A method for preparing glass fiber composite insulating components for high-voltage fuses

By optimizing the processes of modified glass fiber cloth, wound buffer resin, and impregnated resin, as well as plasma activation treatment, the problems of weak interfacial bonding and lack of stress buffering in the interlayer structure of glass fiber composite insulating components for high-voltage fuses have been solved, improving the mechanical and insulating properties of the material, especially its protective ability in humid and polluted environments.

CN123104104APending Publication Date: 2026-11-17HANGZHOU SUPERFUSE TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611258846.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-19
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing glass fiber composite insulation components for high-voltage fuses have shortcomings in terms of weak interfacial bonding, lack of stress buffering in interlayer structure, and surface protection, which leads to a decline in mechanical and insulation performance. In particular, creepage or flashover is prone to occur in humid and dirty environments.

Method used

By optimizing the preparation of modified glass fiber cloth, the winding and impregnation processes of buffer resin, and the application of plasma activation treatment and protective coating, the bonding between fiber and resin interface is enhanced, the interlayer stress distribution is optimized, and the protective capability of the outer wall is improved.

Benefits of technology

It significantly enhances the chemical bonding between fibers and resins, strengthens the flexural and tensile strength of composite materials, improves arc resistance and structural integrity, and enhances weather resistance in harsh environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure REF-OBJ-1787120657371-000001
    Figure REF-OBJ-1787120657371-000001
Patent Text Reader

Abstract

This invention discloses a method for preparing glass fiber composite insulating components for high-voltage fuses, relating to the field of electrical insulation materials technology. The preparation method includes: firstly, preparing modified glass fiber cloth, buffer resin, and impregnating resin; then, alternately winding the modified glass fiber cloth onto a mold core and roller-coating the buffer resin to the designed wall thickness; introducing the impregnating resin after negative pressure venting, and impregnating under pressure in a nitrogen atmosphere; curing in stages; after demolding, plasma activation treatment of the outer wall and spraying a protective coating, followed by curing to obtain the finished product. This invention, through high-temperature heat treatment and coupling agent modification of the glass fiber cloth, combined with the gradient structure of the interlayer buffer resin and impregnating resin, and supplemented by plasma activation and coating treatment of the outer wall, effectively improves the mechanical strength and arc resistance of the insulating components. The product has excellent comprehensive performance and is suitable for high-voltage power systems.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of electrical insulation materials technology, specifically relating to a method for preparing glass fiber composite insulating components for high-voltage fuses. Background Technology

[0002] High-voltage fuses, as crucial protective devices in power systems, are widely used in transmission and distribution lines and various electrical equipment. The performance of their core insulating components directly affects the safety and reliability of the equipment. Glass fiber reinforced composite materials, due to their excellent electrical insulation, mechanical strength, and heat resistance, have gradually become one of the preferred materials for high-voltage fuse insulation tubing. However, with the development of power systems towards higher voltage and larger capacity, higher requirements are placed on the comprehensive performance of insulating components, especially in terms of arc resistance, interlaminar bond strength, and environmental adaptability.

[0003] Currently, the traditional manufacturing process for glass fiber composite insulation components mostly involves winding molding followed by resin impregnation and thermosetting. However, in practical applications, pipes produced by this process often have the following shortcomings: First, the interfacial bonding between the glass fiber and the resin matrix is ​​weak. Under long-term electrical and mechanical stress, problems such as interfacial debonding and microcrack propagation easily occur, leading to a significant decrease in mechanical and insulation properties. Second, the interlayer structure lacks reasonable stress buffering. The internal stress generated during curing due to resin shrinkage and differences in thermal expansion coefficients is difficult to release effectively, easily causing delamination defects and affecting the overall structural integrity. Third, the surface energy of the outer wall of the pipe is low, resulting in insufficient adhesion of subsequent coatings. In harsh environments such as humidity and dirt, surface creep or flashover phenomena easily occur, shortening the product's service life.

[0004] To address the aforementioned issues, existing technologies have implemented measures such as modifying fibers with coupling agents, optimizing resin formulations, or adding protective coatings. However, most of these measures only improve single properties and fail to provide systematic and synergistic optimization from multiple dimensions, including material interfaces, interlayer structures, and surface protection. Furthermore, in existing preparation processes, problems such as insufficient resin wetting and unreasonable curing regimes remain prominent, hindering further improvements in the overall performance of the product.

[0005] Therefore, this invention provides a method for preparing glass fiber composite insulating components that can effectively improve fiber-resin interface bonding, optimize interlayer stress distribution, and enhance the outer wall protection capability, which has significant application value and market prospects. Summary of the Invention

[0006] The purpose of this invention is to provide a method for preparing glass fiber composite insulating components for high-voltage fuses. The insulating components prepared by this method have good arc resistance and mechanical properties.

