A zero-splash lead-free solder wire, its preparation method and application

By combining a tin-silver-copper-bismuth-germanium-antimony alloy formulation with a double-end grafted polyether modified polyethylene glycol flux, the problems of solder wire spatter and poor wetting performance are solved, achieving a high-efficiency and environmentally friendly soldering effect.

CN123103245APending Publication Date: 2026-11-17深圳市永佳润金属有限公司
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611618214.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-20
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing solder wires suffer from problems such as excessive spatter, poor wetting performance, large flux residue, and low soldering yield during the soldering process, especially due to the rapid vaporization of organic components in the flux.

Method used

A tin alloy was prepared using a tin-silver-copper-bismuth-germanium-antimony multi-element low-silver formulation. Double-end grafted polyether modified polyethylene glycol was added to the flux as an anti-spatter agent. By introducing adipate bonds and polyoxypropylene ether segments at the soldering temperature, a physical entanglement network was formed to improve wetting performance and reduce spatter.

Benefits of technology

It achieves low spatter, high wetting, low residue, no cleaning, halogen-free and environmentally friendly solder wire, significantly improving the soldering yield, enhancing solder adhesion stability, and reducing spatter and contamination during the soldering process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123103245A_ABST
    Figure CN123103245A_ABST
Patent Text Reader

Abstract

This invention discloses a zero-splatter lead-free solder wire, its preparation method, and its application, belonging to the field of welding materials. The solder wire comprises a tin alloy hollow wire blank and an internal core wire, the core wire being a flux. The flux comprises the following components by weight: 65-75 parts hydrogenated rosin, 10-15 parts epoxy-modified hydrogenated castor oil, 6-10 parts composite diacid activator, 2-4 parts antioxidant, 1-3 parts plasticizer, and 3-7 parts anti-splatter agent. The anti-splatter agent is a double-end grafted polyether-modified polyethylene glycol, with polyethylene glycol as its main chain. The grafted chains are polyoxypropylene ethers located at both ends of the main chain, connected to the main chain by adipate ester bonds, and capped with methoxy groups at the ends. This invention solves the problems of excessive solder spatter, solder waste, and defects such as cold solder joints, bridging, and solder joint defects caused by the rapid vaporization of organic components in existing fluxes. It has the potential for application in household appliances, PCB soldering, and component lead soldering.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of welding materials technology, specifically to a zero-splash lead-free solder wire, its preparation method, and its application. Background Technology

[0002] Solder wire is a fundamental material used in the largest quantity and widest range of applications in general electronic manufacturing fields such as household appliances, PCB soldering, and component lead soldering. It typically consists of a tin alloy core wire and flux. The soldering spatter, wetting properties, and compatibility of solder wire directly affect soldering yield, production efficiency, and product reliability. Flux is a crucial component for improving the soldering performance of solder wire. In particular, at soldering temperatures, if the organic components in the flux vaporize too quickly, the overflowing gas can carry molten solder and cause spatter, resulting in solder waste, contamination of the PCB board and soldering equipment, and can also lead to cold solder joints, bridging, and other solder joint defects.

[0003] Existing technologies often suppress soldering spatter by increasing flux viscosity or adding antispatter agents to the flux. However, simply increasing flux viscosity often leads to decreased wetting performance; adding polymeric antispatter agents such as white oil or polyisobutylene may increase flux residue, causing problems such as cleaning difficulties; polyethylene glycol is often used as a film-forming agent, wetting agent, or surfactant in flux, but it is prone to main chain breakage and rapid vaporization at soldering temperatures, resulting in spatter.

[0004] Therefore, there is an urgent need for a solder wire that can simultaneously achieve low spatter, high wetting, low residue, and high soldering yield to solve the above problems. Summary of the Invention

[0005] Therefore, the present invention provides a zero-splash lead-free solder wire, its preparation method and application, to solve the problems of excessive soldering spatter, solder waste, cold solder joints, bridging and solder joint defects caused by the rapid vaporization of organic components in flux in the prior art.

[0006] To achieve the above objectives, the present invention provides the following technical solution: According to a first aspect of the present invention, a zero-splash lead-free solder wire is provided, the solder wire comprising a tin alloy hollow wire blank and a core wire inside the tin alloy hollow wire blank; The tin alloy hollow wire blank comprises the following components by weight: 96-97.5 parts tin, 1-1.5 parts silver, 0.5-0.8 parts copper, 0.3-0.6 parts bismuth, 0.01-0.03 parts germanium, and 0.1-0.3 parts antimony; the lead content of the solder wire is ≤0.1 wt.%; the core wire is flux filling the interior of the wire blank; the flux accounts for 2-2.5% of the total mass of the lead-free solder wire. The flux comprises the following components by weight: 65-75 parts hydrogenated rosin, 10-15 parts epoxy-modified hydrogenated castor oil, 6-10 parts composite diacid activator, 2-4 parts antioxidant, 1-3 parts plasticizer, and 3-7 parts anti-spatter agent. The anti-splash agent is a double-end grafted polyether modified polyethylene glycol, with the following general structural formula: CH3-[O-CH(CH3)-CH2]mO-CO-(CH2)4-CO-O-[CH2-CH2-O]n-CO-(CH2)4-CO-O-[CH2-CH(CH3)-O]m-CH3; Wherein, n is the degree of polymerization of the main chain, with a value of 130-140; m is the degree of polymerization of the grafted chain, with a value of 5-7; the main chain of the double-end grafted polyether modified polyethylene glycol is polyethylene glycol with a number average molecular weight of 5800-6200 Da; the grafted chain is polyoxypropylene ether, located at both ends of the main chain, with a number average molecular weight of 320-420 Da at each end, and the main chain and the grafted chain are connected by adipate ester bonds, with the grafted chain ends capped with methoxy groups; the number average molecular weight of the double-end grafted polyether modified polyethylene glycol is 6500-7200 Da, PDI≤1.3, hydroxyl value≤5mg KOH / g, and acid value≤1mg KOH / g.

