Welding apparatus and method for negative electrode current collector and housing

By using a laser beam oscillation welding method and controlling the laser's operating parameters, a high-quality, high-reliability, and high-efficiency connection between copper and steel casing in the 46 series large cylindrical batteries was achieved. This solved the problems of insufficient welding strength and poor consistency, and improved the reliability and safety of the batteries.

CN123103181APending Publication Date: 2026-11-17HEFEI GUOXUAN HIGH TECH POWER ENERGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611342054.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-01
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing welding methods are insufficient to achieve high-quality, high-reliability, and high-efficiency connections between copper and steel casings in 46-series large cylindrical batteries, resulting in problems such as insufficient weld strength, poor consistency, or low efficiency.

Method used

The laser beam oscillating welding method is used to achieve a high-quality connection between the negative electrode current collector and the shell by controlling the working parameters of the laser, suppressing the formation of brittle intermetallic compounds, and forming a dense, crack-free, and pore-free weld nugget.

Benefits of technology

It achieves a high-quality, high-reliability, and high-efficiency connection between the negative electrode current collector and the casing, with low fusion resistance and high pull-out strength, avoiding additional material costs and improving the long-term reliability and safety of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123103181A_ABST
    Figure CN123103181A_ABST
Patent Text Reader

Abstract

This invention discloses a welding apparatus and method for a negative current collector and a housing. The welding method includes pushing the negative current collector into the interior of the housing, so that the surface of the negative current collector to be welded is tightly fitted with the inner wall of the housing, forming an lap structure; employing a laser beam oscillating welding method, controlling the laser to align with the lap structure from the outside according to preset operating parameters for welding. During the laser welding process, part of the laser energy generated by the laser acts on the housing and part acts on the negative current collector, forming a weld nugget, thus completing the welding of the negative current collector and the housing. This invention can achieve a high-quality, high-reliability, and high-efficiency connection between the negative current collector and the housing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of power battery manufacturing technology, specifically relating to a welding device and method for a negative electrode current collector and a housing. Background Technology

[0002] With the development of electric vehicles and large-scale energy storage systems, higher demands are being placed on the energy density, power density, and safety of lithium-ion batteries. Large cylindrical batteries (e.g., 46mm in diameter) have become a current research hotspot due to their excellent structural stability and high energy density. In the battery manufacturing process, a reliable connection between the negative electrode current collector (usually copper or nickel-plated copper) and the steel casing (usually nickel-plated steel) is crucial. This connection is responsible for effectively discharging the current generated inside the battery to the external circuit. However, because copper and steel are two metals with vastly different physicochemical properties, there are many welding challenges between them.

[0003] 1. Poor metallurgical compatibility: Copper and iron have low miscibility and easily form brittle intermetallic compounds, resulting in high brittleness and poor conductivity of the solder joint.

[0004] 2. Significant differences in thermophysical properties: Copper's thermal conductivity and melting point differ significantly from steel, making it difficult to distribute heat evenly during laser welding. This can easily lead to the copper not melting completely while the steel shell is overheated and broken down.

[0005] 3. High weld quality requirements: For the 46 series large cylindrical batteries, the internal current is large, requiring the welded joint to have extremely low contact resistance and extremely high mechanical strength. Any poor weld, sparking, or cracks may cause the battery's internal resistance to increase, overheating, or even failure.

[0006] 4. Space constraints: The compact internal space of large cylindrical batteries poses challenges to the precision and accessibility of welding equipment.

[0007] Existing welding methods (such as ultrasonic welding and resistance welding) often suffer from problems such as insufficient weld strength, poor consistency, or low efficiency when applied to welding dissimilar materials like those used in 46-series batteries. Therefore, there is an urgent need for a welding method that can achieve high-quality, high-reliability, and high-efficiency connections. Summary of the Invention

[0008] To address the aforementioned problems, this invention proposes a welding device and method for connecting the negative current collector to the housing, which can achieve a high-quality, high-reliability, and high-efficiency connection between the negative current collector and the housing.

[0009] To achieve the above-mentioned technical objectives and effects, the present invention is implemented through the following technical solution:

[0010] In a first aspect, the present invention provides a welding device for a negative electrode current collector and a housing, comprising:

[0011] A clamping block is configured to push the negative electrode current collector into the interior of the housing, so that the surface of the negative electrode current collector to be welded is interference-fitted with the inner wall of the housing, and forms an overlapping structure.

