A porous magnesium-based hydrogen production material based on gradient sintering and its preparation method
By constructing porous magnesium-based hydrogen production materials through gradient sintering, the problems of low mass transfer efficiency and passivation deposition were solved, and the high efficiency and stable hydrogen production performance of magnesium-based materials were achieved, which are suitable for portable hydrogen energy devices and small fuel cells.
Patent Information
- Application Number
- CN202611350098.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-02
- Publication Date
- 2026-11-17
AI Technical Summary
Existing magnesium-based hydrolysis hydrogen production materials suffer from poor mass transfer efficiency, easy passivation of magnesium hydroxide byproducts, and difficulty in uniformly alloying high and low melting point metals, resulting in low hydrogen production efficiency and poor stability.
A gradient sintering process combined with powder metallurgy composite pore-forming is adopted to construct a multi-level porous structure. Magnesium-based materials are prepared by high-energy ball milling and low-energy ball milling to achieve uniform dispersion and alloying of catalytic metals, constructing interconnected porous channels and avoiding passivation deposition.
It significantly improves hydrogen production rate and material utilization, ensures the continuity and stability of hydrolysis reaction, and achieves high-efficiency hydrogen production performance.
Smart Images

Figure CN123102998A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a porous magnesium-based hydrogen production material based on gradient sintering and its preparation method, belonging to the field of hydrogen production material technology. Background Technology
[0002] Hydrogen energy, as a clean, pollution-free, and high-energy-density new secondary energy source, is a core energy carrier for replacing traditional fossil fuels and achieving dual-carbon goals. Distributed, on-demand hydrogen production technology, with its advantages of not requiring high-pressure hydrogen storage, safe transportation, and rapid response, has become a core development direction for portable hydrogen energy devices and small fuel cells. Hydrogen production through the hydrolysis of metal materials, with its advantages of mild reaction conditions, high hydrogen purity, simple equipment requirements, and the ability to produce hydrogen in situ on-demand, effectively avoids the safety risks and high costs associated with hydrogen storage and transportation. It has become a research hotspot in the field of new green hydrogen production, possessing extremely high practical value and application prospects.
[0003] Among various water electrolysis hydrogen production materials, magnesium-based materials possess multiple advantages, including abundant reserves, high theoretical hydrogen production capacity, excellent electrochemical activity, and the resource utilization of byproducts (such as as flame retardants), making them an ideal choice for water electrolysis hydrogen production. However, existing magnesium-based hydrogen production materials face three major technological bottlenecks in practical applications, severely restricting their hydrogen production efficiency and industrial application.
[0004] First, the hydrolysis mass transfer efficiency is poor. Traditional bulk, dense magnesium-based materials have extremely low internal porosity, meaning the hydrolysis reaction can only occur on the material surface. The aqueous solution cannot quickly penetrate into the material's interior, preventing the internal magnesium matrix from fully participating in the reaction, significantly reducing the material's effective utilization rate and overall hydrogen production rate. Second, the passivation problem of byproducts is prominent. Magnesium hydroxide generated from magnesium hydrolysis rapidly deposits on the material surface, forming a dense and stable passivation film. This film blocks the contact between the aqueous solution and the unreacted magnesium matrix, causing the hydrolysis reaction rate to rapidly decline or even terminate prematurely, resulting in actual hydrogen production far below the theoretical value. Third, heterogeneous metal alloying is difficult. Magnesium is a low-melting-point metal, while nickel, copper, cobalt, and other metals are high-melting-point metals. Conventional preparation processes struggle to achieve uniform alloying of these two types of metals. The catalytic metal tends to agglomerate and distribute unevenly, failing to fully exert its catalytic effect. Furthermore, insufficient alloying leads to uneven material reactivity and poor hydrogen production stability.
