A manual arc welding method for butt welding of high-strength weather-resistant bridge steel plates

By adopting CJ557NHQ ultra-low hydrogen weather-resistant alkaline welding rods and graded preheating processes, the problems of insufficient weather resistance and low-temperature toughness of Q420qENH steel plate welds were solved, achieving efficient welding of high-strength weather-resistant bridge steel plates, reducing cold cracks and welding defects, and making it suitable for construction in cold regions on bridge sites.

CN123103128APending Publication Date: 2026-11-17INNER MONGOLIA BAOTOU STEEL UNION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611410582.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-11
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing welding processes, Q420qENH steel plates have poor weather resistance, insufficient low-temperature toughness, high incidence of cold cracking, and many on-site welding defects. In particular, delayed cold cracking and welding defects are prone to occur in thick plates and low-temperature open-air conditions. There is a lack of complete processes suitable for manual arc welding.

Method used

The process employs CJ557NHQ ultra-low hydrogen weather-resistant alkaline welding electrodes, involving graded preheating, multi-layer multi-pass manual arc welding, timely hydrogen removal and slow cooling after welding, and aging non-destructive testing. Combined with welding material pretreatment, groove preparation and assembly, graded preheating, multi-layer multi-pass manual arc welding, timely hydrogen removal and slow cooling after welding, and aging non-destructive testing, the weather resistance and low-temperature toughness of the weld are matched with those of the base metal.

Benefits of technology

It improves the weather resistance matching between the weld and the base material, reduces the incidence of cold cracking, ensures the low-temperature impact performance of the weld and the safety of the structure, reduces on-site welding defects, and is suitable for welding high-strength weather-resistant steel plates on bridge sites.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123103128A_ABST
    Figure CN123103128A_ABST
Patent Text Reader

Abstract

This invention discloses a manual arc welding butt welding method for high-strength, weather-resistant bridge steel plates, belonging to the field of bridge steel structure welding technology. The method includes steps such as welding material pretreatment, bevel preparation and assembly, staged preheating, multi-layer, multi-pass manual arc welding, timely hydrogen removal and slow cooling after welding, and aging non-destructive testing. The purpose of this invention is to overcome the shortcomings of existing technologies, such as poor weld weather resistance, insufficient low-temperature toughness, high incidence of cold cracking, and numerous on-site welding defects. It provides a complete set of welding processes specifically for manual arc welding of Q420qENH steel plates with a thickness of 10–50 mm, taking into account corrosion resistance, low-temperature impact resistance, and crack resistance, and is suitable for open-air bridge construction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of bridge steel structure welding technology, and particularly relates to a manual electric arc welding butt welding method for high-strength weather-resistant bridge steel plates. Background Technology

[0002] Q420qENH is a Cu-Cr-Ni series high-strength weather-resistant bridge steel with high sensitivity to cold cracking. It requires stringent impact resistance at -40℃, and the atmospheric corrosion resistance of the weld and heat-affected zone must match that of the base metal. Existing welding processes have the following defects: ordinary low-hydrogen welding electrodes lack weather-resistant alloying elements; general-purpose weather-resistant welding electrodes have low weather resistance indices in the deposited metal; the corrosion potential of the weld and base metal is inconsistent, leading to preferential corrosion of the weld during service; conventional processes only set a single preheating temperature, lacking measures for graded preheating, interpass temperature control, and timely hydrogen removal after welding; thick plates and low-temperature outdoor conditions easily lead to delayed cold cracking, resulting in a large amount of weld rework; welding uses wide-pass, high-heat-intensity welding, resulting in coarse grains in the heat-affected zone and needle-like iron in the weld. The low proportion of raw material makes it difficult to consistently meet the low-temperature impact resistance of the joint at -40℃; the lack of a standardized electrode drying and timely use control system makes the root pass weld prone to porosity and lack of fusion defects in high humidity and windy environments; the absence of a mandatory grinding and carburizing layer process after double-sided welding root cleaning makes the fusion line prone to microcracks; existing related patents are mostly for submerged arc welding and gas shielded welding, and no complete set of coupled processes adapted to pure manual arc welding on construction sites has been disclosed, and there is a lack of a complete technical solution for special flaw detection to investigate delayed cracks after 48 hours of aging. Summary of the Invention

