A high-interface-area, low-defect epoxy resin cored diamond roller and its preparation method
By using epoxy resin AB glue as the core material and employing self-flowing casting and curing technology, the problems of insufficient interface holding performance and internal defects in internally plated diamond rollers have been solved, achieving efficient and low-cost high-precision diamond roller manufacturing, suitable for precision grinding.
Patent Information
- Application Number
- CN202611270322.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-20
- Publication Date
- 2026-11-17
AI Technical Summary
The existing low-temperature alloy core casting process for internally plated diamond rollers has problems such as insufficient interface holding performance, many internal pore defects, low matrix hardness, and cumbersome core casting process with long cycle, which affects processing efficiency and cost.
Using epoxy resin AB glue as the core material, a dense bonding layer is formed through self-flowing pouring and curing. Combining mechanical interlocking and adhesive force, it replaces the traditional low-temperature alloy casting, simplifies the process, and improves interface strength and internal density.
It significantly improves the interface bonding strength, reduces internal defects, shortens the core casting cycle, reduces costs, and extends the service life of rollers, making it suitable for high-precision and high-reliability precision grinding.
Smart Images

Figure CN123103537A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of superhard material tool technology, and specifically relates to a diamond roller for precision forming grinding wheel dressing and its preparation method. Background Technology
[0002] Diamond rollers are the core tools used for dressing grinding wheels in precision forming grinding. With their advantages of high precision, high efficiency and long service life, they are widely used in high-precision forming processing of bearing rollers, automotive parts, aerospace structural parts, precision molds and other fields.
[0003] Currently, the mainstream manufacturing processes for diamond rollers include two main categories: metal sintering and electroplating (internal plating and external plating). Among them, internal plating (random distribution internal plating, UZ method) is the main method for manufacturing high-precision diamond rollers. The basic process route of internal plating is as follows: First, a cavity opposite to the roller profile is machined on a steel or graphite mold using a high-precision forming tool. Diamond abrasive is then solidified on the inner wall of the cavity by electroplating, and a nickel-based plating layer is thickened. Then, a pre-made steel core is assembled with the mold, and a low-melting-point alloy is cast into the cavity between the core and the plating layer. After the alloy cools and solidifies, the mold is removed to expose the diamond, thus obtaining the internally plated diamond roller.
[0004] However, existing methods for manufacturing diamond-plated roller cores still suffer from problems such as insufficient low-temperature alloy interface holding performance, internal air defects, and long core casting times. Commonly used low-temperature alloy cores have low hardness, large internal defects, and require long preheating times for the core cavity, severely restricting processing efficiency and increasing manufacturing costs. For example, utility model patent CN201544125U discloses a thin-walled angled diamond roller. This patent points out that in existing technology, the bonding surfaces between the low-melting-point alloy layer 2, the mandrel 1, and the plating layer 3 are simple. There are no fastening points between the mandrel and the low-melting-point alloy, or between the low-melting-point alloy and the plating layer. When the roller is subjected to rotational force, these two points are prone to detachment. For thin-walled angled rollers, failures such as complete roller detachment and loosening of the connecting layer may occur after 1-2 weeks of use, even before the diamond wears down. For example, the literature "Manufacturing Technology of Diamond Dressing Rollers" points out that when casting low-melting-point alloys, defects such as porosity and shrinkage cavities are easily generated inside the mold cavity due to the limitations of the fluidity and solidification shrinkage characteristics of the alloy melt.
[0005] Therefore, developing an epoxy resin cored diamond roller that can simultaneously achieve high holding strength of the profile and core, low internal defects, high matrix hardness, and high processing efficiency is a core technical challenge that urgently needs to be solved in this field, and has important engineering application value for promoting the quality and efficiency improvement of the precision grinding industry. Summary of the Invention
[0006] This invention addresses the technical problems of existing low-temperature alloy core casting processes for internally plated diamond rollers, such as insufficient interface holding performance, numerous internal pore defects, low matrix hardness, and cumbersome and time-consuming core casting procedures. It proposes a high-interface-low-defect epoxy resin core-cast diamond roller and its preparation method.
[0007] To achieve the above objectives, the technical solution of the present invention is implemented as follows:
[0008] This invention provides a method for preparing a high-interface-area, low-defect epoxy resin cored diamond roller, comprising the following steps:
[0009] (1) The outer circular mating surface of the metal core is machined to form a micro-uneven structure. Then the core is degreased, derusted, rinsed with clean water and dried to obtain a metal core with a roughened surface.