[0005] Currently, the industry primarily employs methods such as high-energy ball milling to refine grains and doping with catalytic metals to improve the hydrogen production performance of magnesium-based materials. While these methods can enhance the material's reactivity to some extent, they cannot fundamentally solve the problems of mass transfer obstruction and by-product passivation deposition. Furthermore, defects such as uneven composite composition of high and low melting point metals and low alloying degree still exist. Magnesium-based hydrogen production materials prepared by existing modification processes still suffer from poor reaction persistence, insufficient active sites, and unstable hydrogen production efficiency. Therefore, developing a porous magnesium-based hydrogen production material preparation technology that can optimize mass transfer channels, suppress by-product passivation, and achieve uniform alloying of high and low melting point metals is an urgent need in this field of technological research. Summary of the Invention
[0006] The purpose of this invention is to address the technical shortcomings of existing magnesium-based hydrolysis hydrogen production materials, such as impaired mass transfer in the aqueous phase, easy deposition and passivation of magnesium hydroxide byproducts, difficulty in uniform alloying of high and low melting point metals, low hydrogen production efficiency, and poor stability. This invention provides a method for preparing porous magnesium-based hydrogen production materials based on gradient sintering. By using powder metallurgy composite pore-forming and gradient sintering processes, a multi-level porous structure is constructed, simultaneously solving the three major technical challenges of mass transfer, passivation, and alloying. This results in the preparation of porous magnesium-based hydrogen production materials that can be rapidly hydrolyzed, exhibit continuous and stable reactions, and have a high hydrogen production conversion rate.
[0007] Meanwhile, this invention provides a porous magnesium-based hydrogen production material based on gradient sintering.
[0008] Meanwhile, this invention provides an application of a porous magnesium-based hydrogen production material based on gradient sintering in the fields of ambient temperature and pressure decentralized on-demand hydrogen production, small fuel cell hydrogen supply, and portable hydrogen energy devices.
[0009] To solve the above-mentioned technical problems, the technical solution adopted by the present invention is as follows: A method for preparing porous magnesium-based hydrogen production materials based on gradient sintering includes the following steps: Step 1: Place magnesium powder and nickel powder and / or copper powder and / or cobalt powder in a ball mill jar in a certain proportion, and continuously ball mill under argon protection to obtain a metal mixed powder, wherein the mass fraction of magnesium powder is 85%-95%, and the remainder is one or two or three of nickel powder, copper powder and cobalt powder in any proportion. Step 2: After vacuum drying of the pore-forming agent, it is ball-milled with the above-mentioned metal mixed powder under argon protection for a short time. The mass fraction of the pore-forming agent is 3%-10% (that is, the mass fraction of the pore-forming agent is 3%-10% of the mass of the above-mentioned metal mixed powder) to obtain mixed powder. Step 3: After pressing the above mixed powder into tablets, perform gradient sintering under argon protection in an atmosphere sintering furnace to obtain a porous magnesium-based material that can rapidly hydrolyze to produce hydrogen, i.e., a porous magnesium-based hydrogen production material based on gradient sintering.
[0010] Preferably, in step one, the ball-to-powder ratio is 30:1-40:1, the high-energy ball milling speed is 1000-1200 rpm, and the continuous ball milling time is 3-5 hours. Through the strong mechanical force of high-energy ball milling, the magnesium-based powder grains are refined, breaking the agglomeration structure of high-melting-point nickel, copper, and cobalt metals, achieving uniform dispersion of the catalytic metal in the magnesium matrix, thus laying the foundation for low-temperature alloying.
[0011] Preferably, in step two, the pore-forming agent is either PMMA microspheres or ammonium bicarbonate powder, and the vacuum drying treatment temperature is 50-60°C for 2-3 hours. The short-time low-energy ball milling speed is 200-250 rpm, and the milling time is 50-70 minutes. Low-energy ball milling can achieve uniform doping of the pore-forming agent and metal mixed powder without damaging the structure of the metal powder and the pore-forming agent, ensuring the uniformity of pore formation in subsequent sintering.