[0003] To overcome the shortcomings of existing technologies, such as poor weather resistance, insufficient low-temperature toughness, high incidence of cold cracking, and numerous on-site welding defects, this invention provides a complete set of welding processes specifically for manual arc welding of Q420qENH steel plates with a thickness of 10-50mm. This process takes into account corrosion resistance, low-temperature impact resistance, and crack prevention, and is suitable for open-air bridge construction.

[0004] To solve the above-mentioned technical problems, the present invention adopts the following technical solution:

[0005] This invention discloses a method for manual arc welding butt jointing of high-strength weather-resistant bridge steel plates, comprising the steps of welding material pretreatment, groove preparation and assembly, staged preheating, multi-layer and multi-pass manual arc welding, timely hydrogen removal and slow cooling after welding, and aging non-destructive testing; its features are as follows:

[0006] S1: Welding material pretreatment

[0007] CJ557NHQ ultra-low hydrogen weather-resistant alkaline welding rods are selected. The welding rods are dried at a constant temperature of 380-400℃ for 60 minutes, cooled to 150℃ in the furnace, and then transferred to the heat preservation cylinder. The heat preservation cylinder is kept at 100-120℃ with electricity for heat preservation. No more than 3 welding rods are used at a time on site. The welding rods are not removed from the heat preservation cylinder for more than 4 hours. Welding rods that are not used within the time limit should be dried again. Wet welding rods are scrapped directly.

[0008] S2: Beveling preparation and assembly

[0009] For plates with a thickness t ≤ 20mm, a single-sided V-shaped bevel is used with a bevel angle of 60°, a blunt edge of 2mm, and an assembly gap of 2-3mm; for plates with a thickness t > 20mm, a double-sided X-shaped bevel is used with a bevel angle of 60° on both sides, a blunt edge of 2mm, and an assembly gap of 2-4mm; the bevel is preferably machined, and the surface hardened layer needs to be removed by grinding for plasma-cut bevels.

[0010] For tack welding, use CJ557NHQ welding rods, with a weld leg height ≥6mm, a single weld length ≥50mm, and a weld spacing of 200~300mm. Tack welds with porosity or cracks should be ground off and re-welded.

[0011] S3: Staged preheating

[0012] Preheating temperatures are set according to plate thickness and ambient temperature: 80℃ when plate thickness t≤12mm or ambient temperature ≥10℃; 100~120℃ when plate thickness t<t≤25mm or ambient temperature 0~10℃; and 130~150℃ when plate thickness t>25mm or ambient temperature <0℃ and for high-restraint joints.

[0013] The heating width on both sides of the weld is ≥1.5 times the plate thickness and ≥100mm, and the temperature measuring point is set on the back of the base material 75mm outside the weld.

[0014] Construction environment restrictions: Welding is prohibited in environments with wind speed > 8m / s, relative humidity > 80%, and rain or snow without protection.

[0015] S4: Multi-layer, multi-pass manual arc welding

[0016] Short arc operation and segmented stepwise symmetrical welding are adopted. The interpass temperature is controlled between 80 and 180℃ throughout the process. If the interpass temperature is higher than 180℃, it should be naturally cooled to within the limit before continuing welding. If welding is stopped midway, the temperature should be restored to the lower limit of the preheating temperature before re-welding.

[0017] For the root pass welding, use Ф3.2 welding rods, welding current 115~135A, arc voltage 22~25V, line energy ≤20kJ / cm, and small oscillation to ensure full penetration of the root;

[0018] For filler welding, use Ф4.0 welding rods, welding current 165~195A, arc voltage 25~27V, line energy ≤25kJ / cm, single weld width ≤12mm, and single weld thickness 3~5mm;

[0019] For cover welding, use Ф4.0 welding rods, welding current 155~175A, arc voltage 24~26V, line energy ≤22kJ / cm, and fill the arc crater when extinguishing the arc.