[0012] Laser;

[0013] The controller, connected to the laser, is configured to use a laser beam oscillating welding method to control the laser to align with the overlapping structure from the outside according to preset working parameters. During the laser welding process, part of the laser energy generated by the laser acts on the shell and part acts on the negative electrode current collector to form a molten nugget, thus completing the welding of the negative electrode current collector to the shell.

[0014] In the above scheme, by controlling the laser's operating parameters and employing a laser beam oscillating welding method, the formation of brittle intermetallic compounds during the welding of the negative electrode current collector to the shell is effectively suppressed, resulting in a dense, crack-free, and porosity-free weld nugget (i.e., weld structure). The weld nugget has low resistance (<10μΩ) and high pull-out strength (>150MPa), enabling a high-quality, high-reliability, and high-efficiency connection between the negative electrode current collector and the shell. Furthermore, compared to methods requiring the addition of an intermediate layer material, this invention directly utilizes existing materials for welding, eliminating the need for additional material costs, simplifying the process, and reducing overall cost.

[0015] In conjunction with the first aspect, optionally, the preset operating parameters include:

[0016] Laser wavelength, wherein the laser wavelength is an infrared laser;

[0017] Laser power, wherein the value of the laser power is in the range of 600W~800W;

[0018] The oscillation frequency, wherein the value of the oscillation frequency is in the range of 100Hz-1000Hz;

[0019] The swing amplitude, wherein the value of the swing amplitude ranges from 0.2 mm to 1.0 mm;

[0020] The moving speed is in the range of 120 mm / s to 150 mm / s;

[0021] Defocusing amount, the value of which ranges from +1mm to +3mm;

[0022] A protective gas, wherein the protective gas is nitrogen with a purity ≥ 99.999%;

[0023] Gas flow rate, wherein the gas flow rate ranges from 10L / min to 25L / min.

[0024] The above scheme has specifically designed the operating parameters of the laser, which can effectively suppress the formation of brittle intermetallic compounds when the negative electrode current collector is welded to the shell.

[0025] In conjunction with the first aspect, optionally, the oscillation trajectory of the laser beam generated by the laser is circular or figure-eight shaped.

[0026] In the above scheme, by designing the oscillation trajectory of the laser beam as a circle or figure-eight shape, combined with an oscillation frequency of 100Hz-1000Hz and an oscillation amplitude of 0.2 mm-1.0 mm, the molten pool can be stirred, making the copper and steel elements in the negative electrode current collector and the shell more uniformly distributed, breaking the continuous network structure of the brittle phase, refining the grains, and thus improving the toughness and strength of the weld.

[0027] In conjunction with the first aspect, optionally, the negative electrode current collector is made of copper or copper alloy with a thickness of 0.3mm-1.0mm; the shell is a nickel-plated steel shell with a nickel plating layer thickness of 2μm-10μm and a shell wall thickness of 0.25mm-0.6mm.

[0028] The above scheme specifies the materials for the negative electrode current collector and the housing to ensure the successful implementation of the welding method.

[0029] In conjunction with the first aspect, optionally, after welding, the thickness of the laser beam penetrating the shell is 60%-90% of the shell thickness, and the thickness of the laser beam penetrating the negative current collector is 20%-50% of the negative current collector thickness.

[0030] Based on the above solution, it not only ensures a sufficient metallurgical bond between the negative current collector and the casing, but also avoids the risk of battery leakage caused by welding through the casing, thus greatly improving the long-term reliability and safety of the battery.

[0031] In conjunction with the first aspect, optionally, the effective width of the melt core is greater than or equal to 527 μm.

[0032] Compared with the effective width of the melt core in the prior art, the effective width of the melt core in the above scheme is significantly higher and the quality is better.

[0033] In conjunction with the first aspect, optionally, the angle between the incident direction of the laser beam generated by the laser and the axial direction of the housing is an obtuse angle.

[0034] In the above scheme, by setting the angle between the incident direction of the laser beam generated by the laser and the axial direction of the shell to an obtuse angle, it can be ensured that the welding process will not affect the lap joint structure.

[0035] Secondly, the present invention provides a method for welding a negative current collector to a housing, comprising:

[0036] The negative electrode current collector is pushed into the interior of the housing, so that the surface of the negative electrode current collector to be welded is interference-fitted with the inner wall of the housing, and an overlapping structure is formed.