[0007] Furthermore, the preparation of the double-end grafted polyether modified polyethylene glycol includes the following steps: Polypropylene glycol monomethyl ether (PPD) and adipic acid were added to a reactor at a molar ratio of 1:1.1. Then, 0.5 wt.% p-toluenesulfonic acid and 0.1 wt.% BHT (an antioxidant) were added, along with a dehydrating agent. The mixture was refluxed at 140-145°C for 3-4 hours under a nitrogen atmosphere. The generated water was separated using a water separator. The reaction was stopped when the acid value decreased to 50-55% of the initial value. The mixture was washed successively with NaOH solution and deionized water, dried with anhydrous sodium sulfate, and the solvent was removed by vacuum distillation to obtain polypropylene glycol-adipate monoester. Polyethylene glycol and polypropylene glycol-adipate monoester were added to a reactor at a molar ratio of 1:2.1. 0.5 wt.% p-toluenesulfonic acid, 0.1 wt.% BHT antioxidant, and a dehydrating agent were also added. The mixture was refluxed at 140-145 °C for 4-6 h under a nitrogen atmosphere. The reaction was stopped when the hydroxyl value was ≤5 mg KOH / g. The mixture was washed successively with NaOH solution and deionized water, dried with anhydrous sodium sulfate, and the solvent was removed by vacuum distillation. The mixture was then recrystallized twice with anhydrous ethanol and dried under vacuum at 40 °C for 24 h to obtain double-end grafted polyether modified polyethylene glycol.

[0008] Further, the polyethylene glycol is PEG6000; the polypropylene glycol monomethyl ether has a number-average molecular weight of 320-420 Da, a degree of polymerization of 5-7, and a moisture content of ≤0.1%; the NaOH solution has a concentration of 0.1 M, and the dehydrating agent is xylene.

[0009] Furthermore, the hydrogenated rosin has a hydrogenation degree ≥92%, a softening point of 75-85℃, and an acid value of 170-200 mg KOH / g; the epoxy-modified hydrogenated castor oil has an epoxy value of 0.3-0.5 eq / 100g and a hydroxyl value of 120-150 mg KOH / g; the composite diacid activator is a mixture of succinic acid, adipic acid, and glutaric acid in a mass ratio of 3:4:3; the antioxidant is a mixture of antioxidant BHT and antioxidant TBHQ in a mass ratio of 1:1; and the plasticizer is tributyl citrate.

[0010] According to a second aspect of the present invention, a method for preparing zero-splash lead-free solder wire is provided, which specifically includes the following steps: S1. Tin, silver, copper, bismuth and antimony are added into a vacuum melting furnace in proportion, stirred and melted under vacuum and nitrogen atmosphere, germanium particles are added after melting and kept at heat for reaction, and then cooled down for later use to obtain molten alloy; S2. Mix hydrogenated rosin and epoxy-modified hydrogenated castor oil, heat and stir, then cool down, add anti-splatter agent and continue stirring, then add composite diacid activator, antioxidant and plasticizer in sequence, stir at constant temperature, filter to remove impurities, cool to room temperature to obtain flux, seal and store in the dark. S3. After the molten alloy is heated and melted, it is injected into a continuous extruder to form a hollow wire blank. The preheated flux is injected into the hollow wire blank and then discharged at a uniform speed. After cooling naturally to room temperature, it is then drawn, annealed, polished and packaged to obtain lead-free solder wire.

[0011] Furthermore, the vacuum degree mentioned in step S1 is ≤10Pa, the stirring and melting conditions are stirring at 100rpm for 10min at 260-280℃, the heat preservation reaction time is 30-40min, and the cooling and standby temperature is 250℃.

[0012] Further, step S2 specifically includes the following steps: mixing hydrogenated rosin and epoxy-modified hydrogenated castor oil, heating to 120-140℃, stirring at 100 rpm for 20-40 minutes, then cooling to 100-110℃, adding anti-splatter agent and continuing to stir for 10-30 minutes, then adding composite diacid activator, antioxidant and plasticizer in sequence, maintaining a constant temperature of 110℃, stirring at 100 rpm for 20-30 minutes, filtering through a 200-mesh filter to remove impurities, cooling to room temperature to obtain flux, and storing in a sealed, light-proof container.

[0013] Further, in step S3, the hollow wire blank has a wire diameter of 1.5 mm, a melting temperature of 250°C, and a preheating temperature of 80°C; the wire drawing is a multi-stage diameter reduction wire drawing, with target diameters of 1.2 mm, 1.0 mm, 0.9 mm, 0.85 mm, and 0.8 mm respectively; the annealing conditions are 180-200°C for 15-25 minutes, with nitrogen protection throughout; the packaging is vacuum packaging, internally filled with nitrogen and sealed, and includes a desiccant.

[0014] Furthermore, in step S3, the amount of flux added to the hollow wire blank is 2-2.5% of the total mass of the lead-free solder wire.

[0015] According to a third aspect of the present invention, an application of zero-splash lead-free solder wire in household appliances, PCB soldering, and component lead soldering is provided.

[0016] The present invention has the following advantages: 1. This invention uses a tin-silver-copper-bismuth-germanium-antimony (Sn-Ag-Cu-Bi-Ge-Sb) multi-element low-silver formula to prepare tin alloy. By synergistically refining grains, reducing melt surface tension, and improving wetting performance through Bi, Ge, and Sb, the solder wire achieves low spatter, high strength, and low cost.