[0010] (2) Process the steel mold according to the roller profile design drawings, and use the internal plating process to complete the nickel-based bonding of diamond abrasive on the inner wall of the mold cavity to form the diamond profile working layer; clean the inner interface of the profile, close the mold and fix the metal core in the center of the mold;
[0011] (3) Take epoxy resin component A and component B, stir and mix them evenly to obtain a glue solution, and after standing, inject the glue solution into the bottom of the mold cavity for self-flowing casting; adopting the "self-flowing casting from bottom to top" method, the glue solution rises steadily, which can orderly discharge the air in the cavity from the top, avoiding the eddies and air bubbles that may be generated by the traditional casting method.
[0012] (4) After casting, the mold is left to stand still and solidify to eliminate internal defects such as porosity and shrinkage cavities to the greatest extent, forming a dense and uniform core layer; after complete demolding, the high interface and low defect epoxy resin core diamond roller is obtained after passing the test.
[0013] The surface roughness after turning in step (1) is Ra0.8-3.2μm. The degreasing is performed by ultrasonic degreasing with anhydrous ethanol for 10-30 min. The drying temperature is 80-100℃ and the drying and holding time is 30-60 min.
[0014] In step (1), a diluted silane coupling agent can also be brushed onto the roughened surface. The silane coupling agent is KH-550 with a mass concentration of 1%-5%.
[0015] In step (2), the coaxiality error after mold closing is ≤0.02mm.
[0016] In step (3), component A is the epoxy resin main agent and component B is the amine mixture curing agent. The mass ratio of components A to B is 2-3:1. The adhesive with this ratio has excellent fluidity and wettability before curing. Under the action of gravity, the highly wettable adhesive can fully penetrate into the micro-grooves of the cavity and metal core and the tiny gaps in the inner wall of the diamond mold. Under this ratio, a three-dimensional network polymer structure with high cross-linking density can be formed, which gives the core layer a hardness and rigidity far greater than that of metal alloys.
[0017] The epoxy resin main agent is a polymer of isopropylidene diphenol and epichlorohydrin, and the effective component of the mixture curing agent is bis(2,1-ethyleneoxy)dipropylamine oxide, with a mass percentage of 30%-50%.
[0018] The curing process in step (4) includes room temperature curing and accelerated curing by heating. The room temperature curing temperature is 23-25℃ and the time is 16-24h, which provides sufficient time for the tiny bubbles remaining in the adhesive to float and escape. The accelerated curing temperature is 60-80℃ and the time is 4-8h.
[0019] The inspection involves sequentially checking the surface contour accuracy, interface bonding strength, core layer hardness, and internal defects.
[0020] This invention provides a high-interface-area, low-defect epoxy resin cored diamond roller prepared using the aforementioned preparation method.
[0021] The diamond roller is coaxially arranged from the inside out, consisting of a metal core, an epoxy resin core-bonding layer, a diamond profile working layer, and a cavity. The epoxy resin core-bonding layer fills the space between the outer wall of the metal core and the inner wall of the diamond profile working layer. Its structural schematic diagram is shown below. Figure 1 As shown, after being uniformly mixed with epoxy resin AB glue, it fills the cavity gaps from bottom to top due to its own fluidity, and forms a dense whole after curing; the glue can fully wet the roughened surface of the metal core and the inner interface of the diamond mold, forming a composite holding structure of "mechanical interlocking + adhesive force" after curing, with a strong bond and very few defects.
[0022] The beneficial effects of this invention are:
[0023] 1. This invention uses epoxy resin AB glue as the core bonding layer material. After mixing, it has excellent fluidity and wettability, and can fully penetrate into the roughened uneven structure of the metal core and the micro gaps of the diamond profile. After curing, it forms a composite holding structure with mechanical interlocking and adhesive force working together. Compared with the traditional low-temperature alloy core casting which only relies on the single mechanical interlocking effect formed by alloy cooling and solidification, the interface bonding strength of this invention is significantly improved. It can effectively avoid problems such as profile debonding, edge chipping, and block falling off under high-speed and high-load operation conditions, and the service life of the roller is greatly extended. It is especially suitable for batch precision grinding processing scenarios with high precision and high reliability requirements.