[0020] Double-sided X-shaped bevel, reverse side carbon arc gouging for root cleaning, after root cleaning, grinding to remove the carburized and hardened layer, then sealing the bottom weld;

[0021] S5: Promptly remove hydrogen and slow cool after welding.

[0022] Within 5 minutes after welding, start hydrogen removal heat treatment at a temperature of 285–325°C. The heat preservation time is calculated as 0.5 hours for every 25 mm of plate thickness, with a total heat preservation time of no less than 1 hour. If the ambient temperature is below 0°C or the plate thickness is greater than 30 mm, the heat preservation time is extended to 2 hours. The heating width is the same as the preheating width. After the heat preservation is completed, wrap the plate with asbestos cloth and slowly cool it to room temperature.

[0023] Furthermore, the CJ557NHQ welding electrode has the following properties for deposited metal: yield strength ReL≥460MPa, tensile strength Rm≥550MPa, low-temperature impact energy KV2≥60J at -40℃, weather resistance index≥6.5, and diffusible hydrogen in the deposited metal≤5mL / 100g.

[0024] Furthermore, grind the area ≥30mm on both sides of the bevel to a metallic luster, and remove rust, scale, oil, moisture and the original weather-resistant rust layer.

[0025] Furthermore, the misalignment at the butt joint shall not exceed 10% of the plate thickness and the maximum value shall not exceed 3mm.

[0026] Furthermore, assemble arc-starting and arc-extinguishing plates of the same material, with the arc-starting and arc-extinguishing plates having a size of not less than 100mm × 80mm.

[0027] Furthermore, all arc-starting operations must be completed within the arc-starting plate; arcing on the surface of the beveled base material is prohibited.

[0028] Furthermore, the time-sensitive non-destructive testing specifically includes:

[0029] After welding, the weld was left to stand for 48 hours, and then visual inspection, ultrasonic UT flaw detection, and magnetic particle MT flaw detection were carried out in sequence. The weld was free of undercut, porosity, slag inclusion, and cracks, with a weld reinforcement of 0-3mm and a smooth transition between the weld and the base metal.

[0030] Compared with the prior art, the beneficial technical effects of the present invention are as follows:

[0031] Excellent weather resistance matching: Specialized weather-resistant ultra-low hydrogen welding electrodes ensure that the Cu, Cr, and Ni weather-resistant alloying elements in the weld are matched with the base metal, resulting in uniform atmospheric corrosion resistance across the joint and preventing preferential weld corrosion. Suitable for long-term service weather-resistant steel bridges; significant cold crack suppression: The synergistic effect of staged preheating, precise interpass temperature control, and timely post-weld hydrogen removal accelerates the escape of diffused hydrogen, significantly reducing the incidence of delayed cracks in thick plates and low-temperature outdoor conditions, minimizing weld repairs; stable low-temperature impact performance: The narrow-channel, multi-layer, low-heat-input welding process minimizes the heat-affected zone and fine... The improved grain size and increased proportion of acicular ferrite in the weld seam ensure stable low-temperature impact resistance of the weld seam, fusion line, and heat-affected zone at -40℃, meeting the required specifications. It is suitable for bridges in cold regions. It has strong adaptability to on-site construction, with standardized processes for complete electrode aging control, environmental condition thresholds, and root cleaning and carburizing layer grinding, reducing human defects in manual welding. It does not require large-scale automated equipment and is suitable for on-site steel plate splicing on bridge construction sites. It has a high degree of structural safety assurance, with joint non-destructive testing conducted after 48 hours of post-weld aging to accurately detect delayed cold cracks in high-strength steel and improve the long-term service reliability of steel structures. Attached Figure Description

[0032] The present invention will be further described below with reference to the accompanying drawings.

[0033] Figure 1 This is a schematic diagram of the welding V-groove in Embodiment 1 of the present invention;

[0034] Figure 2 This is a schematic diagram of welding an X-shaped bevel in Embodiment 2 of the present invention. Detailed Implementation

[0035] The present invention will be further described in detail below with reference to specific embodiments. The embodiments are merely descriptions of the best implementation of the present invention and do not limit the scope of the present invention in any way.