[0017] 2. The flux prepared by this invention adopts a rosin-based formula. By adding double-end grafted polyether modified polyethylene glycol anti-spatter agent, composite organic acid activator, antioxidant, and plasticizer, it achieves low spatter, high wetting, low residue, no cleaning, and halogen-free environmental protection in the welding range of 260–300℃.

[0018] 3. This invention introduces adipate bonds into the anti-spatter agent molecule. These bonds have lower bond energy than CO bonds and break first at the welding temperature, releasing a small amount of CO2 and small molecule alcohols. As the temperature increases, the polyoxypropylene ether segments and the polyethylene glycol backbone gradually degrade. At welding temperatures of 260-280℃, the anti-spatter agent is in a semi-molten viscous flow state. The polyoxypropylene ether segments form a physical entanglement network with rosin molecules, increasing the flux viscosity. Increased viscosity requires greater resistance to gas escape, reducing bubble growth rate and decreasing kinetic energy during bubble collapse, thus reducing the amount of melt carried away by bubbles. Furthermore, this anti-spatter agent is oriented at the molten solder-flux interface, reducing interfacial tension and allowing the molten solder to adhere more stably to the solder joint, making it less susceptible to being blown away by airflow. Attached Figure Description

[0019] To more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are merely exemplary, and those skilled in the art can derive other embodiments based on the provided drawings without creative effort.

[0020] The structures, proportions, sizes, etc. illustrated in this specification are only for the purpose of assisting those skilled in the art in understanding and reading the content disclosed herein, and are not intended to limit the conditions under which the present invention can be implemented. Therefore, they have no substantial technical significance. Any modifications to the structure, changes in the proportions, or adjustments to the size, without affecting the effects and objectives that the present invention can produce, should still fall within the scope of the technical content disclosed in the present invention.

[0021] Figure 1 The TGA curve of the double-end grafted polyether modified polyethylene glycol provided in Example 1 of the present invention. Detailed Implementation

[0022] The following specific embodiments illustrate the implementation of the present invention. Those skilled in the art can easily understand other advantages and effects of the present invention from the content disclosed in this specification. Obviously, the described embodiments are only some, not all, of the embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0023] According to a first aspect of the present invention, a zero-splash lead-free solder wire is provided, the solder wire comprising a tin alloy hollow wire blank and a core wire inside the tin alloy hollow wire blank; The tin alloy hollow wire blank comprises the following components by weight: 96-97.5 parts tin, 1-1.5 parts silver, 0.5-0.8 parts copper, 0.3-0.6 parts bismuth, 0.01-0.03 parts germanium, and 0.1-0.3 parts antimony; the lead content of the solder wire is ≤0.1 wt.%; the core wire is flux filling the interior of the wire blank; the flux accounts for 2-2.5% of the total mass of the lead-free solder wire. The flux comprises the following components by weight: 65-75 parts hydrogenated rosin, 10-15 parts epoxy-modified hydrogenated castor oil, 6-10 parts composite diacid activator, 2-4 parts antioxidant, 1-3 parts plasticizer, and 3-7 parts anti-spatter agent. The anti-splatter agent is a double-end grafted polyether modified polyethylene glycol, with the following general structural formula: CH3-[O-CH(CH3)-CH2]mO-CO-(CH2)4-CO-O-[CH2-CH2-O]n-CO-(CH2)4-CO-O-[CH2-CH(CH3)-O]m-CH3; Wherein, n is the degree of polymerization of the main chain, with a value of 130-140; m is the degree of polymerization of the grafted chain, with a value of 5-7; the main chain of the double-end grafted polyether modified polyethylene glycol is polyethylene glycol, with a number average molecular weight of 5800-6200 Da; the grafted chains are polyoxypropylene ethers, located at both ends of the main chain, with a number average molecular weight of 320-420 Da at each end, and the main chain and the grafted chains are connected by adipate bonds, with the grafted chains capped with methoxy groups; the number average molecular weight of the double-end grafted polyether modified polyethylene glycol is 6500-7200 Da, PDI≤1.3, hydroxyl value≤5mg KOH / g, and acid value≤1mg KOH / g.

[0024] The preparation of double-end grafted polyether modified polyethylene glycol includes the following steps: Polypropylene glycol monomethyl ether (PPD) and adipic acid were added to a reactor at a molar ratio of 1:1.1. Then, 0.5 wt.% p-toluenesulfonic acid and 0.1 wt.% BHT (an antioxidant) were added, along with a dehydrating agent. The mixture was refluxed at 140-145°C for 3-4 hours under a nitrogen atmosphere. The generated water was separated using a water separator. The reaction was stopped when the acid value decreased to 50-55% of the initial value. The mixture was washed successively with NaOH solution and deionized water, dried with anhydrous sodium sulfate, and the solvent was removed by vacuum distillation to obtain polypropylene glycol-adipate monoester. Polyethylene glycol and polypropylene glycol-adipate monoester were added to a reactor at a molar ratio of 1:2.1. 0.5 wt.% p-toluenesulfonic acid, 0.1 wt.% BHT antioxidant, and a dehydrating agent were also added. The mixture was refluxed at 140-145 °C for 4-6 h under a nitrogen atmosphere. The reaction was stopped when the hydroxyl value was ≤5 mg KOH / g. The mixture was washed successively with NaOH solution and deionized water, dried with anhydrous sodium sulfate, and the solvent was removed by vacuum distillation. The mixture was then recrystallized twice with anhydrous ethanol and dried under vacuum at 40 °C for 24 h to obtain double-end grafted polyether modified polyethylene glycol.

