A method for manufacturing an air suspension composite gas storage tank based on hot-melt welding of the bottle neck seal.
By using homogeneous hot-melt welding and fiber winding technology of HDPE material, the sealing and pressure bearing problems of the air suspension tank opening connection area are solved, achieving lightweight and consistent manufacturing, which is suitable for vehicle air suspension systems.
Patent Information
- Application Number
- CN202611203272.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-10
- Publication Date
- 2026-11-17
AI Technical Summary
Existing air suspension tanks lack sufficient sealing reliability, pressure resistance, and fatigue resistance in the bottle neck connection area, posing challenges, especially in terms of vehicle lightweighting and mass production consistency.
HDPE material is used to form the end cap valve seat assembly and the plastic inner liner through homogeneous hot-melt welding. The fiber winding bearing surface is formed by plasma activation treatment and combined with the fiber reinforcement layer to form a continuous sealing bearing structure.
It improves the sealing stability and pressure resistance of the gas tank's nozzle connection, reduces weight, enhances the consistency of the manufacturing process and the reliability of assembly, and is suitable for the comprehensive requirements of vehicle air suspension systems.
Smart Images

Figure CN123104119A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of suspension system component manufacturing technology, specifically to a method for manufacturing an air suspension composite air tank based on hot-melt welding of the bottle mouth seal. Background Technology
[0002] Automotive air suspension systems typically require an air tank to store compressed air and provide the air source for suspension height adjustment, attitude control, and damping response. During vehicle operation, the air tank needs to withstand various working conditions such as repeated inflation and deflation, temperature changes, road vibration, and installation loads. Therefore, the reliability of its bottle mouth seal, pressure bearing capacity, fatigue resistance, and structural consistency all affect the long-term stability of the air suspension system. Existing air suspension tanks are mostly made of metal. Metal tanks have a mature foundation in forming, assembly, and use, and can meet conventional air storage needs. With the increasing demand for lightweight, long-life, and maintenance-free vehicles, air tanks need to further consider weight control, corrosion resistance, bottle neck connection sealing stability, and batch manufacturing consistency while ensuring pressure safety. Especially in application scenarios with limited installation space in the vehicle chassis and frequent operating vibrations, the requirements for the coordinated reliability between the bottle neck connection area and the tank body load-bearing structure are even higher. For composite gas tanks, a stable structural fit is required between the plastic inner liner, the bottle neck connection, and the external reinforcing layer. If there is a lack of continuous fit between the bottle neck connection area, the outer surface condition of the inner liner, the molding state of the fiber reinforcing layer, and the curing process, it may affect the bottle neck sealing, the adhesion of the reinforcing layer, the maintenance of the tank shape, and the consistency of the finished product performance. Therefore, it is necessary to provide a manufacturing method suitable for air suspension composite gas tanks, so that the bottle neck sealing, inner liner molding, surface treatment, fiber reinforcement, and curing processes can form a continuous manufacturing chain. Summary of the Invention
[0003] The purpose of this invention is to provide a method for manufacturing an air suspension composite gas storage tank based on hot-melt welding of the bottle mouth seal, so as to solve the problems mentioned in the background art.
[0004] This invention can be achieved through the following technical solution: a method for manufacturing an air suspension composite gas storage tank based on hot-melt welding of the bottle neck seal, comprising: Step 1: Place the metal connecting insert into the injection mold, and use HDPE material to perform insert injection molding on the metal connecting insert to form a head valve seat assembly. The head valve seat assembly includes a metal valve seat and an HDPE head that is fixedly connected to the outer periphery of the metal valve seat. The HDPE head has a head annular welded part. Step 2: Use HDPE material to blow mold a plastic liner, and form an annular welded part at the bottle mouth of the plastic liner for connection with the annular welded part of the end cap. Step 3: Coaxially clamp the end cap valve seat assembly with the plastic inner liner, so that the annular welded part of the end cap and the annular welded part of the inner liner are positioned opposite each other. Heat the annular welded parts of the end cap and the inner liner until they soften or melt. After pressure butt welding, cool to form a homogeneous hot melt welded seal connection. Step 4: Perform plasma activation treatment on the outer surface of the plastic inner liner and the outer surface of the HDPE end cap after forming a homogeneous hot melt welded seal connection to form a fiber-wound bearing surface. Step 5: Inflate the plastic liner with shaping gas to keep it inflated and supported during the fiber winding process. Step 6: Under the inflated support state, the resin-impregnated fiber is wound onto the fiber winding receiving surface to form a fiber reinforcement layer; Step 7: Curing the plastic inner liner after the fiber reinforcement layer is formed to form an air suspension composite air tank.