[0007] The technical solution adopted by the present invention to achieve the above objectives is as follows: A method for preparing a glass fiber composite insulating component for a high-voltage fuse, comprising: Step 1: Prepare modified glass fiber cloth, buffer resin, and impregnation resin separately; Step 2: Wrap 2-3 layers of modified glass fiber cloth around the mold core with a winding tension of 75-85N. After winding, uniformly roll-coat the buffer resin with a coating thickness of 0.02-0.025mm. Repeat the above operation until the designed wall thickness is achieved. After completion, wrap the outermost layer with another layer of modified glass fiber cloth with a winding tension of 38-42N. Step 3: Place the resin in an impregnation tank and evacuate the air between the fibers under negative pressure for 18-22 minutes at -0.09MPa to -0.095MPa. Then, introduce the impregnation resin until the fibers are completely submerged. In a nitrogen atmosphere, maintain the pressure at 0.5-0.8MPa and 43-47℃ for 35-45 minutes. Then, release the pressure and recover the filtered impregnation resin. Step 4: Curing at 75-85℃ for 8-12 minutes, curing at 125-130℃ for 25-30 minutes, curing at 160-165℃ for 35-40 minutes, then naturally cooling to 60℃ and removing. Step 5: Remove the mold core, take out the tube, and perform plasma activation treatment on the outer wall. The power is 280-320W, the compressed air flow rate is 18-22L / min, and the activation time is 60-90s. Then, spray a protective coating on the outer wall of the tube. After spraying, let it stand at room temperature for 18-25min, and then cure it at a constant temperature of 95-100℃ for 55-70min to obtain the glass fiber composite insulation component for high voltage fuses.

[0008] Preferably, the wall thickness in step one above is designed to be 6-7 mm.

[0009] Preferably, the dry film thickness after spraying in step five above is 15-30 μm.

[0010] This invention also discloses a method for preparing modified glass fiber cloth, comprising: adding deionized water to anhydrous ethanol, then adding glacial acetic acid to adjust the pH to 4-5, adding γ-glycidoxypropyltrimethoxysilane, and stirring at room temperature for 25-35 min at a speed of 180-220 r / min to obtain a hydrolytic coupling solution; laying a single layer of glass fiber cloth flat, then heating it to 440-460℃ at a rate of 3-5℃ / min and keeping it at that temperature in air for 3.5-4.5 h; then naturally cooling it to 75-85℃ and removing it, then immersing the glass fiber cloth in the hydrolytic coupling solution, letting it stand for 25-35 min, then removing it and draining it, drying it at room temperature for 12-18 min, and then drying it at 115-125℃ for 25-35 min to obtain modified glass fiber cloth.

[0011] Preferably, the glass fiber cloth has a strength of 200 g / m². 2 Plain weave alkali-free fiberglass cloth, with a single filament diameter of 9μm.

[0012] Preferably, by weight, the amount of anhydrous ethanol is 93-97 parts, the amount of deionized water is 4-6 parts, and the amount of γ-glycidyl etheroxypropyltrimethoxysilane is 0.02-0.03 parts.

[0013] This invention also discloses a method for preparing a buffer resin or impregnating resin: Nano-silica and hexagonal boron nitride are dried at 95-105℃ for 2-2.5 hours, then anhydrous ethanol and γ-glycidoxypropyltrimethoxysilane are added and stirred into a slurry. The slurry is allowed to stand for 15-20 minutes to obtain a coupling agent-coated filler. Epoxy resin is preheated to 40-45℃ and stirred at 200-300 r / min for 4-6 minutes. The coupling agent-coated filler is added in 3-4 batches, and after each batch, the mixture is stirred at 280-320 r / min for 8-15 minutes. After 12 minutes, once the filler has been added, stir and disperse it at 110-125 r / min for 25-35 minutes. Then grind it until the filler particle size is ≤2μm. At 35-40℃, add the curing agent, toughening agent, and silicone defoamer in sequence, and stir at 350-450 r / min for 4-6 minutes. Perform segmented vacuum degassing. The first segment is held at -0.08MPa and 38-40℃ for 8-12 minutes, and the second segment is held at -0.095MPa and 43-47℃ for 28-32 minutes. Set aside for later use.

[0014] Preferably, the buffer resin comprises, by weight, 68-72 parts epoxy resin, 16-20 parts curing agent, 7-7.5 parts nano silica, 5-5.5 parts hexagonal boron nitride, 0.8-1.2 parts γ-glycidyl etheroxypropyltrimethoxysilane, 2-3 parts anhydrous ethanol, 4-6 parts toughening agent, and 0.4-0.6 parts silicone defoamer.

[0015] Preferably, in the above-mentioned impregnating resin, by weight, there are 68-72 parts of epoxy resin, 16-20 parts of curing agent, 4.5-5 parts of nano-silica, 3.5-4 parts of hexagonal boron nitride, 0.8-1.2 parts of γ-glycidyl etheroxypropyltrimethoxysilane, 2-3 parts of anhydrous ethanol, 4-6 parts of toughening agent, and 0.4-0.6 parts of silicone defoamer.

[0016] Preferably, the curing agent comprises diaminodiphenylmethane; Toughening agents include carboxyl-terminated butadiene-acrylonitrile rubber; Organosilicon defoamers include epoxy-modified polysiloxanes.

[0017] This invention also discloses a method for preparing a protective coating, comprising: drying nano-silica and wollastonite at 95-105℃ for 1.5-2.5h; sequentially adding UV shielding agent, leveling agent, and coating defoamer to the coating matrix resin, stirring continuously at 180-220r / min for 8-15min, adding nano-silica and wollastonite, stirring at 750-850r / min for 18-25min, then ultrasonically treating at room temperature with a power of 280-320W for 55-65min, pausing for 3min every 15min of ultrasonic treatment, and then continuously stirring at 180-220r / min, adding anhydrous ethanol to adjust the viscosity, stirring evenly, and letting stand for 8-15min for later use. The viscosity of the coating is tested by the flow time of a Cot-4 viscosity cup at 25℃ and controlled within 18-22s.