[0037] The laser beam oscillating welding method is adopted. The laser is controlled to align with the overlapping structure from the outside according to the preset working parameters. During the laser welding process, part of the laser energy generated by the laser acts on the shell and part acts on the negative electrode current collector to form a molten nugget, thus completing the welding of the negative electrode current collector and the shell.

[0038] In the above scheme, by controlling the laser's operating parameters and employing a laser beam oscillating welding method, the formation of brittle intermetallic compounds during the welding of the negative electrode current collector to the shell is effectively suppressed, resulting in a dense, crack-free, and porosity-free weld nugget (i.e., weld structure). The weld nugget has low resistance (<10μΩ) and high pull-out strength (>150MPa), enabling a high-quality, high-reliability, and high-efficiency connection between the negative electrode current collector and the shell. Furthermore, compared to methods requiring the addition of an intermediate layer material, this invention directly utilizes existing materials for welding, eliminating the need for additional material costs, simplifying the process, and reducing overall cost.

[0039] In conjunction with the second aspect, optionally, before pushing the negative current collector into the interior of the housing, the surfaces of the negative current collector to be soldered and the surfaces of the housing to be soldered are cleaned to remove oil and oxides.

[0040] In the above solution, the cleaning process enables efficient laser beam penetration, ensuring welding results.

[0041] In conjunction with the second aspect, optionally, during the welding process, the drive housing rotates the negative electrode current collector while the laser remains stationary.

[0042] The above scheme provides the relative motion relationship between the laser, the housing, and the negative electrode current collector during the welding process to ensure that the laser can complete the welding of the entire circumference.

[0043] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0044] In the above scheme, by controlling the working parameters of the laser and using the laser beam oscillating welding method, the formation of brittle intermetallic compounds during the welding of the negative electrode current collector and the shell is effectively suppressed, resulting in a dense, crack-free, and pore-free weld nugget (i.e., weld structure). The weld nugget has low resistance (<10μΩ) and high pull-out strength (>150MPa), which enables a high-quality, high-reliability, and high-efficiency connection between the negative electrode current collector and the shell. Attached Figure Description

[0045] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the embodiments will be briefly described below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort, wherein:

[0046] Figure 1 This is a schematic flowchart illustrating a welding method between the negative electrode current collector and the housing according to an embodiment of the present invention.

[0047] Figure 2 This is a schematic diagram illustrating the working principle of a welding device for the negative electrode current collector and the housing according to an embodiment of the present invention.

[0048] Figure 3 This is a schematic diagram of the assembly of the clamping block, the housing, and the negative electrode current collector according to one embodiment of the present invention;

[0049] Figure 4 This is one of the assembly diagrams of the clamping block, housing, negative current collector, and battery cell according to one embodiment of the present invention;

[0050] Figure 5 This is a second schematic diagram of the assembly of the clamping block, housing, negative current collector, and battery cell according to one embodiment of the present invention;

[0051] Figure 6 This is a schematic diagram of the parameters of the weld nugget generated based on the welding method of the present invention;

[0052] Figure 7 A schematic diagram of the parameters of the weld nugget generated by the welding method in the prior art;

[0053] In the picture:

[0054] 1-Laser incident direction, 2-Battery cell, 3-Housing, 4-Negative current collector, 5-Clamping block. Detailed Implementation

[0055] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. The following description of at least one exemplary embodiment is merely illustrative and is in no way intended to limit the present invention or its application or use. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0056] Unless otherwise specifically stated, the relative arrangement, numerical expressions, and values ​​of the components and steps set forth in these embodiments do not limit the scope of the invention. It should also be understood that, for ease of description, the dimensions of the various parts shown in the drawings are not drawn to actual scale. Techniques, methods, and devices known to those skilled in the art may not be discussed in detail, but where appropriate, such techniques, methods, and devices should be considered part of the specification. In all examples shown and discussed herein, any specific values ​​should be interpreted as merely exemplary and not as limitations. Therefore, other examples of exemplary embodiments may include different values. It should be noted that similar reference numerals and letters in the following figures denote similar items; therefore, once an item is defined in one figure, it need not be further discussed in subsequent figures.