[0005] A further technical improvement of the present invention is that: in step one, the metal connecting insert is made of 6061-T6 aluminum alloy and constitutes the metal valve seat in the end cap valve seat assembly. The metal valve seat is provided with a tapered thread connecting hole for connecting the air suspension pipeline connector, and the end cap valve seat assembly is provided with an annular sealing groove for accommodating the sealing ring.
[0006] A further technical improvement of the present invention is that: in step one, the interface between the metal valve seat and the HDPE end cap is provided with a plastic-embedded locking structure. The insert locking structure includes at least one dovetail groove extending circumferentially along the metal valve seat. During insert injection molding, HDPE material enters the dovetail groove, causing the HDPE end cap to form a mechanical interlocking connection with the metal valve seat.
[0007] A further technical improvement of the present invention is that: in step two, the annular welding part of the inner liner is formed by the annular bevel reserved at the mouth of the plastic inner liner; In step three, after the annular welded part of the end cap and the annular welded part of the inner liner are pressure-jointed, a closed fusion zone is formed around the mouth of the plastic inner liner bottle.
[0008] A further technical improvement of the present invention is as follows: In step three, the coaxiality of the end cap valve seat assembly and the plastic inner liner after coaxial clamping is no more than 0.2 mm. The end cap annular welded part and the inner liner annular welded part are heated by a hot plate at a temperature of 230°C for 20 to 30 seconds. The pressure applied during the butt joint is 0.3 MPa to 0.5 MPa, and the pressure holding time is 30 to 60 seconds.
[0009] A further technical improvement of the present invention is that: in step four, plasma activation treatment covers the outer surface of the plastic inner liner and the outer surface of the HDPE end cap located within the fiber winding path, and the treated outer surface of the plastic inner liner and the outer surface of the HDPE end cap together form the fiber winding receiving surface.
[0010] A further technical improvement of the present invention is that: in step five, a shaping gas is injected into the plastic inner liner to make the pressure inside the plastic inner liner 0.015MPa to 0.03MPa, and the plastic inner liner is kept in an inflated support state during the fiber winding process in step six.
[0011] A further technical improvement of the present invention is that, in step six, the resin-impregnated fiber is one or a combination of two of continuous glass fiber and continuous carbon fiber impregnated with epoxy resin. The fiber reinforcement layer includes a first circumferential layer, a helical layer, and a second circumferential layer formed sequentially from the inside out. The winding angles of the first circumferential layer and the second circumferential layer are both ±88°, and the winding angle of the helical layer is ±12°.
[0012] A further technical improvement of the present invention is that: in step six, a first fiber winding layer is first formed on the outer side of the fiber winding receiving surface, and the first fiber winding layer is first cured to form a primary composite reinforced shell; Then, a fixed bracket is installed at the bracket installation position of the primary composite reinforced shell, and the fixed bracket is wrapped in the second fiber winding layer by circumferential winding, so that the first fiber winding layer and the second fiber winding layer together form a fiber reinforced layer. In step seven, the second fiber winding layer undergoes a secondary curing process.