[0018] By weight, the composition includes 7-9 parts nano-silica, 3-5 parts wollastonite, 95-105 parts coating matrix resin, 1-1.5 parts UV shielding agent, 0.5-0.7 parts leveling agent, and 0.25-0.35 parts coating defoamer.

[0019] Preferably, the particle size of the wollastonite is 80-125 μm; Preferably, the ultraviolet shielding agent includes 2-hydroxy-4-n-octyloxybenzophenone; Leveling agents include polyacrylate leveling agents; Paint defoamers include polyether-modified polysiloxanes.

[0020] The present invention also discloses a method for preparing a coating matrix resin, comprising: adding a mixed solvent to an epoxy resin, treating it at 280-350 r / min and 80-85℃ for 18-23 min, adding dibutyltin dilaurate, dispersing it evenly for 4-6 min, adding methylphenyl polysiloxane at a uniform rate, controlling the addition time at 80-100 min, maintaining the temperature at 80-85℃ throughout the process, raising the temperature to 130-140℃ and holding it for 2.5-3.5 h after completion, cooling to 90℃, distilling under reduced pressure at -0.08 MPa for 1.5 h, and cooling to room temperature to obtain the coating matrix resin.

[0021] Preferably, the above-mentioned components, by weight, consist of 72-78 parts epoxy resin, 23-27 parts mixed solvent, 0.35-0.45 parts dibutyltin dilaurate, and 23-28 parts methylphenyl polysiloxane.

[0022] The mixed solvent consists of xylene and n-butanol; the volume ratio of xylene to n-butanol is 1:0.4-0.45.

[0023] Preferably, all of the above-mentioned epoxy resins are hydrogenated bisphenol A type epoxy resins.

[0024] A glass fiber composite insulating component is prepared by the above-described preparation method.

[0025] This invention provides a method for preparing glass fiber composite insulating components for high-voltage fuses, which has the following beneficial effects: First, by performing high-temperature thermal cleaning and silane coupling agent grafting modification on the glass fiber cloth, impurities on the fiber surface are effectively removed and active functional groups are introduced, which significantly enhances the chemical bonding between the fiber and the resin matrix and greatly improves the interfacial bonding strength, thereby giving the composite material excellent flexural strength and tensile strength.

[0026] Secondly, a buffer resin with a high filler content is introduced during the interlayer winding process, forming a performance gradient structure with the subsequent impregnation resin with a lower filler content. This buffer layer can effectively transfer and alleviate interlayer thermal shrinkage and curing stress, inhibit the initiation and propagation of microcracks, and enhance the insulation barrier effect, significantly improving the arc resistance and structural integrity of the product.

[0027] Third, after curing, the outer wall of the pipe is subjected to plasma activation treatment to increase the surface polar groups, improve the wettability and adhesion of the coating, and then a protective coating is used to form a dense protective layer, which effectively improves the weather resistance of the insulating components in harsh environments such as humidity.

[0028] In summary, this invention achieves synergistic improvements from three aspects: interface enhancement, interlayer structure optimization, and surface protection. The resulting insulating component exhibits excellent overall performance and has promising prospects for widespread application. Detailed Implementation

[0029] To make the objectives, technical solutions, and advantages of the present invention clearer, the technical solutions of the present invention will be further described in detail below with reference to specific embodiments: Fiberglass cloth is 200g / m 2 Plain weave alkali-free fiberglass cloth, with a single filament diameter of 9μm; The particle size of wollastonite is 100 μm; All epoxy resins were hydrogenated bisphenol A type epoxy, purchased from Suzhou Senfida Chemical Co., Ltd.

[0030] Example 1:

[0031] A method for preparing a glass fiber composite insulating component for a high-voltage fuse, comprising: Step 1: Prepare modified glass fiber cloth, buffer resin, and impregnation resin separately; Step 2: Wrap two layers of modified glass fiber cloth around the mold core with a winding tension of 75N. After winding, uniformly roll-coat the buffer resin with a coating thickness of 0.02mm. Repeat the above operation until the designed wall thickness of 6.5mm is achieved. After completion, wrap the outermost layer with another layer of modified glass fiber cloth with a winding tension of 38N. Step 3: Place the resin in the impregnation tank, and under negative pressure, continuously pump air for 22 minutes at -0.09MPa to remove air from the gaps between the fibers. Introduce the impregnation resin until completely submerged. Under nitrogen atmosphere, maintain pressure at 0.5MPa and 43℃ for 45 minutes. Depressurize and recover the filtered impregnation resin. Step 4: Curing at 75℃ for 12 minutes, at 125℃ for 30 minutes, and at 160℃ for 40 minutes; then allowing to cool naturally to 60℃ before removing. Step 5: Remove the mold core, take out the tube, and perform plasma activation treatment on the outer wall. The power is 280W, the compressed air flow rate is 22L / min, and the activation time is 60s. Then, spray a protective coating on the outer wall of the tube. After spraying, let it stand at room temperature for 18min, and then cure it at 95℃ for 70min. The dry film thickness after spraying is 15μm, and the glass fiber composite insulation component for high voltage fuses is obtained.