[0057] In the description of this invention, "several" means one or more, "multiple" means two or more, "greater than," "less than," and "exceeding" are understood to exclude the stated number, while "above," "below," and "within" are understood to include the stated number. The use of "first" and "second" in the description is merely for distinguishing technical features and should not be construed as indicating or implying relative importance, or implicitly indicating the number of indicated technical features, or implicitly indicating the order of the indicated technical features.

[0058] In the description of this invention, the terms "one embodiment," "some embodiments," "illustrative embodiment," "example," "specific example," or "some examples," etc., refer to specific features, structures, materials, or characteristics described in connection with that embodiment or example, which are included in at least one embodiment or example of the invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.

[0059] The application principle of the present invention will be described in detail below with reference to the accompanying drawings.

[0060] Example 1

[0061] This invention provides a welding device for a negative electrode current collector and a housing, comprising:

[0062] The clamping block 5 is configured to push the negative electrode current collector 4 into the interior of the housing 3, so that the surface of the negative electrode current collector 4 to be welded is interference-fitted with the inner wall of the housing 3, and forms an overlapping structure.

[0063] Laser;

[0064] The controller, connected to the laser, is configured to use a laser beam oscillating welding method to control the laser to align with the overlapping structure from the outside according to preset working parameters for welding. During the laser welding process, part of the laser energy generated by the laser acts on the housing 3 and part acts on the negative electrode current collector 4 to form a molten nucleus, thus completing the welding of the negative electrode current collector 4 and the housing 3.

[0065] In the above scheme, by controlling the operating parameters of the laser and employing a laser beam oscillating welding method, the formation of brittle intermetallic compounds during the welding of the negative electrode current collector 4 and the shell 3 is effectively suppressed, resulting in a dense, crack-free, and porosity-free weld nugget (i.e., weld structure). The weld nugget has low resistance (<10μΩ) and high pull-out strength (>150MPa), enabling a high-quality, high-reliability, and high-efficiency connection between the negative electrode current collector 4 and the shell 3. Furthermore, compared to methods that require the addition of an intermediate layer material, this invention directly utilizes existing materials for welding, eliminating the need for additional material costs, simplifying the process, and reducing overall cost.

[0066] In one specific embodiment of the present invention, the preset operating parameters include:

[0067] Laser wavelength, wherein the laser wavelength is an infrared laser;

[0068] Laser power, wherein the value of the laser power is in the range of 600W~800W;

[0069] The oscillation frequency, wherein the value of the oscillation frequency is in the range of 100Hz-1000Hz;

[0070] The swing amplitude, wherein the value of the swing amplitude ranges from 0.2 mm to 1.0 mm;

[0071] The moving speed is in the range of 120 mm / s to 150 mm / s;

[0072] Defocusing amount, the value of which ranges from +1mm to +3mm;

[0073] A protective gas, wherein the protective gas is nitrogen with a purity ≥ 99.999%;

[0074] Gas flow rate, wherein the gas flow rate ranges from 10L / min to 25L / min.

[0075] In the above scheme, the operating parameters of the laser are specifically designed, which can effectively suppress the formation of brittle intermetallic compounds when the negative electrode current collector 4 is welded to the shell 3.

[0076] In one specific embodiment of the present invention, the oscillation trajectory of the laser beam generated by the laser is circular or figure-eight shaped.

[0077] In the above scheme, by designing the oscillation trajectory of the laser beam as a circle or figure-eight shape, combined with an oscillation frequency of 100Hz-1000Hz and an oscillation amplitude of 0.2 mm-1.0 mm, the molten pool can be stirred, making the copper and steel elements of the negative electrode current collector 4 and the shell 3 more evenly distributed, breaking the continuous network structure of the brittle phase, refining the grains, and thus improving the toughness and strength of the weld.

[0078] In one specific embodiment of the present invention, the negative electrode current collector 4 is made of copper or copper alloy with a thickness of 0.3mm-1.0mm; the housing 3 is a nickel-plated steel shell with a nickel plating layer thickness of 2μm-10μm and a wall thickness of 0.25mm-0.6mm.

[0079] The above scheme specifies the materials for the negative electrode current collector 4 and the housing 3 to ensure the implementation of the welding method.

[0080] In one specific embodiment of the present invention, after welding is completed, the thickness of the laser beam penetrating the housing 3 is 60%-90% of the thickness of the housing 3, and the thickness of the laser beam penetrating the negative current collector is 20%-50% of the thickness of the negative current collector.