[0024] 2. Epoxy resin AB adhesive possesses excellent self-leveling and filling properties, capable of fully filling every tiny corner of the cavity. Combined with a post-pouring venting process, it effectively removes air bubbles from within the adhesive and at the interfaces. Simultaneously, the curing shrinkage rate of epoxy resin is far lower than that of traditional low-temperature alloys, resulting in minimal volume change during curing. This effectively eliminates internal defects such as pores, shrinkage cavities, and looseness, ensuring a dense, uniform, and consistent hardness of the core-cast bonding layer. The stable rigid support of the core-cast layer guarantees the long-term maintenance of the roller profile accuracy, consistently meeting high-precision machining requirements.
[0025] 3. This invention completely eliminates the series of cumbersome processes required by traditional low-temperature alloy core casting processes, such as high-temperature cavity preheating, metal melting, high-temperature casting, and long-term heat preservation and cooling. It eliminates the need for specialized high-temperature casting equipment; only room-temperature mixed adhesive is required, and self-leveling is sufficient for casting and filling. Curing conditions are flexible (it can cure naturally at room temperature or be accelerated by heating), reducing the cycle time for a single batch of core casting by more than 40%. Simultaneously, the cost of epoxy resin raw materials is far lower than that of special low-temperature alloys, and equipment investment and energy consumption are also significantly reduced, resulting in a substantial decrease in overall manufacturing costs. It is easy to operate and has low requirements for the working environment, making it highly valuable for industrial promotion and engineering applications. Attached Figure Description
[0026] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0027] Figure 1 It has a diamond roller structure.
[0028] Figure 2 This is the curing curve of the epoxy resin.
[0029] Figure 3 This is a schematic diagram of self-flowing casting.
[0030] Figure 4 Image of the high-interface-area, low-defect epoxy resin cored diamond roller prepared in Example 1.
[0031] Figure 5 Image of a diamond-plated roller cast from a low-temperature alloy prepared for Comparative Example 1. Detailed Implementation
[0032] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0033] Example 1
[0034] A method for preparing a high-interface-area, low-defect epoxy resin cored diamond roller, the specific steps of which are as follows:
[0035] (1) The outer cylindrical mating surface of the 45# steel core is machined to control the roughness Ra0.8, ultrasonically degreased with anhydrous ethanol for 10 min, rinsed with water and dried at 100℃; then coated with 2% KH-550 silane coupling agent dilution and air-dried at room temperature to obtain the pretreated metal core.
[0036] (2) Process a high-precision steel mold according to the bearing roller drawings, and use conventional internal plating process to solidify 3035 grade artificial diamond abrasive on the inner wall of the cavity to form a diamond surface working layer; use anhydrous ethanol to clean the inner interface of the surface to remove oil and impurities; after the mold is closed, fix the pre-treated metal core to ensure that the coaxiality error is ≤0.02mm.
[0037] (3) Weigh 100g of epoxy resin component A (polymer of isopropylidene diphenol and epichlorohydrin) and 46g of component B (a mixture of curing agent with a mass ratio of 30% of [bis(2,1-ethyleneoxy)] dipropylamine), stir at room temperature for 3 minutes until the mixture is uniform, let stand for 2 minutes to remove air bubbles; slowly inject the adhesive into the bottom gate of the mold, and the adhesive fills the gap between the core and the mold surface by its own flow until the adhesive overflows from the gate;
[0038] (4) After casting, let it stand at room temperature (25°C) for 24 hours to cure. Keep the mold horizontal and stationary throughout the curing process to avoid vibration. After demolding, grind the inner hole, end faces and outer circle, correct the dynamic balance, and test the surface accuracy, bonding strength and hardness. After passing the test, a high interface and low defect epoxy resin core diamond roller is obtained.
[0039] The epoxy resin curing curve described in this invention is as follows: Figure 2As shown, the adhesive reacts slowly at room temperature, allowing bubbles to escape fully. Over time, the bonding strength of the epoxy resin increases exponentially. This process can significantly improve production efficiency and is simpler to operate, requiring no high-temperature equipment.
[0040] This embodiment uses an epoxy resin self-flowing casting core. A schematic diagram of the self-flowing casting is shown below. Figure 3 As shown, the adhesive's own fluidity allows it to fully wet the roughened surface of the metal core and the inner wall of the diamond layer, effectively reducing interfacial porosity defects.
[0041] The high-interface-area, low-defect epoxy resin cored diamond roller product prepared in this embodiment is as follows: Figure 4 As shown, the interfaces of each layer of the roller are tightly bonded, with no obvious delamination, pores, cracks or other defects. The overall coaxiality is good, which meets the requirements for use in precision dressing grinding wheels.