[0013] Compared with the prior art, the present invention has the following beneficial effects: This invention can improve the sealing stability of the air suspension composite air tank bottle mouth connection area; after the bottle mouth connection forms a continuous sealing bearing structure, it can reduce the risk of leakage caused by discontinuous connection interface, assembly gap or local stress concentration, so that the air tank can maintain relatively stable air tightness under repeated filling and defilling and vehicle vibration conditions. Furthermore, this invention can balance the lightweight design and pressure-bearing performance of the air tank; by combining the airtight load-bearing foundation with the external reinforced load-bearing structure, it can improve the tank's ability to withstand internal pressure and external impact loads while controlling the tank's weight, making the air tank more suitable for the comprehensive requirements of vehicle air suspension systems for weight, strength and fatigue life. On the other hand, the present invention can improve the consistency of the manufacturing process and the reliability of subsequent assembly. After the continuous control is formed between the inner liner outer surface bearing state, the air-supporting state, the fiber laying state and the curing state, it is beneficial to reduce problems such as winding deformation, interlayer debonding, local thickness unevenness and bracket loosening, so that the air suspension composite air tank is improved in terms of dimensional stability, installation stability and batch production consistency. Attached Figure Description
[0014] To facilitate understanding by those skilled in the art, the present invention will be further described below with reference to the accompanying drawings.
[0015] Figure 1 This is a process flow diagram of the present invention. Detailed Implementation
[0016] To further illustrate the technical means and effects adopted by the present invention to achieve the intended purpose, the following detailed description of the specific implementation methods, structures, features and effects of the present invention, in conjunction with the accompanying drawings and preferred embodiments, is provided.
[0017] Please see Figure 1 As shown, this invention provides a method for manufacturing an air suspension composite air tank based on a thermoplastic welded bottle neck seal, used to manufacture composite air tanks in vehicle air suspension systems. The air suspension composite air tank includes a plastic inner liner, a valve seat assembly, and a fiber reinforcement layer. The plastic inner liner is blow-molded from HDPE material; the valve seat assembly includes a metal valve seat and an HDPE end cap that is embedded and fixedly connected to the outer periphery of the metal valve seat; the HDPE end cap and the bottle neck of the plastic inner liner are sealed together by homogeneous thermoplastic welding; the fiber reinforcement layer is formed on the outer side of the plastic inner liner and the HDPE end cap.
[0018] The specific manufacturing process includes the following steps: Step 1: Place the metal connecting insert into the injection mold, ensuring the outer periphery of the insert is within the head forming cavity of the mold. The metal connecting insert is made of 6061-T6 aluminum alloy and forms the metal valve seat in the head valve seat assembly. The metal valve seat has a tapered threaded connection hole for connecting the air suspension pipe connector. Near the bottom of the valve, the metal valve seat has an annular sealing groove that extends continuously along the circumference of the metal valve seat, and a sealing ring is installed within the groove. The sealing ring abuts against the corresponding sealing surface in the bottle neck connection area, creating a sealed fit between the bottom of the metal valve seat and the bottle neck connection area. The outer periphery of the metal valve seat also features a dovetail groove structure and a curved transition structure. During injection molding, HDPE material covers the outer periphery of the metal valve seat and enters the dovetail groove structure, creating a mechanical interlocking connection between the HDPE head and the metal valve seat.
[0019] The interface between the metal valve seat and the HDPE end cap is provided with a plastic-fit locking structure. The plastic-fit locking structure includes at least one dovetail groove extending circumferentially along the metal valve seat. During insert injection molding, the molten HDPE material enters the dovetail groove, and after cooling and solidification, it forms a mechanical interlocking connection with the dovetail groove, thereby limiting the HDPE end cap and the metal valve seat in the axial pull-out direction and the circumferential rotation direction.
[0020] In one specific embodiment, the insert locking structure further includes a curved transition structure adjacent to the dovetail groove, which guides the HDPE material to continuously fill between the outer periphery of the metal valve seat and the dovetail groove. During insert injection molding, the HDPE material enters the dovetail groove along the curved transition structure, and after cooling, forms an insert portion within the dovetail groove that interlocks with the metal valve seat.