[0025] Among them, polyethylene glycol is PEG6000; polypropylene glycol monomethyl ether has a number average molecular weight of 320-420 Da, a degree of polymerization of 5-7, and a moisture content of ≤0.1%; the concentration of NaOH solution is 0.1M, and the dehydrating agent is xylene.

[0026] The hydrogenated rosin has a hydrogenation degree ≥92%, a softening point of 75-85℃, and an acid value of 170-200mg KOH / g; the epoxy-modified hydrogenated castor oil has an epoxy value of 0.3-0.5 eq / 100g and a hydroxyl value of 120-150mg KOH / g; the composite diacid activator is a mixture of succinic acid, adipic acid, and glutaric acid in a mass ratio of 3:4:3; the antioxidant is a mixture of antioxidant BHT and antioxidant TBHQ in a mass ratio of 1:1; and the plasticizer is tributyl citrate.

[0027] According to a second aspect of the present invention, a method for preparing zero-splash lead-free solder wire is provided, which specifically includes the following steps: S1. Tin, silver, copper, bismuth and antimony are added into a vacuum melting furnace in proportion, stirred and melted under vacuum and nitrogen atmosphere, germanium particles are added after melting and kept at heat for reaction, and then cooled down for later use to obtain molten alloy; S2. Mix hydrogenated rosin and epoxy-modified hydrogenated castor oil, heat and stir, then cool down, add anti-splatter agent and continue stirring, then add composite diacid activator, antioxidant and plasticizer in sequence, stir at constant temperature, filter to remove impurities, cool to room temperature to obtain flux, seal and store in the dark. S3. After the molten alloy is heated and melted, it is injected into a continuous extruder to form a hollow wire blank. The preheated flux is injected into the hollow wire blank and then discharged at a uniform speed. After cooling naturally to room temperature, it is then drawn, annealed, polished and packaged to obtain lead-free solder wire.

[0028] In step S1, the vacuum degree is ≤10Pa, the stirring and melting conditions are 260-280℃ at 100rpm for 10min, the heat preservation reaction time is 30-40min, and the cooling temperature for standby is 250℃.

[0029] Step S2 specifically includes the following steps: mixing hydrogenated rosin and epoxy-modified hydrogenated castor oil, heating to 120-140℃, stirring at 100 rpm for 20-40 minutes, then cooling to 100-110℃, adding an anti-splatter agent and continuing to stir for 10-30 minutes, then sequentially adding a composite diacid activator, an antioxidant, and a plasticizer, maintaining a constant temperature of 110℃, stirring at 100 rpm for 20-30 minutes, filtering through a 200-mesh filter to remove impurities, cooling to room temperature to obtain flux, and storing it in a sealed, light-proof container.

[0030] In step S3, the hollow wire blank has a diameter of 1.5 mm, a melting temperature of 250 °C, and a preheating temperature of 80 °C. The wire drawing is a multi-stage diameter reduction drawing with target diameters of 1.2 mm, 1.0 mm, 0.9 mm, 0.85 mm, and 0.8 mm, respectively. The annealing conditions are 180-200 °C for 15-25 min, with nitrogen protection throughout. The packaging is vacuum packaging, sealed after being filled with nitrogen, and includes a desiccant.

[0031] In step S3, the amount of flux added to the hollow wire blank is 2-2.5% of the total mass of the lead-free solder wire.

[0032] To better illustrate the technical path of the present invention, the following embodiments and comparative examples are provided.