[0012] Preferably, in step three, the mixed powder is compressed into tablets using a metal powder tablet press at a pressure of 25-30 MPa for 5 minutes. If the added pore-forming agent is PMMA microspheres, the sintering heating process is as follows: heating from room temperature to 380-400 °C at a rate of 2-5 °C / min and holding for 2 hours, then continuing to heat to 500-550 °C at a rate of 5-10 °C / min and holding for 2-3 hours. If the added pore-forming agent is ammonium bicarbonate powder, the sintering heating process is as follows: heating from room temperature to 80-100 °C at a rate of 2-5 °C / min and holding for 0.5 hours, then continuing to heat to 500-550 °C at a rate of 5-10 °C / min and holding for 2-3 hours. After cooling, a porous magnesium-based hydrogen production material (i.e., the porous magnesium-based hydrogen production material based on gradient sintering of the present invention) can be obtained. The gradient heating sintering process allows for the complete decomposition and removal of pore-forming agents in the low-temperature section, creating uniform and interconnected porous channels. In the high-temperature section, the low-melting-point magnesium and high-melting-point catalytic metals are fully alloyed, enhancing the material's structural stability and reactivity.
[0013] This invention provides a gradient-sintered porous magnesium-based hydrogen production material with a total hydrogen production of 153-198 mL / g within 20 minutes, 335-401 mL / g within 40 minutes, 469-524 mL / g within 60 minutes, 546-597 mL / g within 80 minutes, 602-655 mL / g within 100 minutes, and 644-691 mL / g within 120 minutes. This invention also provides applications of the above-mentioned gradient-sintered porous magnesium-based hydrogen production material in ambient temperature and pressure dispersed on-demand hydrogen production, small fuel cell hydrogen supply, and portable hydrogen energy devices (preferably outdoor power supplies, emergency backup power supplies, 0.5-2L portable hydrogen cylinders, etc.).
[0014] Compared with the prior art, the beneficial effects of the present invention are as follows: (1) This invention constructs a large number of interconnected multi-level porous structures inside magnesium-based materials by combining pore-forming agent doping with gradient sintering process, fundamentally solving the problem of water phase mass transfer in the hydrolysis process of traditional magnesium-based materials. The porous structure can provide sufficient permeation and diffusion channels for aqueous solution, greatly increasing the specific surface area of the material in contact with water, exposing more hydrolysis active sites, allowing the internal matrix of the material to fully participate in the hydrolysis reaction, and significantly improving the hydrogen production rate and material utilization efficiency.
[0015] (2) The porous network structure constructed in this invention can effectively solve the problem of deposition and passivation of magnesium hydroxide byproducts. During the hydrolysis reaction, the porous channels can realize the continuous flow of solution and rapid desorption of products, avoiding the accumulation of magnesium hydroxide on the material surface and in the pores to form a dense passivation layer, ensuring the continuous and stable hydrolysis reaction, effectively improving the actual hydrogen production and reaction sustainability of the material, and solving the core problem of easy termination of reaction in traditional magnesium-based materials.
[0016] (3) This invention employs a high-energy ball milling pre-dispersion combined with a segmented gradient sintering process to successfully achieve uniform alloying of low-melting-point magnesium with high-melting-point nickel, copper, and cobalt metals at a relatively low sintering temperature. High-energy ball milling refines the powders of each component in advance and eliminates component segregation. Gradient heating sintering avoids the problems of high-temperature oxidation and ablation of the magnesium matrix. At the same time, it achieves full composite alloying of dissimilar metals. The uniformly distributed catalytic metal can continuously activate the hydrolysis reaction, further improving the hydrogen production kinetics.
[0017] (4) The invention uses argon atmosphere protection throughout the process, which effectively avoids the oxidation and deactivation of magnesium-based materials during powder ball milling, pressing and sintering, and ensures the material reactivity. The overall preparation process is simple, the parameters are controllable and highly repeatable, the raw material cost is low, and there is no need for complex equipment and harsh reaction conditions. It is suitable for large-scale industrial production and has extremely high application value in the field of decentralized hydrogen production such as portable hydrogen energy and emergency hydrogen supply.