[0021] During insert injection molding, HDPE material enters the injection mold and covers the area to be inserted around the metal valve seat. After cooling and solidification, it forms an HDPE end cap that is firmly connected to the outer periphery of the metal valve seat. The HDPE end cap has an annular welded part, which is used for heat fusion welding with the annular welded part of the inner liner at the mouth of the plastic bottle.
[0022] In one specific embodiment, during HDPE head injection molding, the barrel temperature is 190°C to 210°C, preferably 200°C; the mold temperature is 40°C to 50°C, preferably 45°C; the injection pressure is 80MPa to 100MPa, preferably 90MPa; the holding pressure is 40MPa to 60MPa, preferably 50MPa; and the cooling time is 30 seconds to 45 seconds, preferably 40 seconds.
[0023] Step 2: Use HDPE material to blow mold the plastic inner liner. During blow molding, the HDPE material is plasticized to form a tubular preform. The tubular preform is placed in the inner liner blow molding mold. After the mold is closed, molding gas is introduced into the tubular preform, so that the HDPE material adheres to the inner wall of the inner liner blow molding mold cavity. After cooling, a plastic inner liner with a gas storage cavity is formed.
[0024] In one specific embodiment, during the blow molding of the HDPE inner liner, the extruder feed section temperature is 200℃, with a temperature control deviation of ±5℃; the extruder melt section temperature is 180℃ to 195℃, with a temperature control deviation of ±5℃; the die head temperature is 180℃, with a temperature control deviation of ±5℃; the blow pressure is 0.3MPa to 0.5MPa; the cooling water temperature is 15℃ to 20℃; and the wall thickness of the blow-molded plastic inner liner is 1.5mm.
[0025] The plastic inner liner has an annular welded section at the bottle mouth for connection with the annular welded section of the end cap. This annular welded section is formed by a pre-drilled annular bevel at the bottle mouth of the plastic inner liner. The annular bevel extends continuously along the circumference of the bottle mouth and is used to connect with the annular welded section of the end cap during hot-melt welding.
[0026] After blow molding, the annular welded part of the inner liner at the bottle mouth is trimmed so that the annular welded part of the inner liner and the annular welded part of the end cap have a corresponding annular contour.
[0027] Step 3: Clamp the end cap valve seat assembly and the plastic inner liner onto the welding fixture, ensuring that the end cap valve seat assembly and the plastic inner liner are coaxial. After clamping, the annular welded part of the end cap and the annular welded part of the inner liner are positioned opposite each other, with the circumferential center line of the annular welded part of the end cap corresponding to the circumferential center line of the annular welded part of the inner liner.
[0028] In one specific embodiment, the coaxiality of the end cap valve seat assembly and the plastic inner liner after coaxial clamping is no greater than 0.2 mm, preferably 0.15 mm. The annular welded portion of the end cap and the annular welded portion of the inner liner are heated by a hot plate at a temperature of 230°C for 20 to 30 seconds, preferably 25 seconds. After heating, the annular welded portion of the end cap and the annular welded portion of the inner liner reach a softened or molten state.
[0029] The hot plate is then removed, allowing the annular welded portion of the end cap to be pressed together with the annular welded portion of the inner liner under a pressure of 0.3 MPa to 0.5 MPa, preferably 0.4 MPa; the pressure holding time is 30 to 60 seconds, preferably 45 seconds. After the pressure holding is completed, the welded area is allowed to cool naturally to room temperature.
[0030] After the annular welded part of the end cap and the annular welded part of the inner liner are pressurized and joined together, a closed fusion zone is formed around the circumference of the bottle mouth of the plastic inner liner. The fusion zone is formed by the fusion of the molten material of the HDPE end cap and the molten material of the bottle mouth of the plastic inner liner, followed by cooling. After cooling, the joint at the bottle mouth forms a homogeneous hot-melt welded seal. After welding, the flash generated at the weld edge is removed, creating a continuous surface on the outer circumference of the bottle mouth.