[0033] Example 1 S1. Add 971.8g of tin, 13g of silver, 7g of copper, 5g of bismuth and 3g of antimony into a vacuum melting furnace in proportion. Stir and melt at 270℃ and 100rpm for 10min under a vacuum of 10Pa and a nitrogen atmosphere. After melting, add 0.2g of germanium particles and keep it at the temperature for 35min. After keeping it at the temperature, cool it down for later use to obtain the molten alloy. S2. Mix 70g of hydrogenated rosin (hydrogenation degree ≥92%, softening point 75-85℃, acid value 170-200mg KOH / g, purchased from Guangxi Wuzhou Richeng Forestry Chemical Co., Ltd., model RH-302) and 12g of epoxy-modified hydrogenated castor oil (purchased from Jiangsu Haian Petrochemical Plant, model EL-10, epoxy value 0.3-0.5eq / 100g, hydroxyl value 120-130mg KOH / g). Heat to 130℃ and stir at 100rpm for 30min, then cool to 105℃. Add 5g of anti-splatter agent and continue stirring for 20min. Then add 2.4g of succinic acid (purchased from Langfang Qianyao Technology Co., Ltd., CAS: 110-15-6), 3.2g of adipic acid (purchased from Langfang Qianyao Technology Co., Ltd., CAS: 124-04-9), and 2.4g of glutaric acid (purchased from Shanghai Kaisai Chemical Co., Ltd., CAS: 110- 94-1), 1.5g of antioxidant BHT (purchased from Henan Kangzhiwang Biotechnology Co., Ltd., molecular weight 220.36Da, CAS: 105-11-3), 1.5g of antioxidant TBHQ (purchased from Henan Kangzhiwang Biotechnology Co., Ltd., CAS: 106-51-4) and 2g of tributyl citrate were stirred at 110℃ and 100rpm for 25min, then filtered through a 200-mesh filter to remove impurities, cooled to room temperature, and the flux was obtained. It was then sealed and stored away from light. The preparation of the anti-splash agent includes the following steps: 47.9 g of polypropylene glycol monomethyl ether (purchased from Hubei Langbowan Biopharmaceutical Co., Ltd., molecular weight 400 Da, degree of polymerization 5-7, moisture ≤0.1%) and 19.25 g of adipic acid (purchased from Langfang Qianyao Technology Co., Ltd., CAS: 124-04-9) were added to a reaction vessel, along with 336 mg of p-toluenesulfonic acid (purchased from Shandong Yukang Chemical Co., Ltd., CAS: 104-15-4), 67 mg of antioxidant BHT, and 23 mL of xylene (purchased from Jinan Xichuan Chemical Technology Co., Ltd.). The reaction was refluxed at 145 °C for 3 h under a nitrogen atmosphere, and the generated water was separated by a water separator. The product was washed successively with 0.1 M NaOH solution and deionized water, dried with anhydrous sodium sulfate, and the solvent was removed by vacuum distillation to obtain 52.81 g of polypropylene glycol-adipate monoester, with a yield of 83.5%. 285.71g of PEG6000, dried under vacuum at 80℃ for 4h, and 52.81g of polypropylene glycol-adipate monoester were added to a reaction vessel, along with 1.69g of p-toluenesulfonic acid, 339mg of antioxidant BHT, and 116mL of xylene. The mixture was refluxed at 145℃ for 5h under a nitrogen atmosphere. After washing with 0.1M NaOH solution and deionized water, the mixture was dried with anhydrous sodium sulfate. The solvent was removed by vacuum distillation, and the mixture was recrystallized twice with anhydrous ethanol. After drying under vacuum at 40℃ for 24h, 301 was obtained. 2g of bi-terminated polyether-modified polyethylene glycol was prepared, with a yield of 90.1%. Furthermore, the molecular weight and molecular weight distribution of the prepared bi-terminated polyether-modified polyethylene glycol were determined by gel permeation chromatography. The mobile phase was tetrahydrofuran, the standard was polystyrene, the column temperature was 35℃, the flow rate was 1mL / min, and the injection concentration was 1.5mg / mL. The number-average molecular weight of the bi-terminated polyether-modified polyethylene glycol was determined to be 7019 Da, and the PDI was 1.1. The hydroxyl value calculated by the acetic acid-pyridine esterification method was 3.3 mg. The KOH / g concentration was determined by titration with KOH, yielding an acid value of 0.87 mg KOH / g. The measured number-average molecular weight of the product was 7019 Da, which closely matches the theoretical value of 7020 Da calculated based on complete double-end grafting, indicating that both hydroxyl groups at both ends of the polyethylene glycol were quantitatively esterified, and the grafting reaction was complete. A PDI of 1.1 indicates a narrow molecular weight distribution and few side reactions. A hydroxyl value of 3.3 mg KOH / g (≤5 mg KOH / g) further confirms that the terminal hydroxyl groups have essentially reacted completely. An acid value of 0.87 mg KOH / g (≤1 mg KOH / g) indicates that free acid was sufficiently removed after washing and recrystallization. These molecular weight and yield data collectively demonstrate that the two-step esterification process can stably produce double-end grafted polyether-modified polyethylene glycol with the target structure. Furthermore, this invention employs a thermogravimetric analyzer to determine the TGA curves of double-end-grafted polyether-modified polyethylene glycol under a nitrogen atmosphere at a heating rate of 10°C / min and a temperature range of 30-600°C. The thermogravimetric analysis was performed on the double-end-grafted polyether-modified polyethylene glycol prepared in Example 1, and the curves are shown below. Figure 1 As shown, the thermal weight loss of double-end grafted polyether modified polyethylene glycol can be divided into three stages: the first stage (230-280℃) involves a weight loss of approximately 4.5%, which is due to the breakage of the adipate bonds at both ends, releasing a small amount of carbon dioxide and small molecule alcohols; the second stage (280-350℃) involves a weight loss of approximately 10%, which is due to the depolymerization of the polyoxypropylene ether grafted segments; the third stage (350-430℃) involves a weight loss of approximately 62%, which is due to the degradation of the polyethylene glycol backbone; at 600℃, the remaining mass is approximately 23.0%. S3. The molten alloy is heated to 250°C and then injected into a continuous extruder to form a hollow wire blank with a diameter of 1.5 mm. Flux preheated to 80°C is injected into the hollow wire blank and then discharged at a uniform speed. After natural cooling to room temperature, it is then drawn, annealed, polished and packaged to obtain lead-free solder wire. The annealing conditions are as follows: annealing at 190℃ for 20 minutes in an annealing furnace under nitrogen protection throughout the process; the packaging is vacuum-packed, sealed after being filled with nitrogen, and contains a desiccant; the flux added to the hollow wire blank is 2.2% of the total mass of the lead-free solder wire; the wire drawing is a multi-stage diameter reduction drawing, with target diameters of 1.2mm, 1.0mm, 0.9mm, 0.85mm and 0.8mm respectively, that is, the final solder wire diameter is 0.8mm.

[0034] Example 2 This embodiment is based on Embodiment 1, except that the amount of anti-splatter agent added in step S2 is 3g and the amount of hydrogenated rosin added is 72g, while the other specific parameters are the same as in Embodiment 1.

[0035] Example 3 This embodiment is based on Embodiment 1, except that the amount of anti-splatter agent added in step S2 is 7g and the amount of hydrogenated rosin added is 68g, while the other specific parameters are the same as in Embodiment 1.

[0036] Comparative Example 1 This comparative example is based on Example 1, except that an equal amount of hydrogenated rosin is used instead of the anti-splatter agent, while the other specific parameters are the same as in Example 1.

[0037] Comparative Example 2 This comparative example is based on Example 1, except that an equal amount of PEG6000 is used to replace the double-end grafted polyether modified polyethylene glycol as the anti-splatter agent, while the other specific parameters are the same as in Example 1.