[0081] Based on the above solution, it not only ensures the full metallurgical bond between the negative current collector and the casing 3, but also avoids the risk of battery leakage caused by welding through the casing 3, which greatly improves the long-term reliability and safety of the battery.

[0082] In one specific embodiment of the present invention, such as Figure 6 As shown, the effective width of the melt core is greater than or equal to 527 μm.

[0083] and Figure 7 Compared to the effective width of the weld nugget (350μm) generated by existing technologies that do not employ beam oscillation welding, the effective width of the weld nugget in the above-mentioned scheme is significantly higher and of better quality.

[0084] In one specific embodiment of the present invention, such as Figure 2 As shown, the angle between the incident direction 1 of the laser beam generated by the laser and the axis of the housing 3 is an obtuse angle.

[0085] In the above scheme, by setting the angle between the incident direction 1 of the laser beam generated by the laser and the axis of the housing 3 to an obtuse angle, it can be ensured that the welding process will not affect the lap joint structure. In specific implementation, such as Figure 2 As shown, the obtuse angle is 130°.

[0086] Example 2

[0087] This invention provides a method for welding a negative electrode current collector to a housing, such as... Figure 1 As shown, it includes the following steps:

[0088] (1) Push the negative electrode current collector 4 into the interior of the housing 3 so that the surface of the negative electrode current collector 4 to be welded is interference fit with the inner wall of the housing 3 and forms an overlapping structure;

[0089] (2) Using the laser beam oscillating welding method, the laser is controlled to align the lap structure from the outside according to the preset working parameters for welding. During the laser welding process, part of the laser energy generated by the laser acts on the shell 3 and part acts on the negative electrode current collector 4 to form a molten nucleus and complete the welding of the negative electrode current collector 4 and the shell 3.

[0090] In the above scheme, by controlling the operating parameters of the laser and employing a laser beam oscillating welding method, the formation of brittle intermetallic compounds during the welding of the negative electrode current collector 4 and the shell 3 is effectively suppressed, resulting in a dense, crack-free, and porosity-free weld nugget (i.e., weld structure). The weld nugget has low resistance (<10μΩ) and high pull-out strength (>150MPa), enabling a high-quality, high-reliability, and high-efficiency connection between the negative electrode current collector 4 and the shell 3. Furthermore, compared to methods that require the addition of an intermediate layer material, this invention directly utilizes existing materials for welding, eliminating the need for additional material costs, simplifying the process, and reducing overall cost.

[0091] In one specific embodiment of the present invention, the preset operating parameters include:

[0092] Laser wavelength, wherein the laser wavelength is an infrared laser;

[0093] Laser power, wherein the value of the laser power is in the range of 600W~800W;

[0094] The oscillation frequency, wherein the value of the oscillation frequency is in the range of 100Hz-1000Hz;

[0095] The swing amplitude, wherein the value of the swing amplitude ranges from 0.2 mm to 1.0 mm;

[0096] The moving speed is in the range of 120 mm / s to 150 mm / s;

[0097] Defocusing amount, the value of which ranges from +1mm to +3mm;

[0098] A protective gas, wherein the protective gas is nitrogen with a purity ≥ 99.999%;

[0099] Gas flow rate, wherein the gas flow rate ranges from 10L / min to 25L / min.

[0100] In the above scheme, the operating parameters of the laser are specifically designed, which can effectively suppress the formation of brittle intermetallic compounds when the negative electrode current collector 4 is welded to the shell 3.

[0101] In one specific embodiment of the present invention, the oscillation trajectory of the laser beam generated by the laser is circular or figure-eight shaped.

[0102] In the above scheme, by designing the oscillation trajectory of the laser beam as a circle or figure-eight shape, combined with an oscillation frequency of 100Hz-1000Hz and an oscillation amplitude of 0.2 mm-1.0 mm, the molten pool can be stirred, making the copper and steel elements of the negative electrode current collector 4 and the shell 3 more evenly distributed, breaking the continuous network structure of the brittle phase, refining the grains, and thus improving the toughness and strength of the weld.

[0103] In one specific embodiment of the present invention, the negative electrode current collector 4 is made of copper or copper alloy with a thickness of 0.3mm-1.0mm; the housing 3 is a nickel-plated steel shell with a nickel plating layer thickness of 2μm-10μm and a wall thickness of 0.25mm-0.6mm.