[0031] In one specific embodiment, the welding strength of the homogeneous hot melt welded sealing connection is tested, and the strength of the welded joint is not less than 90% of the strength of the HDPE base material.
[0032] After hot-melt welding, the HDPE end cap and the plastic inner liner bottle mouth are fused together to form a sealed connection, and the metal valve seat is connected to the plastic inner liner bottle mouth as one unit through the HDPE end cap.
[0033] Step 4: Perform plasma activation treatment on the outer surface of the plastic inner liner and the outer surface of the HDPE end cap after forming a homogeneous hot melt welded seal connection to form a fiber-wound bonding surface.
[0034] Plasma activation treatment is applied to the outer surface of the plastic inner liner and the outer surface of the HDPE end cap located within the fiber winding path. The treated outer surfaces of the plastic inner liner and the HDPE end cap together form the fiber winding receiving surface.
[0035] During the plasma activation process, the plasma nozzle is moved relative to the plastic inner liner in both the axial and circumferential directions, or the plastic inner liner is rotated around its own axis while the plasma nozzle moves axially, so that the outer surface of the plastic inner liner and the outer surface of the HDPE end cap pass through the plasma action zone. After plasma activation, the fiber-wound receiving surface is used to receive the resin-impregnated fibers.
[0036] Step 5: Inflate the plastic inner liner with a shaping gas to maintain its inflated and supported state during fiber winding. The shaping gas is air. After inflation, the internal pressure of the plastic inner liner should be between 0.015 MPa and 0.03 MPa, preferably 0.02 MPa.
[0037] Inflatable shaping is used to support the connection area between the plastic liner and the bottle mouth during the fiber winding process, ensuring that the plastic liner maintains its roundness and cavity dimensions when subjected to fiber winding tension. When the plastic liner is directly subjected to winding tension in an uninflated state, it is prone to local collapse, elliptical deformation, or relative displacement of the bottle mouth.
[0038] When the internal pressure of the plastic inner liner is controlled between 0.015 MPa and 0.03 MPa, the plastic inner liner receives internal support. When the internal pressure of the plastic inner liner is below 0.015 MPa, the plastic inner liner's resistance to deformation under winding tension is insufficient; when the internal pressure of the plastic inner liner is above 0.03 MPa, the plastic inner liner is at risk of dimensional expansion before winding, affecting the finished product's dimensions and the fiber layer's placement.
[0039] During the fiber winding process in step six, the plastic liner is kept in an inflated and supported state.
[0040] Step Six: Under inflated support, resin-impregnated fibers are wound around the fiber winding receiving surface to form a fiber reinforcement layer. The resin-impregnated fibers are one or a combination of two of continuous glass fibers and continuous carbon fibers impregnated with epoxy resin. Preferably, the resin-impregnated fibers are continuous glass fibers impregnated with epoxy resin; in other embodiments, the resin-impregnated fibers are continuous carbon fibers impregnated with epoxy resin, or a combination of continuous glass fibers impregnated with epoxy resin and continuous carbon fibers.
[0041] In one specific embodiment, during fiber winding, the fiber tension is 15 N / bundle, and the winding speed is 15 m / min to 25 m / min, preferably 20 m / min; in the wet winding embodiment, the resin content is 30 ± 2%; in another winding control embodiment, the resin content is 26%. The winding ambient temperature is 10-35℃, preferably 23℃; the winding ambient humidity is 50 ± 10% RH, preferably 50% RH. Based on the fiber tension, winding speed, and resin content, the resin-impregnated fibers are continuously laid on the fiber winding receiving surface.
[0042] The fiber reinforcement layer comprises a first circumferential layer, a helical layer, and a second circumferential layer formed sequentially from the inside out. The winding angles of the first and second circumferential layers are both ±88°, and the winding angle of the helical layer is ±12°. The winding angles are determined with reference to the axial direction of the plastic inner liner.