[0038] Comparative Example 3 This comparative example is based on Example 1, except that an equal amount of polyethylene glycol-maleic anhydride graft is used as the anti-splatter agent, while the other specific parameters are the same as in Example 1. The preparation method of the polyethylene glycol-maleic anhydride graft is based on patent CN120170328A, which involves heating and melting 60g of PEG-600 under a nitrogen atmosphere, then adding 11.8g of maleic anhydride and 0.72g of p-toluenesulfonic acid, stirring at 82°C for 5.5h until the acid value reaches 130mgKOH / g, and controlling the grafting rate at 40%.

[0039] Comparative Example 4 This comparative example is based on Example 1, except that an equal amount of polyethylene glycol-polypropylene glycol copolymer was used as the anti-splatter agent (poloxam 188, purchased from Hubei Weideli Chemical Reagent Co., Ltd.), and the other specific parameters are the same as in Example 1.

[0040] Test Example 1 This invention refers to the method of GB / T 10574.14-2017 "Chemical Analysis Methods for Tin-Lead Solder Part 14: Determination of the Contents of Tin, Lead, Antimony, Bismuth, Silver, Copper, Zinc, Cadmium and Arsenic by Photoelectric Emission Spectrometry", and uses a direct-reading spectrometer (Shimadzu PDA-7000) to determine the elemental composition of tin alloys. The results are recorded in Table 1.

[0041] Table 1. Elemental composition of tin alloys

[0042] It can be seen that the lead content in the tin alloy prepared by this invention is 0.004 wt.% and the impurity content is 0.038 wt.%, which meets the industry standard for lead-free solder wire (refer to the standards: RoHS, GB / T 20422-2018 "Lead-free solder").

[0043] The present invention also refers to the standard IEC 61249-2-21 to test the halogen content of the solder wire and flux prepared in Example 1 using a halogen detector, and the results are recorded in Table 2.

[0044] Table 2 Halogen content of solder wire and flux prepared in Example 1

[0045] As can be seen from Table 2, the flux and finished solder wire prepared by this invention have low halogen content, and the halogen-free index of the finished product is far below the industry limit, which is environmentally friendly.

[0046] Test Example 2 This invention uses a rotational viscometer to measure the flux in solder wires prepared in each embodiment and comparative example at 280°C and a shear rate of 10 s. -1The melt viscosity was measured, and the surface tension of the solder-flux at 280°C was determined by the pendant drop method using a contact angle meter.

[0047] This invention refers to the method in GB / T 38265.13-2021 "Test Methods for Flux - Part 13: Determination of Flux Splashing" to determine the amount of solder spatter in the solder wires prepared in each embodiment and comparative example, specifically including the following steps: Take a 100mm solder wire sample and weld it at a uniform speed on a 280℃ soldering station. Collect the spatter with a smooth inner wall collecting cover, weigh it, and record the amount of spatter.

[0048] This invention, referring to GB / T 11364-2008 "Test Method for Wetting Properties of Solder Wire", determines the wetting performance of solder wire, specifically including the following steps: Place 0.3g of solder wire in the center of a 40mm×40mm×0.3mm copper sheet, heat it on a 280℃ soldering station for 30s, and measure the spreading area after cooling.

[0049] This invention uses 0.8mm diameter solder wire to continuously solder 1000 joints on a 280℃ soldering station, recording the number of qualified joints. Joints without cold solder joints, bridging, or spikes are considered good joints, and the good solder joint rate is recorded. The results of the above experiment are recorded in Table 3.

[0050] In this invention, a commercially available ALPHA Telecore Plus SAC305 lead-free solder wire (purchased from MacDermid Alpha, USA, Sn96.5Ag3.0Cu0.5 alloy, wire diameter 0.8mm, flux 2.0%, no-clean system) was selected as a control group sample.

[0051] Table 3. Flux viscosity, flux-solder surface tension, solder wire spatter, spreading area, and soldering yield.

[0052] Note: "-" in the table indicates that no test was performed.

[0053] As shown in Table 3, the solder wire prepared in the embodiments of the present invention has a significantly higher viscosity than the comparative example and the control group, approaching 3 Pa·s, and a lower surface tension, only about 400 mN / m. Furthermore, the viscosity is positively correlated with the flux viscosity and the amount of anti-spatter agent added, while the surface tension is negatively correlated. After preparing complete solder wire, the spatter amounts of the solder wires in Examples 1-3 and the control group were 0.007 g / 100 mm, 0.009 g / 100 mm, and 0.007 g / 100 mm, respectively, with a spreading area of ​​88 mm². 2 86mm 2 89mm 2The soldering yields were 99.8%, 99.6%, and 99.7%, significantly better than the comparative and control groups. The results of the example and control groups indicate that, under the same alloy conditions (Sn96.5Ag3.0Cu0.5), Example 1, using double-end grafted polyether-modified polyethylene glycol as an anti-spatter agent, significantly reduced spatter and significantly improved the soldering yield compared to commercially available SAC305 solder wires using different flux / anti-spatter agent systems, demonstrating significantly superior anti-spatter performance compared to commercially available products.