[0104] The above scheme specifies the materials for the negative electrode current collector 4 and the housing 3 to ensure the implementation of the welding method.

[0105] In one specific embodiment of the present invention, after welding is completed, the thickness of the laser beam penetrating the housing 3 is 60%-90% of the thickness of the housing 3, and the thickness of the laser beam penetrating the negative current collector is 20%-50% of the thickness of the negative current collector.

[0106] Based on the above solution, it not only ensures the full metallurgical bond between the negative current collector and the casing 3, but also avoids the risk of battery leakage caused by welding through the casing 3, which greatly improves the long-term reliability and safety of the battery.

[0107] In one specific embodiment of the present invention, such as Figure 6 As shown, the effective width of the melt core is greater than or equal to 527 μm.

[0108] and Figure 7 Compared to the effective width of the weld nugget (350μm) generated by existing technologies that do not employ beam oscillation welding, the effective width of the weld nugget in the above-mentioned scheme is significantly higher and of better quality.

[0109] In one specific embodiment of the present invention, during the welding process, the drive housing 3 drives the negative electrode current collector 4 to rotate, while the laser remains stationary.

[0110] The above scheme provides the relative motion relationship between the laser, the housing 3, and the negative electrode current collector 4 during the welding process to ensure that the laser can complete the welding of the entire circumference.

[0111] In one specific embodiment of the present invention, such as Figure 2 As shown, the angle between the incident direction 1 of the laser beam generated by the laser and the axis of the housing 3 is an obtuse angle.

[0112] In the above scheme, by setting the angle between the incident direction 1 of the laser beam generated by the laser and the axis of the housing 3 to an obtuse angle, it can be ensured that the welding process will not affect the lap joint structure. In specific implementation, such as Figure 2 As shown, the obtuse angle is 130°.

[0113] In one specific embodiment of the present invention, before placing the negative electrode current collector 4 inside the housing 3, the surfaces of the negative electrode current collector 4 to be soldered and the surfaces of the housing 3 to be soldered are cleaned to remove oil and oxides.

[0114] In the above solution, the cleaning process enables efficient laser beam penetration, ensuring welding results.

[0115] The welding method between the negative current collector 4 and the housing 3 in this embodiment of the invention will be described in detail below with reference to a specific implementation method.

[0116] Taking a large cylindrical battery with a diameter of 46mm and a height of 80mm as an example. The negative electrode current collector 4 is made of 0.5mm thick copper; the casing 3 is made of nickel-plated steel with a wall thickness of 0.4mm and a nickel plating layer of 5μm; the welding method includes the following steps:

[0117] S1 Preprocessing:

[0118] The areas of the copper manifold and nickel-plated steel shell to be soldered were ultrasonically cleaned and dried using alcohol and acetone.

[0119] S2 Positioning and Assembly:

[0120] The copper current collector is precisely placed at the bottom center of the nickel-plated steel shell. A pressure of 0.5 MPa is applied using the clamping block 5 to ensure a tight fit (i.e., interference fit) and form an overlapping structure. The copper current collector is in contact with the battery cell 2. See details... Figures 3-5 .

[0121] More specifically, the diameter of the copper current collector is 45.2±0.1 mm, and the inner diameter of the housing 3 is 45.2±0.1 mm. The copper current collector and the housing 3 are interference fit. The edge of the clamping block 5 is chamfered to avoid interference from the incident direction of the laser beam. The edge thickness of the clamping block 5 is 0.4 mm, which ensures that the clamping block 5 can effectively press each weld seam and also ensures that the laser incident will not interfere. This ensures that the 6 welding lines of the negative current collector 4 cannot be guaranteed to be on "one line" when the cylinder is rotated for welding, and also improves the welding yield (approximately 99%).

[0122] S3 laser welding:

[0123] An IPG single-mode ring fiber laser was used, with a center core diameter of 14μm and an outer ring core diameter of 100μm. The laser power was set to 800W, the moving speed to 140mm / s (welding displacement speed), and the positive defocusing amount to +2mm. Simultaneously, the beam oscillation function was activated, with a circular oscillation trajectory at a frequency of 800Hz and an amplitude of 0.7mm. 99.999% high-purity nitrogen gas was used for protection at a flow rate of 15L / min, to weld a continuous sealing weld bead around the lap joint.