[0043] In another specific embodiment, step six also includes a support fixing process. First, a first fiber winding layer is formed on the outer side of the fiber winding receiving surface, and the first fiber winding layer is cured for the first time to form a primary composite reinforced shell. The first curing process uses a process of holding at 90°C for 40 minutes + 105°C for 120 minutes to gel and set the first fiber winding layer.
[0044] After the first curing, a mounting bracket is installed at the support mounting position on the primary composite reinforced shell. The mounting bracket is used to install the air suspension composite air tank to the vehicle chassis or the assembly position of the air suspension system.
[0045] After the mounting bracket is installed, it is wrapped around the second fiber winding layer in a circumferential manner, so that the mounting bracket is compressed and confined to the outside of the primary composite reinforced shell by the second fiber winding layer. The first and second fiber winding layers together form the fiber reinforcement layer. The second fiber winding layer covers the outside of the mounting bracket and, after subsequent curing, connects with the first fiber winding layer, so that the mounting bracket remains in the bracket installation position within the primary composite reinforced shell.
[0046] Step 7: Curing treatment is applied to the plastic inner liner after the fiber reinforcement layer is formed to create an air suspension composite air tank. The curing treatment is used to cross-link and cure the epoxy resin in the resin-impregnated fibers, so that the fiber reinforcement layer forms a composite pressure-bearing shell.
[0047] In one specific embodiment, the curing process is carried out in a curing oven. The plastic inner liner with completed fiber winding is placed in the curing oven and slowly rotated during the curing process. The effective volume of the curing oven meets the requirements for rotational curing of the air suspension composite air tank, and the allowance in the diameter direction of the tank is not less than 200mm; the temperature difference in the working area of the curing oven is not greater than ±3℃, preferably ±2℃; the temperature control accuracy is ±1℃; the heating rate of the curing oven is adjustable from 0.5℃ / min to 5℃ / min; the hot air circulation speed is 0.5m / s to 1m / s; the curing oven has a program control function for setting the heating, holding, and cooling curves.
[0048] During the curing process, the rotation speed of the rotating tool is 1 rpm to 5 rpm, preferably 3 rpm; the coaxiality of the rotating tool is no greater than 0.5 mm; the load-bearing capacity of the rotating tool is no less than 50 kg. The ambient temperature before curing is 10-35℃, and the ambient humidity is 50±10%RH; after curing, the air suspension composite air tank is allowed to cool naturally to below 40℃ in the curing oven before being removed.
[0049] In one specific embodiment, the curing process includes: heating from room temperature to 90°C at a heating rate of 1°C / min to 2°C / min, preferably at a heating rate of 1.5°C / min; holding at 90°C for 40 min; then heating to 105°C at a heating rate of 1°C / min and holding at 105°C for 120 min; after the holding period, cooling at a cooling rate of no more than 1°C / min, or naturally cooling to below 40°C in the curing oven before removal.
[0050] When step six includes a secondary winding process for the fixed bracket, the curing treatment in step seven includes a secondary curing treatment of the second fiber winding layer. The secondary curing treatment employs a curing process of raising the temperature from room temperature to 105°C and holding it at that temperature for 120 minutes, causing the epoxy resin in the second fiber winding layer to crosslink and cure. After curing, an air suspension composite air tank is obtained.
[0051] In one specific embodiment, the cured fiber-reinforced layer is subjected to curing degree testing and glass transition temperature testing. The curing degree testing is performed using DSC quantitative detection, and the obtained curing degree is not less than 95%; the glass transition temperature Tg is not less than 105℃.
[0052] After curing, the air suspension composite air tank undergoes quality inspection. The quality inspection includes visual inspection, dimensional inspection, pressure resistance test, and airtightness test. Visual inspection confirms the absence of cracks, bubbles, delamination, and exposed fibers on the outer surface of the air suspension composite air tank; dimensional inspection confirms that the tank's diameter and length meet design requirements; the pressure resistance test tests the tank's pressure-bearing capacity; and the airtightness test tests the sealing performance of the hot-melt weld at the bottle neck, the valve seat assembly, and the overall tank body.