[0042] Example 2
[0043] A method for preparing a high-interface-area, low-defect epoxy resin cored diamond roller, the specific steps of which are as follows:
[0044] (1) The outer cylindrical mating surface of the 45# steel core was machined to control the roughness Ra1.6 μm. It was ultrasonically degreased with anhydrous ethanol for 20 min, rinsed with water and dried at 90℃. It was then coated with a 3% KH-550 silane coupling agent dilution solution and air-dried at room temperature to obtain the pretreated metal core.
[0045] (2) Process a high-precision steel mold according to the bearing roller drawings, and use conventional internal plating process to solidify 3035 grade artificial diamond abrasive on the inner wall of the cavity to form a diamond surface working layer; use anhydrous ethanol to clean the inner interface of the surface to remove oil and impurities; after mold closing, fix the pre-treated metal core and control the coaxiality error ≤0.02 mm.
[0046] (3) Weigh 100 g of epoxy resin component A (polymer of isopropylidene diphenol and epichlorohydrin) and 44 g of component B (a mixture of curing agent with 50% mass of [bis(2,1-ethyleneoxy)] dipropylamine), stir at room temperature for 3 min until uniformly mixed, let stand for 2 min to remove air bubbles; slowly inject the adhesive into the bottom gate of the mold, the adhesive fills the gap between the core and the mold surface by its self-flowing nature until the gate overflows;
[0047] (4) After casting, the mold is kept in a static state at 25°C for 20 hours to pre-cur. The mold is kept horizontal and stationary throughout the process to avoid vibration. After demolding, the inner hole, end faces and outer circle are finely ground, the dynamic balance is corrected, and the high interface and low defect epoxy resin core diamond roller is obtained after passing the inspection.
[0048] Example 3
[0049] A method for preparing a high-interface-area, low-defect epoxy resin cored diamond roller, the specific steps of which are as follows:
[0050] (1) The outer cylindrical mating surface of the 45# steel core was machined to control the roughness Ra3.2 μm, ultrasonically degreased with anhydrous ethanol for 30 min, rinsed with water and dried at 80℃; then coated with 5% KH-550 silane coupling agent dilution and air-dried at room temperature to obtain the pretreated metal core.
[0051] (2) Process a high-precision steel mold according to the bearing roller drawings, and use conventional internal plating process to solidify 3035 grade artificial diamond abrasive on the inner wall of the cavity to form a diamond surface working layer; use anhydrous ethanol to clean the inner interface of the surface to remove oil and impurities; after mold closing, fix the pre-treated metal core and control the coaxiality error ≤0.02 mm.
[0052] (3) Weigh 100 g of epoxy resin component A (polymer of isopropylidene diphenol and epichlorohydrin) and 50 g of component B (a mixture of curing agent with a mass ratio of 40% of [bis(2,1-ethyleneoxy)] dipropylamine), stir at room temperature for 3 min until uniformly mixed, let stand for 2 min to remove air bubbles; slowly inject the adhesive into the bottom gate of the mold, and the adhesive fills the gap between the core and the mold surface by its self-flowing properties until the adhesive overflows from the gate;
[0053] (4) After casting, the mold is kept in a static state at 25°C for 16 hours to pre-cur. The mold is kept horizontal and stationary throughout the process to avoid vibration. After demolding, the inner hole, end faces and outer circle are finely ground, the dynamic balance is corrected, and the high interface and low defect epoxy resin core diamond roller is obtained after passing the inspection.
[0054] Comparative Example
[0055] A method for preparing a low-temperature alloy cast diamond-plated roller, the specific steps of which are as follows:
[0056] (1) Select a 45# steel core of the same specifications as in the example, machine its shape, clean and dry it with anhydrous ethanol for later use; prepare a steel mold with a 3035 grade diamond working layer using the same process.
[0057] (2) Heat the tin-based low-temperature alloy ingot to 200 °C until it is completely melted; preheat the metal core and mold to 160 °C; pour the molten alloy liquid into the mold cavity, keep it at the temperature for 12 hours and then slowly cool it to room temperature to solidify;
[0058] (3) After demolding, the roller is finely ground and the dynamic balance is corrected to obtain a low-temperature alloy cast diamond-plated roller.
[0059] The low-temperature alloy cast diamond-plated roller prepared in this comparative example is as follows: Figure 5 As shown, the low-temperature alloy core casting process involves significant cooling shrinkage, and micro-gaps and shrinkage cavities are prone to occur at the interfaces between the alloy and the metal core, as well as the inner wall of the diamond.