[0032] A method for preparing modified glass fiber cloth includes: adding deionized water to anhydrous ethanol, then adding glacial acetic acid to adjust the pH to 4, adding γ-glycidoxypropyltrimethoxysilane, and stirring at room temperature for 35 min at 180 r / min to obtain a hydrolytic coupling solution. A single layer of glass fiber cloth is laid flat, and then heated to 440℃ at a rate of 3℃ / min and kept at that temperature in air for 4.5 h; then naturally cooled to 85℃ and removed. The glass fiber cloth is then immersed in the hydrolytic coupling solution, allowed to stand for 25 min, drained, dried at room temperature for 12 min, and then dried at 115℃ for 35 min to obtain the modified glass fiber cloth. By weight, the amount of anhydrous ethanol is 93 parts, the amount of deionized water is 4 parts, and the amount of γ-glycidoxypropyltrimethoxysilane is 0.02 parts.

[0033] A method for preparing a buffer resin or impregnating resin: Nano-silica and hexagonal boron nitride are dried at 95°C for 2.5 h, then anhydrous ethanol and γ-glycidyl etheroxypropyltrimethoxysilane are added and stirred into a slurry. After standing for 15 min, a coupling agent-coated filler is obtained. Epoxy resin is preheated to 40°C and stirred at 200 r / min for 6 min. The coupling agent-coated filler is added in 3 batches, and after each batch is added, the mixture is stirred at 280 r / min for 12 min. After the addition is complete, the mixture is stirred at 110 r / min. Stir and disperse for 35 min, then grind until the filler particle size is ≤2μm. At 35℃, add curing agent diaminodiphenylmethane, toughening agent carboxyl-terminated nitrile rubber, and organosilicon defoamer epoxy-modified polysiloxane (purchased from Hubei Longsheng Sihai New Material Co., Ltd.) in sequence. Stir at 350 r / min for 6 min, and perform segmented vacuum degassing. The first segment is set at -0.08 MPa and 38℃ and allowed to stand for 12 min. The second segment is set at -0.095 MPa and 43℃ and allowed to stand for 32 min.

[0034] The buffer resin contains, by weight, 68 parts epoxy resin, 16 parts curing agent, 7 parts nano silica, 5 parts hexagonal boron nitride, 0.8 parts γ-glycidyl etheroxypropyltrimethoxysilane, 2 parts anhydrous ethanol, 4 parts toughening agent, and 0.4 parts silicone defoamer.

[0035] The resin impregnation mixture contains, by weight, 68 parts epoxy resin, 16 parts curing agent, 4.5 parts nano silica, 3.5 parts hexagonal boron nitride, 0.8 parts γ-glycidyl etheroxypropyltrimethoxysilane, 2 parts anhydrous ethanol, 4 parts toughening agent, and 0.4 parts silicone defoamer.

[0036] A method for preparing a protective coating includes: drying nano-silica and wollastonite at 95°C for 2.5 hours; sequentially adding UV shielding agent 2-hydroxy-4-n-octyloxybenzophenone, polyacrylate leveling agent, and coating defoamer polyether-modified polysiloxane (purchased from Hubei Longsheng Sihai New Material Co., Ltd.) to the coating matrix resin, stirring continuously at 180 r / min for 15 minutes, adding nano-silica and wollastonite, stirring at 750 r / min for 25 minutes, then ultrasonically treating at room temperature with a power of 280 W for 65 minutes, pausing for 3 minutes every 15 minutes of ultrasonic treatment, and then continuously stirring at 180 r / min, adding anhydrous ethanol to adjust the viscosity, stirring evenly, and letting stand for 8 minutes for later use. The viscosity of the coating is tested by the flow time of a Ford-4 viscosity cup at 25°C and controlled to be within 18 seconds. By weight, the composition includes 7 parts nano-silica, 3 parts wollastonite, 95 parts coating matrix resin, 1 part UV shielding agent, 0.5 parts leveling agent, and 0.25 parts coating defoamer.

[0037] A method for preparing a coating matrix resin includes: adding a mixed solvent to an epoxy resin, treating it at 280 r / min and 80℃ for 23 min, adding dibutyltin dilaurate, dispersing it uniformly for 4 min, adding methylphenyl polysiloxane at a uniform rate for 80 min, maintaining the temperature at 80℃ throughout, raising the temperature to 130℃ and holding it for 3.5 h, cooling to 90℃, distilling under reduced pressure at -0.08 MPa for 1.5 h, and cooling to room temperature to obtain the coating matrix resin. By weight, the epoxy resin comprises 72 parts, the mixed solvent 23 parts, dibutyltin dilaurate 0.35 parts, and methylphenyl polysiloxane 23 parts. The mixed solvent consists of xylene and n-butanol; the volume ratio of xylene to n-butanol is 1:0.4.

[0038] Example 2:

[0039] A method for preparing a glass fiber composite insulating component for a high-voltage fuse, comprising: Step 1: Prepare modified glass fiber cloth, buffer resin, and impregnation resin separately; Step 2: Wrap two layers of modified glass fiber cloth around the mold core with a winding tension of 85N. After winding, uniformly roll-coat the buffer resin with a coating thickness of 0.025mm. Repeat the above operation until the designed wall thickness of 6.5mm is achieved. After completion, wrap the outermost layer with another layer of modified glass fiber cloth with a winding tension of 42N. Step 3: Place the resin in the impregnation tank and evacuate the air between the fibers under negative pressure for 18 minutes at -0.095MPa. Then, introduce the impregnation resin until the fibers are completely submerged. In a nitrogen atmosphere, maintain the pressure at 0.8MPa and 47℃ for 35 minutes. Then, release the pressure and recover the filtered impregnation resin. Step 4: Curing at 85℃ for 8 minutes, curing at 130℃ for 25 minutes, and curing at 165℃ for 35 minutes, then allowing to cool naturally to 60℃ before removing. Step 5: Remove the mold core, take out the tube, and perform plasma activation treatment on the outer wall. The power is 320W, the compressed air flow rate is 22L / min, and the activation time is 60s. Then, spray a protective coating on the outer wall of the tube. After spraying, let it stand at room temperature for 25min, and then cure it at 100℃ for 55min. The thickness of the dry film after spraying is 30μm, and the glass fiber composite insulation component for high voltage fuses is obtained.