[0053] In one specific implementation, the airtightness test uses a 3MPa pressure holding period of 3 minutes, with a pressure drop not exceeding 0.01%. The pass standard for the airtightness test is that the helium leakage at room temperature is ≤1.6 × 10⁻⁶. -5 Pa·m³ / s. After passing the airtightness test, the air suspension composite air tank is cleaned, protected, and packaged.
[0054] Comparative Cases: To verify the performance of the air suspension composite air tank prepared in this embodiment, the air suspension composite air tank manufactured in accordance with this embodiment is used as the embodiment sample, and an aluminum inner liner air tank under the same application scenario is used as a comparative sample for comparison testing.
[0055] The example sample is made of HDPE plastic liner, HDPE end cap, 6061-T6 aluminum alloy metal valve seat, and glass fiber or carbon fiber wound reinforcement layer. The HDPE end cap and the bottle mouth of the plastic liner are sealed by homogeneous hot-melt welding. The comparative sample uses an aluminum liner structure, and the bottle mouth connection area uses a metal welding or metal interface connection structure.
[0056] The tests included working pressure, burst pressure, total tank weight, airtightness, fatigue resistance, and adaptability to humid and hot environments. The test results are shown in Table 1 below: Table 1
[0057] The test results above show that, under the same air suspension tank application scenario, the sample in the example form a bottle mouth sealing structure by homogeneous hot-melt welding of HDPE plastic liner and HDPE end cap, and the external pressure-bearing reinforcement is undertaken by fiber reinforcement layer, so that the tank exhibits better comprehensive performance in terms of weight, burst pressure, fatigue cycle number and adaptability to humid and hot environment.
[0058] The weight of the entire tank in the example sample was approximately 1.7 kg, while the weight of the comparative sample was approximately 2.5 kg, indicating that the example sample was lighter than the comparative sample. The burst pressure of the example sample was not less than 10 MPa, while the burst pressure of the comparative sample was 6 MPa to 8 MPa. The design fatigue cycle count of the example sample was not less than 200,000 cycles, while the aluminum tank of the comparative sample was prone to micro-leakage due to repeated fatigue filling and discharging. These results demonstrate that the manufacturing method of using HDPE plastic inner liner, homogeneous hot-melt welding of the bottle mouth, and fiber winding reinforcement can improve the pressure-bearing capacity and cyclic stability of the composite gas storage tank while reducing its weight.
[0059] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art can make some modifications or alterations to the above-disclosed technical content to create equivalent embodiments without departing from the scope of the present invention. Any simple modifications, equivalent changes and alterations made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the scope of the present invention.
Claims
1. A method for manufacturing an air suspension composite gas storage tank based on hot-melt welding of the bottle neck seal, characterized in that, include: Step 1: Place the metal connecting insert into the injection mold, and use HDPE material to perform insert injection molding on the metal connecting insert to form a head valve seat assembly. The head valve seat assembly includes a metal valve seat and an HDPE head that is fixedly connected to the outer periphery of the metal valve seat. The HDPE head has a head annular welded part. Step 2: Use HDPE material to blow mold a plastic liner, and form an annular welded part at the bottle mouth of the plastic liner for connection with the annular welded part of the end cap. Step 3: Coaxially clamp the end cap valve seat assembly with the plastic inner liner, so that the annular welded part of the end cap and the annular welded part of the inner liner are positioned opposite each other. Heat the annular welded parts of the end cap and the inner liner until they soften or melt. After pressure butt welding, cool to form a homogeneous hot melt welded seal connection. Step 4: Perform plasma activation treatment on the outer surface of the plastic inner liner and the outer surface of the HDPE end cap after forming a homogeneous hot melt welded seal connection to form a fiber-wound bearing surface. Step 5: Inflate the plastic liner with shaping gas to keep it inflated and supported during the fiber winding process. Step 6: Under the inflated support state, the resin-impregnated fiber is wound onto the fiber winding receiving surface to form a fiber reinforcement layer; Step 7: Curing the plastic inner liner after the fiber reinforcement layer is formed to form an air suspension composite air tank.