[0060] Example of implementation effect 1
[0061] The performance of the high-interface-area, low-defect epoxy resin cored diamond rollers prepared in Examples 1-3 and the low-temperature alloy cast diamond-plated rollers prepared in the comparative example were tested, and the results are shown in Table 1:
[0062] Table 1. Comparison of Performance of Samples in Each Group
[0063]
[0064] As can be seen from the data in Table 1:
[0065] Compared to traditional cryogenic alloy casting methods, the rollers prepared in Examples 1-3 of this invention exhibit an interface shear strength increase of over 35%, resulting in significantly better holding performance. The internal defect rate is reduced to below 0.5%, far lower than the defect level of cryogenic alloy casting, leading to more stable molding quality. Traditional cryogenic alloy core substrates have a Brinell hardness of only 17-35 HB, making them relatively soft and lacking in deformation resistance. The epoxy resin AB adhesive used in this invention achieves a Shore hardness of 75-85 HD after curing, significantly improving the substrate's load-bearing capacity and deformation resistance.
[0066] Furthermore, comparing Examples 1-3 reveals that products with low defects and high interfacial bonding performance can be obtained within the process parameter range defined in the claims; among them, Example 1, which uses the optimal ratio of 100:46 and a coupling agent concentration of 2%, exhibits the best overall performance.
[0067] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for preparing a high-interface-area, low-defect epoxy resin cored diamond roller, characterized in that, Includes the following steps: (1) The outer circular mating surface of the metal core is machined, and then the core is degreased, derusted, rinsed with clean water and dried to obtain a roughened metal core. (2) Process the steel mold according to the roller profile design drawings, and use the internal plating process to complete the nickel-based bonding of diamond abrasive on the inner wall of the mold cavity to form the diamond profile working layer; clean the inner interface of the profile, close the mold and fix the metal core in the center of the mold; (3) Take epoxy resin component A and component B, stir and mix them evenly to obtain a glue solution, let it stand, and then inject the glue solution into the bottom of the mold cavity for self-flowing casting. (4) After casting, the mold is left to stand still for curing and molding. After complete demolding, the high interface low defect epoxy resin core diamond roller is obtained after passing the test.
2. The method for preparing the high-interface-area, low-defect epoxy resin cored diamond roller according to claim 1, characterized in that: The surface roughness after turning in step (1) is Ra0.8-3.2μm. The degreasing is performed by ultrasonic degreasing with anhydrous ethanol for 10-30 min. The drying temperature is 80-100℃ and the drying and holding time is 30-60 min.
3. The method for preparing the high-interface-area, low-defect epoxy resin cored diamond roller according to claim 2, characterized in that: In step (1), a diluted silane coupling agent may also be brushed onto the roughened surface, wherein the mass concentration of the silane coupling agent is 1%-5%.
4. The method for preparing the high-interface-area, low-defect epoxy resin cored diamond roller according to claim 3, characterized in that: In step (2), the coaxiality error after mold closing is ≤0.02mm.
5. The method for preparing the high-interface-area, low-defect epoxy resin cored diamond roller according to claim 4, characterized in that: In step (3), component A is the epoxy resin main agent and component B is the mixed curing agent. The mass ratio of components A to B is 2-3:
1.
6. The method for preparing the high-interface-area, low-defect epoxy resin cored diamond roller according to claim 5, characterized in that: In step (3), the epoxy resin main agent is a polymer of isopropylidene diphenol and epichlorohydrin, and the effective component of the mixture curing agent is [bis(2,1-ethyleneoxy)]dipropylamine, with a mass percentage of 30%-50%.
7. The method for preparing the high-interface-area, low-defect epoxy resin cored diamond roller according to claim 6, characterized in that: The curing process in step (4) includes room temperature curing and accelerated curing by heating. The room temperature curing temperature is 23-25℃ and the time is 16-24h. The accelerated curing temperature is 60-80℃ and the time is 4-8h.
8. The method for preparing the high-interface-area, low-defect epoxy resin cored diamond roller according to claim 7, characterized in that: In step (4), the detection involves sequentially detecting the surface contour accuracy, interface bonding strength, core layer hardness, and internal defects.
9. A high-interface-area, low-defect epoxy resin cored diamond roller prepared by the preparation method according to any one of claims 1-8.
10. The high-interface-area, low-defect epoxy resin cored diamond roller according to claim 9, characterized in that: The diamond roller is coaxially arranged from the inside out with a metal core, an epoxy resin core bonding layer, a diamond profile working layer, and a cavity. The epoxy resin core bonding layer fills the space between the outer wall of the metal core and the inner wall of the diamond profile working layer.