[0040] A method for preparing modified glass fiber cloth includes: adding deionized water to anhydrous ethanol, then adding glacial acetic acid to adjust the pH to 5, adding γ-glycidoxypropyltrimethoxysilane, and stirring at room temperature for 25 min at 220 r / min to obtain a hydrolytic coupling solution. A single layer of glass fiber cloth is laid flat, and then heated to 460℃ at a rate of 5℃ / min and kept at that temperature in air for 3.5 h; then naturally cooled to 85℃ and removed. The glass fiber cloth is then immersed in the hydrolytic coupling solution, allowed to stand for 35 min, drained, dried at room temperature for 18 min, and then dried at 125℃ for 25 min to obtain the modified glass fiber cloth. By weight, the amount of anhydrous ethanol is 97 parts, the amount of deionized water is 6 parts, and the amount of γ-glycidoxypropyltrimethoxysilane is 0.03 parts.

[0041] A method for preparing a buffer resin or impregnating resin: Nano-silica and hexagonal boron nitride are dried at 105℃ for 2 hours, then anhydrous ethanol and γ-glycidyl etheroxypropyltrimethoxysilane are added and stirred into a slurry. The slurry is allowed to stand for 20 minutes to obtain a coupling agent-coated filler. Epoxy resin is preheated to 45℃ and stirred at 300 r / min for 4 minutes. The coupling agent-coated filler is added in 4 batches, with stirring at 320 r / min for 8 minutes after each batch. After the addition is complete, the mixture is stirred at 12... Stir and disperse at 5 r / min for 25 min, then grind until the filler particle size is ≤2 μm. At 40℃, add curing agent diaminodiphenylmethane, toughening agent terminal carboxyl nitrile rubber, and organosilicon defoamer epoxy-modified polysiloxane in sequence. Stir at 450 r / min for 4 min, and degas in stages under vacuum. The first stage is set at -0.08 MPa and 40℃ for 8 min, and the second stage is set at -0.095 MPa and 47℃ for 28 min.

[0042] The buffer resin contains, by weight, 72 parts epoxy resin, 20 parts curing agent, 7.5 parts nano silica, 5.5 parts hexagonal boron nitride, 1.2 parts γ-glycidyl etheroxypropyltrimethoxysilane, 3 parts anhydrous ethanol, 6 parts toughening agent, and 0.6 parts silicone defoamer.

[0043] The resin impregnation mixture contains, by weight, 72 parts epoxy resin, 20 parts curing agent, 5 parts nano silica, 4 parts hexagonal boron nitride, 1.2 parts γ-glycidyl etheroxypropyltrimethoxysilane, 3 parts anhydrous ethanol, 6 parts toughening agent, and 0.6 parts silicone defoamer.

[0044] A method for preparing a protective coating includes: drying nano-silica and wollastonite at 105°C for 1.5 h; sequentially adding UV shielding agent 2-hydroxy-4-n-octyloxybenzophenone, polyacrylate leveling agent, and coating defoamer polyether-modified polysiloxane to the coating matrix resin, stirring continuously at 220 r / min for 8 min; adding nano-silica and wollastonite, stirring at 850 r / min for 18 min; then ultrasonically treating at room temperature with a power of 320 W for 55 min, pausing for 3 min every 15 min of ultrasonic treatment, and then continuously stirring at 220 r / min; adding anhydrous ethanol to adjust the viscosity; stirring evenly; and letting stand for 8 min for later use. The viscosity of the coating is measured by the flow time of a Coat-4 viscosity cup at 25°C, and controlled to be within 22 s. By weight, the composition includes 9 parts nano-silica, 5 parts wollastonite, 105 parts coating matrix resin, 1.5 parts UV shielding agent, 0.7 parts leveling agent, and 0.35 parts coating defoamer.

[0045] A method for preparing a coating matrix resin includes: adding a mixed solvent to an epoxy resin, treating it at 350 r / min and 85℃ for 18 min, adding dibutyltin dilaurate, dispersing it uniformly for 4 min, adding methylphenyl polysiloxane at a uniform rate for 100 min, maintaining the temperature at 85℃ throughout, raising the temperature to 140℃ and holding it for 2.5 h, cooling to 90℃, distilling under reduced pressure at -0.08 MPa for 1.5 h, and cooling to room temperature to obtain the coating matrix resin. By weight, the epoxy resin comprises 78 parts, the mixed solvent 27 parts, dibutyltin dilaurate 0.45 parts, and methylphenyl polysiloxane 28 parts. The mixed solvent consists of xylene and n-butanol; the volume ratio of xylene to n-butanol is 1:0.45.