[0018] This invention discloses a porous magnesium-based hydrogen production material based on gradient sintering and its preparation method, belonging to the technical field of hydrogen production materials. The preparation method includes the following steps: Step 1, magnesium powder and nickel powder and / or copper powder and / or cobalt powder are placed in a ball mill jar in a certain proportion and continuously ball-milled at high energy under argon protection to obtain a metal mixed powder; Step 2, a pore-forming agent is vacuum dried and then ball-milled with the above metal mixed powder at a short time under argon protection; Step 3, the above mixed powder is pressed into sheets and then subjected to gradient sintering under argon protection in an atmosphere sintering furnace to obtain a porous magnesium-based material capable of rapid hydrolysis for hydrogen production. This invention features a simple preparation process, low energy consumption, and the ability to alloy high-melting-point metals with Mg at relatively low temperatures. The material is porous, exhibits high hydrogen production rate and conversion rate, and can be stably stored and transported, making it suitable for industrial production. Attached Figure Description
[0019] Figure 1 The SEM morphology of the porous magnesium-based hydrogen production material prepared in Example 1 of this invention is shown. Figure 2 The SEM morphology of the porous magnesium-based hydrogen production material prepared in Example 2 of this invention is shown. Figure 3 The SEM morphology of the porous magnesium-based hydrogen production material prepared in Example 3 of this invention is shown. Figure 4 SEM morphology of the magnesium-based hydrogen production material prepared in Comparative Example 1; Figure 5 SEM morphology of the magnesium-based hydrogen production material in Comparative Example 3; Figure 6 The image shows the SEM morphology of the magnesium-based hydrogen production material in Comparative Example 4. Detailed Implementation
[0020] The present invention will now be described in further detail with reference to the accompanying drawings and specific embodiments. The following embodiments are for illustrative purposes only and are not intended to limit the scope of the invention.
[0021] Example 1
[0022] A method for preparing porous magnesium-based hydrogen production materials based on gradient sintering includes the following steps: Weighed magnesium powder and copper powder (mass ratio 90:10) were placed in a stainless steel ball mill jar and ball-milled under argon protection. The ball-to-powder ratio was 30:1, the rotation speed was 1200 rpm, and the milling time was 4 hours to prepare a metal mixed powder. Then, ammonium bicarbonate powder was placed in a vacuum drying oven for vacuum drying at 50 °C for 2 hours. The treated ammonium bicarbonate powder was then ball-milled with the metal mixed powder for a short time at low energy. The ammonium bicarbonate powder mass fraction was 5%, the rotation speed was 200 rpm, and the milling time was 50 minutes under argon protection. Finally, the mixed powder was compressed into tablets using a metal powder tablet press at a pressure of 30 MPa for a holding time of 5 minutes. Finally, the compressed material was sintered in an atmosphere sintering furnace. The sintering heating process was as follows: first, the temperature was increased from room temperature to 100 °C at a rate of 5 °C / min, and held at 100 °C for 0.5 hours. Then, the temperature was increased to 550 °C at a rate of 10 °C / min, and held at 550 °C for 2 hours. After cooling, the porous magnesium-based hydrogen production material was obtained. The SEM morphology of the obtained porous magnesium-based hydrogen production material is shown in the figure. Figure 1 As shown in the figure, a large number of micron-sized pores can be seen, which can significantly accelerate the diffusion of aqueous solution into the interior of the material. Its hydrogen production performance is shown in Table 1.
[0023] Table 1 Hydrogen generation performance of the magnesium-based porous material prepared in Example 1
[0024] The gradient sintered porous magnesium-based hydrogen production material obtained in this embodiment can be applied in the fields of ambient temperature and pressure dispersed on-demand hydrogen production, small fuel cell hydrogen supply, and portable hydrogen energy devices (preferably outdoor power supplies, emergency backup power supplies, 0.5-2L portable hydrogen cylinders, etc.).