[0054] Compared to the examples, Comparative Example 1, which replaced modified polyethylene glycol with hydrogenated rosin (i.e., without anti-spatter agent), showed a significant increase in flux-solder surface tension to 610 mN / m, a significant decrease in viscosity, spreading area, and solder yield, and an increase in solder spatter. Comparative Examples 2, 3, and 4, which replaced double-end-grafted polyether-modified polyethylene glycol as anti-spatter agents with PEG6000, polyethylene glycol-maleic anhydride graft, and polyethylene glycol-polypropylene glycol copolymer, respectively, showed flux viscosity decreases by 78.8%, 48.5%, and 54.5% compared to Example 1, respectively; flux-solder surface tension increases by 38.1%, 21.4%, and 26.2%; solder spatter increases by 50-160%; spreading area decreases by 4.5%-9.1%; and solder yield decreases by 0.4-0.6 percentage points. The above results indicate that using double-end grafted polyether-modified polyethylene glycol (PEG) as an anti-spatter agent can significantly increase flux viscosity and reduce the surface tension at the flux-solder interface without reducing the flux's wetting properties, thus significantly improving soldering yield. This is because the preferential breakage of adipate bonds allows for the slow release of gas in the initial stage of soldering, preventing the concentrated breakage and rapid vaporization of the PEG backbone at the soldering temperature, which would otherwise cause spatter. Furthermore, at 280°C, the double-end grafted polyether-modified PEG anti-spatter agent is in a semi-thermal viscous flow state, where the polyoxypropylene ether segments form a physical entanglement network with rosin molecules, increasing the flux system viscosity, hindering gas escape during soldering, reducing the bubble generation rate, and thus reducing solder molten spatter. Additionally, the low surface tension between the molten solder and flux allows the anti-spatter agent to oriented at the interface, making it easier for the molten solder to adhere stably to the solder joint, reducing spatter.

[0055] Furthermore, although PEG6000, polyethylene glycol-maleic anhydride grafts, and polyethylene glycol-polypropylene glycol copolymers all contain polyether segments, PEG6000 has linear segments and does not contain polyoxypropylene ether grafts or ester bonds. In double-end grafted polyether-modified polyethylene glycol, the bond energy of the ester bond is approximately 350 kJ / mol, lower than the 360 ​​kJ / mol of the CO bond. During soldering, the ester bond breaks before the polyethylene glycol main chain and the polyoxypropylene ether chain, producing carbon dioxide and small molecule alcohols. As the temperature rises, the polyoxypropylene ether segments gradually depolymerize and the polyethylene glycol main chain breaks, and the gas generated by flux vaporization is gradually released, thereby reducing spatter. In contrast, pure polyethylene glycol undergoes homolytic chain cleavage at 250°C, rapidly vaporizing to produce a large amount of gas. This gas rushes out from inside the core wire, causing molten solder to spatter. While polyethylene glycol-maleic anhydride grafts and polyethylene glycol-polypropylene glycol copolymers contain ester bonds and polyoxypropylene ether segments, respectively, the polyethylene glycol-maleic anhydride graft lacks polyoxypropylene ether segments, making it difficult to entangle with rosin molecules and unable to orient the anti-spatter agent at the solder-flux interface through hydrophobic segments. This limits its effectiveness in improving melt viscosity and interfacial tension. In contrast, the polyethylene glycol-polypropylene glycol copolymer does not contain ester bonds; it connects polyethylene glycol and polypropylene glycol segments through ether bonds. Lacking preferential thermal breakage sites in its molecule, the main molecular chain breaks rapidly at high temperatures, causing spatter. Furthermore, double-end-grafted polyether-modified polyethylene glycol has polyoxypropylene ether segments grafted at both ends, forming a symmetrical polyoxypropylene ether-ester bond-polyethylene glycol-ester bond-polyoxypropylene ether structure. This structure allows both polyoxypropylene ether segments to extend freely and participate in entanglement with rosin, constructing a more complete physical network and a more ordered interface arrangement. Furthermore, the two adipate bonds break uniformly, resulting in a gradual gas release. Table 3 also shows that grafting polyoxypropylene ether segments onto both ends of polyethylene glycol via ester bonds significantly improves the anti-splatter performance of solder wires, and there is a synergistic effect between the ester bonds and the polyoxypropylene ether segments.

[0056] Although the present invention has been described in detail above with general descriptions and specific embodiments, modifications or improvements can be made to it, which will be obvious to those skilled in the art. Therefore, all such modifications or improvements made without departing from the spirit of the present invention fall within the scope of protection claimed by the present invention.

Claims

1. A zero-splash lead-free solder wire, characterized in that, The solder wire comprises a tin alloy hollow wire blank and a core wire inside the tin alloy hollow wire blank; The tin alloy hollow wire blank comprises the following components by weight: 96-97.5 parts tin, 1-1.5 parts silver, 0.5-0.8 parts copper, 0.3-0.6 parts bismuth, 0.01-0.03 parts germanium, and 0.1-0.3 parts antimony; the lead content of the solder wire is ≤0.1 wt.%; the core wire is flux filling the interior of the wire blank; the flux accounts for 2-2.5% of the total mass of the lead-free solder wire. The flux comprises the following components by weight: 65-75 parts hydrogenated rosin, 10-15 parts epoxy-modified hydrogenated castor oil, 6-10 parts composite diacid activator, 2-4 parts antioxidant, 1-3 parts plasticizer, and 3-7 parts anti-spatter agent. The anti-splash agent is a double-end grafted polyether modified polyethylene glycol, with the following general structural formula: CH3-[O-CH(CH3)-CH2]mO-CO-(CH2)4-CO-O-[CH2-CH2-O]n-CO-(CH2)4-CO-O-[CH2-CH(CH3)-O]m-CH3; Wherein, n is the degree of polymerization of the main chain, with a value of 130-140; m is the degree of polymerization of the grafted chain, with a value of 5-7; the main chain of the double-end grafted polyether modified polyethylene glycol is polyethylene glycol with a number average molecular weight of 5800-6200 Da; the grafted chain is polyoxypropylene ether, located at both ends of the main chain, with a number average molecular weight of 320-420 Da at each end, and the main chain and the grafted chain are connected by adipate ester bonds, with the grafted chain ends capped with methoxy groups; the number average molecular weight of the double-end grafted polyether modified polyethylene glycol is 6500-7200 Da, PDI≤1.3, hydroxyl value≤5mg KOH / g, and acid value≤1mg KOH / g.

