paint is obtained by compounding polyacrylic acid, microcrystalline graphite and CNT in a mass ratio of 6:3:2, using deionized water as the dispersion medium, and has a solid content of 11%.
5. The microchannel heat exchange cold plate material as described in claim 1, characterized in that: The bonding strength between the microcrystalline carbon coating and the inner wall of the microchannel is ≥10MPa, and the thermal conductivity is ≥200W / (m·K).
6. The method for preparing the microchannel heat exchange cold plate material according to any one of claims 1 to 5, characterized in that: include, Titanium powder and diamond particles of different volume fractions are ultrasonically mixed at an ultrasonic power of 300-500W for 30-60 minutes to obtain mixed powders with different diamond contents. Sintering aids of 0.5%-2% of the total mass of the mixed powder are added, and the mixture is wet ball-milled with alcohol at a speed of 200-300r / min for 4-8 hours. After ball milling and drying, titanium / diamond composite powders with different diamond mass fractions are obtained. Titanium / diamond composite powders with different diamond volume fractions were layered and loaded into a mold, and then pressed using a cold isostatic pressing process. The pressing pressure was 80-120 MPa and the holding time was 5-10 min to obtain cold plate blanks with different diamond volume fractions. The cold-rolled steel blanks were placed into a vacuum sintering furnace for sintering in descending order of diamond volume fraction and diamond particle size, starting from the outer surface of the cold-rolled steel blank and moving towards the inner wall of the microchannel. The pressure was 10 MPa and the vacuum degree was ≤1×10⁻⁶. -3 Under the conditions of Pa, the temperature is first raised to 800-900℃ at a rate of 5-10℃ / min and held for 2-3 hours. Then, the temperature is raised to 1200-1400℃ at a rate of 3-5℃ / min and held for 4-6 hours. After sintering, the plate is hot rolled at 800-1000℃ for 15-20 minutes to obtain the cold plate body. The cold plate body is etched with microchannels with micron-level grooves using precision etching technology, and then a microcrystalline carbon coating is applied to the surface of the micron-level groove structure to obtain the microchannel heat exchange cold plate material.
7. The method for preparing the microchannel heat exchange cold plate material as described in claim 6, characterized in that: The sintering aid is obtained by mixing titanium boron alloy powder and phenolic resin in a mass ratio of 1:
1.
8. The method for preparing the microchannel heat exchange cold plate material as described in claim 6, characterized in that: The precision etching process involves a spray pressure of 3 MPa and a temperature of 40-50°C. The etchant comprises, by mass, 10 parts ammonium bifluoride, 5 parts sodium nitrate, 15 parts nitric acid, and 1 part ethylenediaminetetraacetic acid.
9. The application of the microchannel heat exchange cold plate material as described in claim 1 in the efficient heat dissipation of heat-generating elements under harsh working conditions of high temperature, high corrosion, and high vibration.