[0025] Example 2
[0026] A porous magnesium-based hydrogen production material based on gradient sintering and its preparation method include the following steps: Weighed magnesium powder and a copper-nickel-cobalt mixed powder (magnesium mass fraction 95%, copper powder to nickel powder to cobalt powder mass ratio 1:2:1) were placed in a stainless steel ball mill jar and subjected to high-energy ball milling under argon protection. The ball-to-powder ratio was 30:1, the rotation speed was 1000 rpm, and the milling time was 5 hours to prepare a metallic mixed powder. Ammonium bicarbonate powder was then placed in a vacuum drying oven for vacuum drying at 50 °C for 2 hours. The treated ammonium bicarbonate powder was then combined with the above metallic mixed powder for short-time low-energy ball milling at 200 rpm for 50 minutes under argon protection. Finally, the mixed powder was compressed into tablets using a metal powder tablet press at a pressure of 30 MPa for 5 minutes. Finally, the pressed sheets were sintered in an atmosphere sintering furnace. The sintering heating process was as follows: first, the temperature was increased from room temperature to 80 °C at a rate of 2 °C / min, and held at 80 °C for 0.5 hours. Then, the temperature was increased to 500 °C at a rate of 5 °C / min, and held at 500 °C for 3 hours. After cooling, the porous magnesium-based hydrogen production material was obtained. The SEM morphology of the obtained porous magnesium-based hydrogen production material is shown below. Figure 2 As shown in the figure, a large number of micron-sized pores can be seen, which can significantly accelerate the diffusion of aqueous solution into the interior of the material. Its hydrogen production performance is shown in Table 2.
[0027] Table 2 Hydrogen generation performance of the magnesium-based porous material prepared in Example 2
[0028] The gradient sintered porous magnesium-based hydrogen production material obtained in this embodiment can be applied in the fields of ambient temperature and pressure dispersed on-demand hydrogen production, small fuel cell hydrogen supply, and portable hydrogen energy devices (preferably outdoor power supplies, emergency backup power supplies, 0.5-2L portable hydrogen cylinders, etc.).
[0029] Example 3
[0030] A porous magnesium-based hydrogen production material based on gradient sintering and its preparation method include the following steps: Weighed magnesium powder and a copper-nickel-cobalt mixed powder (magnesium mass fraction 85%, copper powder to nickel powder to cobalt powder mass ratio 2:1:2) were placed in a stainless steel ball mill jar and subjected to high-energy ball milling under argon protection. The ball-to-powder ratio was 40:1, the rotation speed was 1200 rpm, and the ball milling time was 3 hours to prepare a metal mixed powder. PMMA microspheres were then placed in a vacuum drying oven for vacuum drying at 60 °C for 3 hours. The treated PMMA microspheres were then subjected to short-time low-energy ball milling with the aforementioned metal mixed powder. The PMMA microsphere mass fraction was 3%, the rotation speed was 250 rpm, and the ball milling time was 70 minutes under argon protection. Finally, the mixed powder was compressed into tablets using a metal powder tablet press at a pressure of 25 MPa for a holding time of 5 minutes. Finally, the compressed material was sintered in an atmosphere sintering furnace. The sintering temperature rise process was as follows: the temperature was increased from room temperature to 400 °C at a rate of 5 °C / min, and held at 400 °C for 2 hours. Then, the temperature was increased to 550 °C at a rate of 5 °C / min, and held at 550 °C for 2 hours. After cooling, a porous magnesium-based hydrogen production material was obtained. The SEM morphology of the obtained porous magnesium-based hydrogen production material is shown in the figure. Figure 3 As shown in the figure, a large number of micron-sized pores can be seen, which can significantly accelerate the diffusion of aqueous solution into the interior of the material. Its hydrogen production performance is shown in Table 3.
[0031] Table 3 Hydrogen generation performance of the magnesium-based porous material prepared in Example 3
[0032] The gradient sintered porous magnesium-based hydrogen production material obtained in this embodiment can be applied in the fields of ambient temperature and pressure dispersed on-demand hydrogen production, small fuel cell hydrogen supply, and portable hydrogen energy devices (preferably outdoor power supplies, emergency backup power supplies, 0.5-2L portable hydrogen cylinders, etc.).