[0046] Example 3:

[0047] A method for preparing a glass fiber composite insulating component for a high-voltage fuse, comprising: Step 1: Prepare modified glass fiber cloth, buffer resin, and impregnation resin separately; Step 2: Wrap two layers of modified glass fiber cloth around the mold core with a winding tension of 80N. After winding, uniformly roll-coat the buffer resin with a coating thickness of 0.023mm. Repeat the above operation until the designed wall thickness of 6.5mm is achieved. After completion, wrap the outermost layer with another layer of modified glass fiber cloth with a winding tension of 40N. Step 3: Place the resin in the impregnation tank, and under negative pressure, continuously pump air for 20 minutes at -0.092MPa to remove air from the gaps between the fibers. Introduce the impregnation resin until completely submerged. Under nitrogen atmosphere, maintain pressure at 0.6MPa and 45℃ for 40 minutes. Depressurize and recover the filtered impregnation resin. Step 4: Curing at 80℃ for 10 minutes, at 128℃ for 28 minutes, and at 163℃ for 37 minutes, then allowing to cool naturally to 60℃ before removing. Step 5: Remove the mold core, take out the tube, and perform plasma activation treatment on the outer wall. The power is 300W, the compressed air flow rate is 20L / min, and the activation time is 70s. Then, spray a protective coating on the outer wall of the tube. After spraying, let it stand at room temperature for 20min, and then cure it at 98℃ for 60min. The dry film thickness after spraying is 20μm, and the glass fiber composite insulation component for high voltage fuses is obtained.

[0048] A method for preparing modified glass fiber cloth includes: adding deionized water to anhydrous ethanol, then adding glacial acetic acid to adjust the pH to 4.5, adding γ-glycidoxypropyltrimethoxysilane, and stirring at room temperature for 30 min at 200 r / min to obtain a hydrolytic coupling solution. A single layer of glass fiber cloth is laid flat, and then the temperature is raised to 450℃ at a rate of 4℃ / min and kept at that temperature in air for 4 h; then it is naturally cooled to 80℃ and removed. The glass fiber cloth is then immersed in the hydrolytic coupling solution, allowed to stand for 30 min, drained, dried at room temperature for 15 min, and then dried at 120℃ for 30 min to obtain the modified glass fiber cloth. By weight, the amount of anhydrous ethanol is 95 parts, the amount of deionized water is 5 parts, and the amount of γ-glycidoxypropyltrimethoxysilane is 0.025 parts.

[0049] A method for preparing a buffer resin or impregnating resin: Nano-silica and hexagonal boron nitride are dried at 100℃ for 2 hours, then anhydrous ethanol and γ-glycidyl etheroxypropyltrimethoxysilane are added and stirred into a slurry. The slurry is allowed to stand for 18 minutes to obtain a coupling agent-coated filler. Epoxy resin is preheated to 42℃ and stirred at 280 r / min for 5 minutes. The coupling agent-coated filler is added in three batches, with stirring at 300 r / min for 10 minutes after each batch. After the addition is complete, the mixture is stirred at 12... Stir and disperse at 0 r / min for 30 min, then grind until the filler particle size is ≤2 μm. At 38℃, add curing agent diaminodiphenylmethane, toughening agent terminal carboxyl nitrile rubber, and organosilicon defoamer epoxy-modified polysiloxane in sequence. Stir at 400 r / min for 5 min, and degas in stages under vacuum. The first stage is set at -0.08 MPa and 39℃ and allowed to stand for 10 min. The second stage is set at -0.095 MPa and 45℃ and allowed to stand for 30 min.

[0050] The buffer resin contains, by weight, 70 parts epoxy resin, 18 parts curing agent, 7.3 parts nano silica, 5.2 parts hexagonal boron nitride, 1 part γ-glycidyl etheroxypropyltrimethoxysilane, 2.5 parts anhydrous ethanol, 5 parts toughening agent, and 0.5 parts silicone defoamer.

[0051] The resin impregnation mixture contains, by weight, 70 parts epoxy resin, 18 parts curing agent, 4.8 parts nano silica, 3.6 parts hexagonal boron nitride, 1 part γ-glycidyl etheroxypropyltrimethoxysilane, 2.5 parts anhydrous ethanol, 5 parts toughening agent, and 0.5 parts silicone defoamer.

[0052] A method for preparing a protective coating includes: drying nano-silica and wollastonite at 100°C for 2 hours; sequentially adding UV shielding agent 2-hydroxy-4-n-octyloxybenzophenone, polyacrylate leveling agent, and coating defoamer polyether-modified polysiloxane to the coating matrix resin, stirring continuously at 200 r / min for 10 minutes; adding nano-silica and wollastonite, stirring at 800 r / min for 20 minutes; then ultrasonically treating at room temperature with a power of 300 W for 60 minutes, pausing for 3 minutes every 15 minutes of ultrasonic treatment, and then continuously stirring at 200 r / min; adding anhydrous ethanol to adjust the viscosity; stirring evenly; and letting stand for 10 minutes for later use. The viscosity of the coating is measured by the flow time of a Coat-4 viscosity cup at 25°C, and controlled to be within 20 seconds. By weight, the composition includes 8 parts nano-silica, 4 parts wollastonite, 100 parts coating matrix resin, 1.2 parts UV shielding agent, 0.6 parts leveling agent, and 0.3 parts coating defoamer.