2. The lead-free solder wire as described in claim 1, characterized in that, The preparation of the double-end grafted polyether modified polyethylene glycol includes the following steps: Polypropylene glycol monomethyl ether (PPD) and adipic acid were added to a reactor at a molar ratio of 1:1.

1. Then, 0.5 wt.% p-toluenesulfonic acid and 0.1 wt.% BHT (an antioxidant) were added, along with a dehydrating agent. The mixture was refluxed at 140-145°C for 3-4 hours under a nitrogen atmosphere. The generated water was separated using a water separator. The reaction was stopped when the acid value decreased to 50-55% of the initial value. The mixture was washed successively with NaOH solution and deionized water, dried with anhydrous sodium sulfate, and the solvent was removed by vacuum distillation to obtain polypropylene glycol-adipate monoester. Polyethylene glycol and polypropylene glycol-adipate monoester were added to a reactor at a molar ratio of 1:2.

1. 0.5 wt.% p-toluenesulfonic acid, 0.1 wt.% BHT antioxidant, and a dehydrating agent were also added. The mixture was refluxed at 140-145 °C for 4-6 h under a nitrogen atmosphere. The reaction was stopped when the hydroxyl value was ≤5 mg KOH / g. The mixture was washed successively with NaOH solution and deionized water, dried with anhydrous sodium sulfate, and the solvent was removed by vacuum distillation. The mixture was then recrystallized twice with anhydrous ethanol and dried under vacuum at 40 °C for 24 h to obtain double-end grafted polyether modified polyethylene glycol.

3. The lead-free solder wire as described in claim 2, characterized in that, The polyethylene glycol is PEG6000; the polypropylene glycol monomethyl ether has a number-average molecular weight of 320-420 Da, a degree of polymerization of 5-7, and a moisture content of ≤0.1%; the NaOH solution has a concentration of 0.1 M, and the dehydrating agent is xylene.

4. The lead-free solder wire as described in claim 1, characterized in that, The hydrogenated rosin has a hydrogenation degree ≥92%, a softening point of 75-85℃, and an acid value of 170-200 mg KOH / g; the epoxy-modified hydrogenated castor oil has an epoxy value of 0.3-0.5 eq / 100g and a hydroxyl value of 120-150 mg KOH / g; the composite diacid activator is a mixture of succinic acid, adipic acid, and glutaric acid in a mass ratio of 3:4:3; the antioxidant is a mixture of antioxidant BHT and antioxidant TBHQ in a mass ratio of 1:1; and the plasticizer is tributyl citrate.

5. A method for preparing zero-splash lead-free solder wire, used to prepare the lead-free solder wire according to any one of claims 1-4, characterized in that, Specifically, the following steps are included: S1. Tin, silver, copper, bismuth and antimony are added into a vacuum melting furnace in proportion, stirred and melted under vacuum and nitrogen atmosphere, germanium particles are added after melting and kept at heat for reaction, and then cooled down for later use to obtain molten alloy; S2. Mix hydrogenated rosin and epoxy-modified hydrogenated castor oil, heat and stir, then cool down, add anti-splatter agent and continue stirring, then add composite diacid activator, antioxidant and plasticizer in sequence, stir at constant temperature, filter to remove impurities, cool to room temperature to obtain flux, seal and store in the dark. S3. After the molten alloy is heated and melted, it is injected into a continuous extruder to form a hollow wire blank. The preheated flux is injected into the hollow wire blank and then discharged at a uniform speed. After cooling naturally to room temperature, it is then drawn, annealed, polished and packaged to obtain lead-free solder wire.

6. The preparation method according to claim 5, characterized in that, The vacuum degree mentioned in step S1 is ≤10Pa, the stirring and melting conditions are 100rpm stirring for 10min at 260-280℃, the heat preservation reaction time is 30-40min, and the cooling and standby temperature is 250℃.

7. The preparation method according to claim 5, characterized in that, Step S2 specifically includes the following steps: Mix hydrogenated rosin and epoxy-modified hydrogenated castor oil, heat to 120-140℃, stir at 100 rpm for 20-40 minutes, then cool to 100-110℃, add anti-splatter agent and continue stirring for 10-30 minutes, then add composite diacid activator, antioxidant and plasticizer in sequence, keep at 110℃ and stir at 100 rpm for 20-30 minutes, filter through a 200-mesh filter to remove impurities, cool to room temperature to obtain flux, and store in a sealed, light-proof container.

8. The preparation method according to claim 5, characterized in that, The hollow wire blank mentioned in step S3 has a wire diameter of 1.5 mm, a heating and melting temperature of 250°C, and a preheating temperature of 80°C; the wire drawing is a multi-stage diameter reduction wire drawing, with target diameters of 1.2 mm, 1.0 mm, 0.9 mm, 0.85 mm, and 0.8 mm respectively; the annealing conditions are 180-200°C for 15-25 minutes, with nitrogen protection throughout; the packaging is vacuum packaging, filled with nitrogen and sealed, and includes a desiccant.

9. The preparation method according to claim 5, characterized in that, The amount of flux added to the hollow wire blank in step S3 is 2-2.5% of the total mass of the lead-free solder wire.

10. The application of a zero-splash lead-free solder wire in household appliances, PCB soldering, and component lead soldering, characterized in that... The lead-free solder wire described in any one of claims 1-4 is used.

Citation Information

Patent Citations

  • VOC-free water-soluble environment-friendly scaling powder and preparation method thereof

    CN120170328A