[0033] Example 4
[0034] The only difference between this embodiment and embodiment 3 is that: The sintering heating process is as follows: the temperature is increased from room temperature to 380 °C at a rate of 2 °C / min, and held at 380 °C for 2 hours. Then, the temperature is increased to 500 °C at a rate of 10 °C / min, and held at 500 °C for 3 hours.
[0035] Comparative Example 1
[0036] The only difference between this comparative example and Example 1 is the absence of ammonium bicarbonate pore-forming agent; all other processing techniques and parameters are identical. The SEM morphology of the prepared magnesium-based hydrogen production material is as follows: Figure 4 As shown in Table 4, the material without added pore-forming agent is dense and compact, with no visible pores or other structures. Its hydrogen production performance is significantly lower than that of Example 1.
[0037] Table 4 Hydrogen generation performance of magnesium-based porous materials prepared in Comparative Example 1
[0038] Comparative Example 2 The only difference between this comparative example and Example 3 is that no copper, nickel, or cobalt powder was added; it was pure Mg powder. All other processing techniques and parameters were exactly the same. The prepared porous magnesium-based hydrogen production material hardly reacts with water, and the total hydrogen production within 120 minutes was only 8 mL / g.
[0039] Comparative Example 3 (both the heating rate and temperature during sintering were relatively low)
[0040] The only difference between this comparative example and Example 1 is that: The sintering heating process was as follows: first, the temperature was increased from room temperature to 70 °C at a rate of 1 °C / min, and held at 70 °C for 0.5 hours. Then, the temperature was increased to 450 °C at a rate of 4 °C / min, and held at 450 °C for 2 hours. The SEM morphology of the prepared magnesium-based hydrogen production material is shown below. Figure 5 As shown, the number of micron-sized pores is significantly less than in Examples 1-3. The sintering temperature is low, atomic activity is low, and diffusion ability is insufficient, making it impossible to achieve uniform alloying of magnesium with high-melting-point metal elements within the sintering time. Its hydrogen production performance is shown in Table 5, with a hydrogen production rate significantly lower than that of Examples 1-3.
[0041] Table 5 Hydrogen generation performance of magnesium-based materials prepared in Comparative Example 3
[0042] Comparative Example 4 (both the heating rate and temperature during sintering were too high) The only difference between this comparative example and Example 1 is that: The sintering heating process was as follows: first, the temperature was increased from room temperature to 120 °C at a rate of 10 °C / min, and held at 120 °C for 0.5 hours. Then, the temperature was increased to 600 °C at a rate of 12 °C / min, and held at 600 °C for 2 hours. The SEM morphology of the prepared magnesium-based hydrogen production material is shown below. Figure 6 As shown, the number of micron-sized pores in this comparative example is significantly less than in Examples 1-3. The sintering temperature in this example is too high; 600 °C is close to the melting point of Mg, causing rapid diffusion of Mg atoms and easily leading to over-burning defects. The resulting microstructure is relatively coarse, the material is generally dense, and the number of micron-sized pores is very small. Its hydrogen production performance is shown in Table 6, with a hydrogen production rate significantly lower than that of Examples 1-3.
[0043] Table 6 Hydrogen generation performance of magnesium-based materials prepared in Comparative Example 4
[0044] It should be understood that, in order to simplify this disclosure and aid in understanding one or more of the various aspects of the invention, features of the invention are sometimes grouped together in a single embodiment, figure, or description thereof in the above description of exemplary embodiments of the invention. However, this method of disclosure should not be interpreted as reflecting an intention that the claimed invention requires more features than expressly recited in each claim. Rather, as reflected in the claims, inventive aspects lie in fewer than all the features of the foregoingly disclosed embodiments. Therefore, the claims, following the detailed description, are hereby expressly incorporated into that detailed description, wherein each claim itself is a separate embodiment of the invention.