[0053] A method for preparing a coating matrix resin includes: adding a mixed solvent to an epoxy resin, treating it at 300 r / min and 82℃ for 20 min, adding dibutyltin dilaurate, dispersing it uniformly for 5 min, adding methylphenyl polysiloxane at a uniform rate for 90 min, maintaining the temperature at 83℃ throughout, raising the temperature to 135℃ and holding the reaction for 3 h, cooling to 90℃, distilling under reduced pressure at -0.08 MPa for 1.5 h, and cooling to room temperature to obtain the coating matrix resin. By weight, the epoxy resin comprises 75 parts, the mixed solvent 25 parts, dibutyltin dilaurate 0.4 parts, and methylphenyl polysiloxane 25 parts. The mixed solvent consists of xylene and n-butanol; the volume ratio of xylene to n-butanol is 1:0.43.

[0054] Comparative Example 1: The difference between the preparation method of a glass fiber composite insulating component for a high-voltage fuse and Example 1 is that glass fiber cloth is used instead of modified glass fiber cloth.

[0055] Comparative Example 2: The difference between the preparation method of a glass fiber composite insulating component for a high-voltage fuse and Example 1 is that the buffer resin is not rolled.

[0056] Comparative Example 3: The difference between the preparation method of a glass fiber composite insulating component for a high-voltage fuse and Example 1 is that the amounts of buffer resin and impregnation resin are the same, both being: by weight, 68 parts epoxy resin, 16 parts curing agent, 4.5 parts nano silica, 3.5 parts hexagonal boron nitride, 0.8 parts γ-glycidyl etheroxypropyltrimethoxysilane, 2 parts anhydrous ethanol, 4 parts toughening agent, and 0.4 parts organosilicon defoamer.

[0057] Comparative Example 4: The difference between the preparation method of a glass fiber composite insulating component for a high-voltage fuse and Example 1 is that plasma activation treatment is not performed.

[0058] Performance testing Arc resistance time was tested using IEC 61621 standard; bending strength was tested using ASTM D790 standard; and tensile strength was tested using ASTM D638 standard.

[0059] Table 1 Performance Test Results

[0060] The insulating components prepared in Examples 1-3 and Comparative Examples 1-4 were subjected to the above tests, and the results are shown in Table 1. As can be seen from Table 1, the performance of all components in the embodiments of the present invention is superior to that in the comparative examples. This is likely because the present invention significantly improves the interfacial bonding force between the fiber and the resin matrix through high-temperature heat treatment and silane coupling agent modification of the glass fiber cloth, thereby effectively improving the mechanical strength and arc resistance of the composite material. Furthermore, the present invention uses a buffer resin with a high filler content coated between each structural layer, combined with a wetting resin with a low filler content, forming a performance gradient structure that effectively transmits and buffers interlayer stress while enhancing insulation and barrier effects. After surface plasma activation treatment, a protective coating is sprayed, further improving the outer wall density and environmental adaptability of the insulating component, ensuring long-term reliable operation of the product. In contrast, Comparative Example 1 lacks coupling agent modification on the fiber surface, resulting in the inability to form a strong chemical bond between the resin matrix and the reinforcing fiber, leading to a large number of physical gaps in the interfacial area. When subjected to external forces, the interface cannot effectively transmit the load, and stress concentrates at the weak interface, resulting in significantly lower overall mechanical properties. Meanwhile, microscopic defects at the fiber-resin interface provide channels for charge accumulation and partial discharge, reducing the material's arc resistance. In Comparative Example 2, the coating step of the buffer resin was omitted during the interlayer winding process. The bonding between structural layers relied solely on subsequent impregnation with the wetting resin. The interfacial bonding strength between layers was insufficient, making the material prone to interlayer delamination and cracking under stress. Cracks could propagate rapidly along the interlayer interfaces, resulting in a significant weakening of the overall structure. Furthermore, the high content of inorganic fillers in the buffer resin, which originally served to disperse stress and enhance insulation, was lost after its removal. In Comparative Example 3, when the filler content of the buffer resin and the impregnation resin were the same, the insulating component lacked a stepwise buffering mechanism under load, making it easier for cracks to penetrate the entire wall thickness. The arc resistance also decreased due to the lack of protection from the filler-rich layer. In Comparative Example 4, due to the reduced adhesion of the unactivated surface coating and insufficient density of the protective layer, local breakdown or creepage was more likely to occur under arcing, resulting in decreased arc protection performance.

[0061] The conventional techniques described in the above embodiments are existing technologies known to those skilled in the art, and therefore will not be described in detail here.

[0062] The above description is merely a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention should be included within the scope of protection of the present invention. Therefore, the scope of protection of the present invention should be determined by the scope of the claims.

Claims

1. A method for preparing a glass fiber composite insulating component for a high-voltage fuse, comprising: Step 1: Prepare modified glass fiber cloth, buffer resin, and impregnation resin separately; Step 2: Wrap 2-3 layers of modified glass fiber cloth around the mold core with a winding tension of 75-85N. After winding, uniformly roll-coat the buffer resin with a coating thickness of 0.02-0.025mm. Repeat the above operation until the designed wall thickness is achieved. After completion, wrap the outermost layer with another layer of modified glass fiber cloth with a winding tension of 38-42N. Step 3: Place the resin in an impregnation tank and evacuate the air between the fibers under negative pressure for 18-22 minutes at -0.09MPa to -0.095MPa. Then, introduce the impregnation resin until the fibers are completely submerged. In a nitrogen atmosphere, maintain the pressure at 0.5-0.8MPa and 43-47℃ for 35-45 minutes. Then, release the pressure and recover the filtered impregnation resin. Step 4: Curing at 75-85℃ for 8-12 minutes, curing at 125-130℃ for 25-30 minutes, curing at 160-165℃ for 35-40 minutes, then naturally cooling to 60℃ and removing. Step 5: Remove the mold core, take out the tube, and perform plasma activation treatment on the outer wall. The power is 280-320W, the compressed air flow rate is 18-22L / min, and the activation time is 60-90s. Then, spray a protective coating on the outer wall of the tube. After spraying, let it stand at room temperature for 18-25min, and then cure it at a constant temperature of 95-100℃ for 55-70min to obtain the glass fiber composite insulation component for high voltage fuses.