[0036] Example 1

[0037] The base material is a 12mm thick Q420qENH steel plate, with an ambient temperature of 17℃ and a single-sided V-groove.

[0038] Welding electrode CJ557NHQ, dried at 395℃ for 1 hour, stored in an insulated container at 112℃, 2 electrodes per batch, to be used within 3.5 hours;

[0039] Preheating temperature 80℃, heating width on both sides 110mm;

[0040] The root pass uses Ф3.2 welding rods with a current of 125A; the fill and cover passes use Ф4.0 welding rods with a fill current of 170A and a cover current of 165A; the interpass temperature is controlled at 110~150℃.

[0041] After welding, heat to 310℃ for 3 minutes to eliminate hydrogen and hold for 1 hour, then cool slowly with asbestos cloth.

[0042] UT and MT flaw detection were carried out 48 hours after welding. The average impact energy of the joint at -40℃ was 75J, and there were no cracks or corrosion risks.

[0043] Example 2

[0044] The base material is a 30mm thick Q420qENH steel plate, with an ambient temperature of -6℃ and a double-sided X-shaped bevel.

[0045] Welding electrode CJ557NHQ, dry at 390℃ for 1 hour, store in an insulated container at 120℃, take 3 electrodes at a time, and store for no more than 3 hours;

[0046] Preheating temperature 142℃, heating width on both sides 180mm;

[0047] The root pass uses Ф3.2 welding rods with a current of 130A; the fill and cover passes use Ф4.0 welding rods with a fill current of 176A and a cover current of 160A; the interpass temperature is controlled at 120~160℃.

[0048] After cleaning the root with carbon planer and grinding the carburized layer on the reverse side, seal the bottom.

[0049] Start hydrogen elimination 4 minutes after welding, hold at 300℃ for 2 hours, and then slowly cool to room temperature;

[0050] No delayed cracks were found during 48-hour flaw detection, and the weather resistance index of the joint was basically consistent with that of the base material.

[0051] The embodiments described above are merely preferred embodiments of the present invention and are not intended to limit the scope of the present invention. Various modifications and improvements made by those skilled in the art to the technical solutions of the present invention without departing from the spirit of the present invention should fall within the protection scope defined by the claims of the present invention.