[0124] Post-weld inspection revealed aesthetically pleasing weld formation with no spatter or cracks. Cross-sectional analysis of the welded samples showed uniform weld depth, approximately 75% for the nickel-plated steel shell and approximately 40% for the copper manifold. Pull-out tests showed a strength of 180 MPa and a contact resistance of 8 μΩ.

[0125] In the description of this invention, it should be understood that the terms "center," "longitudinal," "lateral," "front," "rear," "left," "right," "vertical," "horizontal," "top," "bottom," "inner," and "outer," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are only used to facilitate the description of this invention and to simplify the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limiting the scope of protection of this invention.

[0126] The foregoing has shown and described the basic principles, main features, and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The embodiments and descriptions in the specification are merely illustrative of the principles of the invention. Various changes and modifications can be made to the invention without departing from its spirit and scope, and all such changes and modifications fall within the scope of the present invention as claimed. The scope of protection of this invention is defined by the appended claims and their equivalents.

Claims

1. A welding device for a negative electrode current collector and a housing, characterized in that, include: A clamping block is configured to push the negative electrode current collector into the interior of the housing, so that the surface of the negative electrode current collector to be welded is interference-fitted with the inner wall of the housing, and forms an overlapping structure. Laser; The controller, connected to the laser, is configured to use a laser beam oscillating welding method to control the laser to align with the overlapping structure from the outside according to preset working parameters. During the laser welding process, part of the laser energy generated by the laser acts on the shell and part acts on the negative electrode current collector to form a molten nugget, thus completing the welding of the negative electrode current collector to the shell.

2. The welding device for the negative electrode current collector and the housing according to claim 1, characterized in that, The preset operating parameters include: Laser wavelength, wherein the laser wavelength is an infrared laser; Laser power, wherein the value of the laser power is in the range of 600W~800W; The oscillation frequency, wherein the value of the oscillation frequency is in the range of 100Hz-1000Hz; The swing amplitude, wherein the value of the swing amplitude ranges from 0.2 mm to 1.0 mm; The moving speed is in the range of 120 mm / s to 150 mm / s; Defocusing amount, the value of which ranges from +1mm to +3mm; A protective gas, wherein the protective gas is nitrogen with a purity ≥ 99.999%; Gas flow rate, wherein the gas flow rate ranges from 10L / min to 25L / min.

3. The welding device for the negative electrode current collector and the housing according to claim 1, characterized in that, The laser beam generated by the laser has a circular or figure-eight oscillation trajectory.

4. The welding device for the negative electrode current collector and the housing according to claim 1, characterized in that, The negative electrode current collector is made of copper or copper alloy with a thickness of 0.3mm-1.0mm; the shell is a nickel-plated steel shell with a nickel plating layer thickness of 2μm-10μm and a shell wall thickness of 0.25mm-0.6mm.

5. The welding device for the negative electrode current collector and the housing according to claim 1, characterized in that, After welding, the laser beam penetrates 60%-90% of the shell thickness and 20%-50% of the negative current collector thickness.

6. The welding device for the negative electrode current collector and the housing according to claim 1, characterized in that, The effective width of the melt core is greater than or equal to 527 μm.

7. The welding device for the negative electrode current collector and the housing according to claim 1, characterized in that, The angle between the incident direction of the laser beam generated by the laser and the axis of the housing is an obtuse angle.

8. A method for welding a negative electrode current collector to a housing, characterized in that, include: The negative electrode current collector is pushed into the interior of the housing, so that the surface of the negative electrode current collector to be welded is interference-fitted with the inner wall of the housing, and an overlapping structure is formed. The laser beam oscillating welding method is adopted. The laser is controlled to align with the overlapping structure from the outside according to the preset working parameters. During the laser welding process, part of the laser energy generated by the laser acts on the shell and part acts on the negative electrode current collector to form a molten nugget, thus completing the welding of the negative electrode current collector and the shell.

9. The welding method between the negative electrode current collector and the housing according to claim 8, characterized in that, Before pushing the negative current collector into the housing, the surface of the negative current collector to be soldered and the inner wall of the housing are cleaned to remove oil and oxides.

10. The welding method between the negative electrode current collector and the housing according to claim 8, characterized in that, During the welding process, the drive housing rotates the negative electrode current collector while the laser remains stationary.