2. The method for preparing a glass fiber composite insulating component for a high-voltage fuse according to claim 1, characterized in that: The method for preparing the modified glass fiber cloth includes: adding deionized water to anhydrous ethanol, then adding glacial acetic acid to adjust the pH to 4-5, adding γ-glycidoxypropyltrimethoxysilane, and stirring at room temperature for 25-35 min at a speed of 180-220 r / min to obtain a hydrolytic coupling solution; laying a single layer of glass fiber cloth flat, then heating it to 440-460℃ at a rate of 3-5℃ / min and keeping it at that temperature in air for 3.5-4.5 h; then naturally cooling it to 75-85℃ and removing it, then immersing the glass fiber cloth in the hydrolytic coupling solution, letting it stand for 25-35 min, then removing it and draining it, drying it at room temperature for 12-18 min, and then drying it at 115-125℃ for 25-35 min to obtain the modified glass fiber cloth.

3. The method for preparing a glass fiber composite insulating component for a high-voltage fuse according to claim 2, characterized in that: The fiberglass cloth has a strength of 200g / m². 2 Plain weave alkali-free fiberglass cloth, with a single filament diameter of 9μm.

4. The method for preparing a glass fiber composite insulating component for a high-voltage fuse according to claim 1, characterized in that: The preparation method of the buffer resin or impregnating resin includes: drying nano-silica and hexagonal boron nitride at 95-105℃ for 2-2.5h, then adding anhydrous ethanol and γ-glycidoxypropyltrimethoxysilane and stirring to form a slurry, allowing it to stand for 15-20min to obtain a coupling agent-coated filler; preheating the epoxy resin to 40-45℃, stirring at 200-300r / min for 4-6min, adding the coupling agent-coated filler in 3-4 batches, and stirring at 280-320r / min for 8-12 minutes after each batch. After the filler is added, stir and disperse it at 110-125 r / min for 25-35 min. Then grind it until the filler particle size is ≤2μm. At 35-40℃, add the curing agent, toughening agent and silicone defoamer in sequence, and stir at 350-450 r / min for 4-6 min. Perform segmented vacuum degassing. The first segment is set at -0.08MPa and 38-40℃ for 8-12 min, and the second segment is set at -0.095MPa and 43-47℃ for 28-32 min.

5. The method for preparing a glass fiber composite insulating component for a high-voltage fuse according to claim 4, characterized in that: The buffer resin comprises, by weight, 68-72 parts epoxy resin, 16-20 parts curing agent, 7-7.5 parts nano silica, 5-5.5 parts hexagonal boron nitride, 0.8-1.2 parts γ-glycidyl etheroxypropyltrimethoxysilane, 2-3 parts anhydrous ethanol, 4-6 parts toughening agent, and 0.4-0.6 parts silicone defoamer.

6. The method for preparing a glass fiber composite insulating component for a high-voltage fuse according to claim 4, characterized in that: The impregnating resin comprises, by weight, 68-72 parts epoxy resin, 16-20 parts curing agent, 4.5-5 parts nano silica, 3.5-4 parts hexagonal boron nitride, 0.8-1.2 parts γ-glycidyl etheroxypropyltrimethoxysilane, 2-3 parts anhydrous ethanol, 4-6 parts toughening agent, and 0.4-0.6 parts silicone defoamer.

7. The method for preparing a glass fiber composite insulating component for a high-voltage fuse according to claim 1, characterized in that: The preparation method of the protective coating includes: drying nano-silica and wollastonite at 95-105℃ for 1.5-2.5h; sequentially adding UV shielding agent, leveling agent, and coating defoamer to the coating matrix resin, stirring continuously at 180-220r / min for 8-15min, adding nano-silica and wollastonite, stirring at 750-850r / min for 18-25min, then ultrasonically treating at room temperature with a power of 280-320W for 55-65min, pausing for 3min every 15min of ultrasonic treatment, and then continuously stirring at 180-220r / min, adding anhydrous ethanol to adjust the viscosity, stirring evenly, and letting stand for 8-15min for later use.

8. The method for preparing a glass fiber composite insulating component for a high-voltage fuse according to claim 7, characterized in that: The viscosity of the protective coating was tested using the flow time of a Coat-4 viscosity cup at 25°C, and was controlled within 18-22 seconds.

9. The method for preparing a glass fiber composite insulating component for a high-voltage fuse according to claim 1, characterized in that: The wall thickness in step one is designed to be 6-7mm; The dry film thickness after the protective coating is sprayed in step five is 15-30 μm.

10. A glass fiber composite insulating component, characterized in that: The insulating component is prepared by any one of the preparation methods in claims 1-9.