Claims

1. A method for butt welding high-strength weather-resistant bridge steel plates using manual electric arc welding, comprising the steps of welding material pretreatment, groove preparation and assembly, staged preheating, multi-layer and multi-pass manual electric arc welding, timely hydrogen removal and slow cooling after welding, and aging non-destructive testing; characterized in that, Specifically as follows: S1: Welding material pretreatment CJ557NHQ ultra-low hydrogen weather-resistant alkaline welding rods are selected. The welding rods are dried at a constant temperature of 380-400℃ for 60 minutes, cooled to 150℃ in the furnace, and then transferred to the heat preservation cylinder. The heat preservation cylinder is kept at 100-120℃ with electricity for heat preservation. No more than 3 welding rods are used at a time on site. The welding rods are not removed from the heat preservation cylinder for more than 4 hours. Welding rods that are not used within the time limit should be dried again. Wet welding rods are scrapped directly. S2: Beveling preparation and assembly For plates with a thickness t ≤ 20mm, a single-sided V-shaped bevel is used with a bevel angle of 60°, a blunt edge of 2mm, and an assembly gap of 2-3mm; for plates with a thickness t > 20mm, a double-sided X-shaped bevel is used with a bevel angle of 60° on both sides, a blunt edge of 2mm, and an assembly gap of 2-4mm; the bevel is preferably machined, and the surface hardened layer needs to be removed by grinding for plasma-cut bevels. For tack welding, use CJ557NHQ welding rods, with a weld leg height ≥6mm, a single weld length ≥50mm, and a weld spacing of 200~300mm. All tack welds with porosity or cracks should be ground off and re-welded. S3: Staged preheating Preheating temperatures are set according to plate thickness and ambient temperature: 80℃ when plate thickness t≤12mm or ambient temperature≥10℃; 100~120℃ when plate thickness t<t≤25mm or ambient temperature 0~10℃; and 130~150℃ when plate thickness t>25mm or ambient temperature<0℃ and for high-restraint joints. The heating width on both sides of the weld is ≥1.5 times the plate thickness and ≥100mm, and the temperature measuring point is set on the back of the base material 75mm outside the weld. Construction environment restrictions: Welding is prohibited in environments with wind speed > 8m / s, relative humidity > 80%, and rain or snow without protective measures. S4: Multi-layer, multi-pass manual arc welding Short arc operation and segmented stepwise symmetrical welding are adopted. The interpass temperature is controlled between 80 and 180℃ throughout the process. If the interpass temperature is higher than 180℃, it is allowed to cool naturally to within the limit before continuing welding. If welding is stopped midway, the temperature is restored to the lower limit of the preheating temperature before re-welding. For the root pass welding, use Ф3.2 welding rods, welding current 115~135A, arc voltage 22~25V, line energy ≤20kJ / cm, and small oscillation to ensure full penetration of the root; For filler welding, use Ф4.0 welding rods, welding current 165~195A, arc voltage 25~27V, line energy ≤25kJ / cm, single weld width ≤12mm, and single weld thickness 3~5mm; For cover welding, use Ф4.0 welding rods, welding current 155~175A, arc voltage 24~26V, line energy ≤22kJ / cm, and fill the arc crater when extinguishing the arc. Double-sided X-shaped bevel, reverse side carbon arc gouging for root cleaning, after root cleaning, grinding to remove the carburized and hardened layer and then sealing the bottom weld; S5: Promptly remove hydrogen and slow cool after welding. Within 5 minutes after welding, start hydrogen removal heat treatment at a temperature of 285–325°C. The heat preservation time is calculated as 0.5 hours for every 25 mm of plate thickness, with a total heat preservation time of no less than 1 hour. If the ambient temperature is below 0°C or the plate thickness is greater than 30 mm, the heat preservation time is extended to 2 hours. The heating width is the same as the preheating width. After the heat preservation is completed, wrap the plate with asbestos cloth and slowly cool it to room temperature.

2. The method for manual arc welding butt joint of high-strength weather-resistant bridge steel plates according to claim 1, characterized in that, The CJ557NHQ welding electrode has the following properties for deposited metal: yield strength ReL≥460MPa, tensile strength Rm≥550MPa, low-temperature impact energy KV2≥60J at -40℃, weather resistance index≥6.5, and diffusible hydrogen in the deposited metal≤5mL / 100g.

3. The manual arc welding butt welding method for high-strength weather-resistant bridge steel plates according to claim 1, characterized in that, Grind the area ≥30mm on both sides of the bevel to a metallic luster, and remove rust, scale, oil, moisture and the original weather-resistant rust layer.

4. The method for manual arc welding butt joint of high-strength weather-resistant bridge steel plates according to claim 1, characterized in that, The misalignment at the butt joint shall not exceed 10% of the plate thickness and the maximum value shall not exceed 3mm.

5. The manual arc welding butt welding method for high-strength weather-resistant bridge steel plates according to claim 1, characterized in that, Equip with Q420qENH arc-starting and arc-extinguishing plates of the same material, with the arc-starting and arc-extinguishing plates having a size of not less than 100mm × 80mm.

6. The method for manual arc welding butt joint of high-strength weather-resistant bridge steel plates according to claim 1, characterized in that, All arc-starting operations must be completed within the arc-starting plate; arcing on the surface of the beveled base material is prohibited.

7. The manual arc welding butt welding method for high-strength weather-resistant bridge steel plates according to claim 1, characterized in that, The time-sensitive non-destructive testing specifically refers to: After welding, the weld was left to stand for 48 hours, and then visual inspection, ultrasonic UT flaw detection, and magnetic particle MT flaw detection were carried out in sequence. The weld was free of undercut, porosity, slag inclusion, and cracks, with a weld reinforcement of 0-3mm and a smooth transition between the weld and the base metal.