[0045] Although the invention has been described with reference to a limited number of embodiments, those skilled in the art will understand from the foregoing description that other embodiments are conceivable within the scope of the invention described herein. Furthermore, it should be noted that the language used in this specification has been chosen primarily for readability and instructional purposes, and not for the purpose of interpreting or limiting the subject matter of the invention. Therefore, many modifications and variations will be apparent to those skilled in the art without departing from the scope and spirit of the appended claims. The disclosure of the invention is illustrative and not restrictive, and the scope of the invention is defined by the appended claims.
[0046] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A method for preparing porous magnesium-based hydrogen production materials based on gradient sintering, characterized in that, Includes the following steps: Step 1: Place magnesium powder and nickel powder and / or copper powder and / or cobalt powder in a ball mill jar in a certain proportion, and continuously ball mill under argon protection to obtain a metal mixed powder, wherein the mass fraction of magnesium powder is 85%-95%, and the remainder is one or two or three of nickel powder, copper powder and cobalt powder in any proportion. Step 2: After vacuum drying of the pore-forming agent, it is mixed with the above-mentioned metal powder and subjected to short-time low-energy ball milling under argon protection. The mass fraction of the pore-forming agent is 3%-10%, and the mixed powder is obtained. Step 3: After pressing the above mixed powder into tablets, perform gradient sintering under argon protection in an atmosphere sintering furnace. After cooling, a porous magnesium-based hydrogen production material based on gradient sintering is obtained.
2. The preparation method according to claim 1, characterized in that, In step one, the high-energy ball milling process is as follows: the ball-to-material ratio is 30:1-40:1, the high-energy ball milling speed is 1000-1200 rpm, and the continuous ball milling time is 3-5 hours.
3. The preparation method according to claim 1, characterized in that, In step two, the pore-forming agent is either PMMA microspheres or ammonium bicarbonate powder.
4. The preparation method according to claim 1, characterized in that, In step two, the vacuum drying process is as follows: the vacuum drying temperature is 50-60°C, and the time is 2-3 hours.
5. The preparation method according to claim 1, characterized in that, In step two, the short-time low-energy ball milling process is as follows: the ball milling speed is 200-250 rpm, and the milling time is 50-70 minutes.
6. The preparation method according to claim 1, characterized in that, In step three, the tableting process is as follows: the mixed powder is compressed into tablets on a metal powder tablet press at a pressure of 25-30 MPa and a holding time of 5 minutes.
7. The preparation method according to claim 1, characterized in that, In step three, when the added pore-forming agent is PMMA microspheres, the sintering heating process is as follows: the temperature is increased from room temperature to 380-400 °C at a rate of 2-5 °C / min and held for 2 hours, and then the temperature is increased to 500-550 °C at a rate of 5-10 °C / min and held for 2-3 hours.
8. The preparation method according to claim 1, characterized in that, In step three, when the added pore-forming agent is ammonium bicarbonate powder, the sintering heating process is as follows: the temperature is increased from room temperature to 80-100 °C at a rate of 2-5 °C / min and held for 0.5 hours, and then the temperature is increased to 500-550 °C at a rate of 5-10 °C / min and held for 2-3 hours.
9. The porous magnesium-based hydrogen production material based on gradient sintering obtained by the preparation method according to any one of claims 1-8, characterized in that, The total hydrogen production was 153-198 mL / g within 20 min, 335-401 mL / g within 40 min, 469-524 mL / g within 60 min, 546-597 mL / g within 80 min, 602-655 mL / g within 100 min, and 644-691 mL / g within 120 min.
10. The application of the gradient sintering-based porous magnesium-based hydrogen production material according to claim 9 in ambient temperature and pressure dispersed on-demand hydrogen production, small fuel cell hydrogen supply, and portable hydrogen energy devices, characterized in that, On-demand hydrogen production, small fuel cell hydrogen supply, and portable hydrogen energy devices including outdoor power supplies, emergency backup power supplies, and 0.5-2L portable hydrogen cylinders.