2. The method for manufacturing an air suspension composite gas storage tank based on hot-melt welding bottle neck seal according to claim 1, characterized in that, In step one, the metal connecting insert is made of 6061-T6 aluminum alloy and forms the metal valve seat in the end cap valve seat assembly. The metal valve seat is provided with a tapered thread connecting hole for connecting the air suspension pipeline connector, and the end cap valve seat assembly is provided with an annular sealing groove for accommodating the sealing ring.
3. The method for manufacturing an air suspension composite gas storage tank based on hot-melt welding bottle neck seal according to claim 1, characterized in that, In step one, the interface between the metal valve seat and the HDPE end cap is provided with a plastic-embedded locking structure. The insert locking structure includes at least one dovetail groove extending circumferentially along the metal valve seat. During insert injection molding, HDPE material enters the dovetail groove, causing the HDPE end cap to form a mechanical interlocking connection with the metal valve seat.
4. The method for manufacturing an air suspension composite gas storage tank based on hot-melt welding bottle neck seal according to claim 1, characterized in that, In step two, the annular welded part of the inner liner is formed by the annular bevel reserved at the mouth of the plastic inner liner; In step three, after the annular welded part of the end cap and the annular welded part of the inner liner are pressure-jointed, a closed fusion zone is formed around the mouth of the plastic inner liner bottle.
5. The method for manufacturing an air suspension composite gas storage tank based on hot-melt welding bottle neck seal according to claim 1, characterized in that, In step three, the coaxiality of the end cap valve seat assembly and the plastic inner liner after coaxial clamping is no more than 0.2mm. The annular welded part of the end cap and the annular welded part of the inner liner are heated by a hot plate at a temperature of 230℃ for 20 to 30 seconds. The pressure applied during the butt joint is 0.3MPa to 0.5MPa, and the pressure holding time is 30 to 60 seconds.
6. The method for manufacturing an air suspension composite gas storage tank based on hot-melt welding bottle neck seal according to claim 1, characterized in that, In step four, plasma activation treatment is applied to the outer surface of the plastic liner and the outer surface of the HDPE end cap located within the fiber winding path. The treated outer surface of the plastic liner and the outer surface of the HDPE end cap together form the fiber winding receiving surface.
7. The method for manufacturing an air suspension composite gas storage tank based on hot-melt welding bottle neck seal according to claim 1, characterized in that, In step five, a shaping gas is injected into the plastic liner to make the pressure inside the plastic liner between 0.015MPa and 0.03MPa, and the plastic liner is kept in an inflated support state during the fiber winding process in step six.
8. The method for manufacturing an air suspension composite gas storage tank based on hot-melt welding bottle neck seal according to claim 1, characterized in that, In step six, the resin-impregnated fiber is one or a combination of two of continuous glass fiber and continuous carbon fiber impregnated with epoxy resin. The fiber reinforcement layer includes a first circumferential layer, a helical layer, and a second circumferential layer formed sequentially from the inside out. The winding angles of the first circumferential layer and the second circumferential layer are both ±88°, and the winding angle of the helical layer is ±12°.
9. The method for manufacturing an air suspension composite gas storage tank based on hot-melt welding bottle neck seal according to claim 1, characterized in that, In step six, a first fiber winding layer is first formed on the outer side of the fiber winding receiving surface, and the first fiber winding layer is cured for the first time to form a primary composite reinforced shell; Then, a fixed bracket is installed at the bracket installation position of the primary composite reinforced shell, and the fixed bracket is wrapped in the second fiber winding layer by circumferential winding, so that the first fiber winding layer and the second fiber winding layer together form a fiber reinforced layer. In step seven, the second fiber winding layer undergoes a secondary curing process.