A high-adhesion self-adhesive modified bitumen waterproof membrane and its preparation method
By using silane coupling agent KH550/A17 and a multi-layer silicone oil release film structure in self-adhesive modified bitumen waterproof membrane, the balance between low-temperature flexibility and adhesion performance of self-adhesive membrane is solved, improving the adhesion strength to metal substrates and reducing construction difficulty and cost.
Patent Information
- Application Number
- CN202611418699.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-14
- Publication Date
- 2026-11-17
AI Technical Summary
Existing self-adhesive rolls struggle to balance low-temperature flexibility and adhesive performance, especially exhibiting insufficient adhesion strength to metal substrates. Furthermore, the release liner is prone to sticking at high temperatures, impacting construction efficiency and resulting in high costs.
By using silane coupling agent KH550/A17 at low temperature and optimizing the self-adhesive compound formulation, combined with a multi-layer silicone oil release film structure, high-temperature aging is avoided, the amount of SBR/tackifying resin is reduced, and low-temperature flexibility and adhesion are improved.
It significantly improves the bonding strength of aluminum plates, galvanized plates and cement-based surfaces, reduces costs, improves construction efficiency, and ensures low-temperature flexibility and high-temperature stability.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of building waterproofing materials technology, and in particular to a high-adhesion self-adhesive modified bitumen waterproof membrane and its preparation method. It is suitable for waterproofing projects such as industrial metal roofs, basements, tunnels, and cement-based surfaces, and is especially compatible with self-adhesive membrane standards designed for direct full adhesion to metal and concrete substrates. Background Technology
[0002] In the design process of self-adhesive rolls, a balance between adhesive performance and low-temperature performance needs to be considered in the formulation design. This is especially true for Type II self-adhesive rolls in the GB 23441-2009 standard, which requires low-temperature flexibility without cracking at -30℃ and a peel strength of ≥1.5N / mm between the roll and aluminum sheet. Traditional formulations require the addition of a large amount of softening oil to improve low-temperature performance. However, high levels of softening oil significantly reduce the adhesion strength between the asphalt adhesive and metal (aluminum sheet, galvanized sheet, color steel sheet) and cement-based surfaces, easily leading to delamination and detachment. Conventional solutions include: 1) increasing the amount of SBR / tackifying resin, which increases costs and results in poor high-temperature stability; 2) increasing the amount of SBS, which leads to excessive cohesion in the adhesive, making full adhesion to metal substrates difficult and resulting in low peel strength. Furthermore, even with improved self-adhesive adhesion, traditional PE / PET release films tend to stick to the adhesive in high summer temperatures, making film removal difficult and affecting construction efficiency.
[0003] Existing technological shortcomings:
[0004] 1. Self-adhesive formulations, especially Type II formulations conforming to standard 23441, have high softening oil content, resulting in poor adhesion to metal substrates and low peel strength of aluminum plates.
[0005] 2. Using a high SBS formulation to reduce the amount of softening oil will result in excessive cohesion and low full adhesion to the metal substrate.
[0006] 3. Conventional thickening systems are costly and have poor aging resistance;
[0007] 4. The release liner is bonded at high temperatures after the bonding process, making construction inconvenient. Summary of the Invention
[0008] Purpose of the invention
[0009] To address the shortcomings of existing technologies, a high-adhesion self-adhesive modified bitumen waterproof membrane and its preparation method are provided. By adding silane coupling agent KH550 / A17 at low temperature, the adhesion to metal / cement base surfaces is improved, the amount of SBR / tackifying resin is reduced, the anti-sticking properties of the release liner are optimized, and the low-temperature toughness, adhesion and workability are balanced.
[0010] Technical solution
[0011] This invention relates to a highly adhesive self-adhesive modified bitumen waterproof membrane, employing the following technical solution:
[0012] 1. Roll structure: base material + self-adhesive material + multi-layer silicone oil release film;
[0013] 2. Self-adhesive compound formulation (parts by weight): 70# asphalt 100, 200# asphalt 40-70, naphthenic oil 10-30, high-saturation oil 15-30, tackifying resin 5-10, SBR 3-6, SBS 8-15, talc 20-25, antioxidant 0.5-1.5, silane coupling agent 2‰-5‰;
[0014] 3. Coupling agent addition: KH550 / A171 alone or in combination, added at a low temperature below 180℃ to avoid high-temperature aging and failure;
[0015] 4. Release film: The PET / PE substrate is coated with multiple layers of modified silicone oil to reduce high-temperature adhesion.
[0016] 5. Preparation process: High-temperature shearing to form adhesive → Cooling and adding coupling agent → Coating and film coating.
[0017] Preferably, the present invention relates to a highly adhesive self-adhesive modified bitumen waterproof membrane, comprising a sequentially laminated structure:
[0018] The middle layer is the tire base;
[0019] Both the upper and lower sides of the tire base are coated with a self-adhesive modified asphalt rubber layer;
[0020] The self-adhesive modified asphalt adhesive layer is covered with a multi-layer silicone oil release film on the underside and a PE film or a multi-layer silicone oil release film on the top side.
[0021] The self-adhesive modified asphalt compound, by weight, comprises: 100 parts of 70# petroleum asphalt, 40-70 parts of 200# petroleum asphalt, 10-30 parts of tackifying softening oil, 15-30 parts of high-saturation softening oil, 5-10 parts of tackifying resin, 3-6 parts of styrene-butadiene rubber (SBR), 8-15 parts of linear SBS, 20-25 parts of talc, 0.5-1.5 parts of antioxidant, and 2‰-5‰ of silane coupling agent.
[0022] Preferably, the silane coupling agent is one or a combination of two of KH550 and A171;
[0023] Preferably, during the preparation of the rubber compound, the silane coupling agent is added after the asphalt system has cooled to below 180°C, and the subsequent temperature is controlled not to exceed 180°C.
[0024] Preferably, the tire base is a polyester tire or a glass fiber reinforced polyester tire, with a thickness of 0.8–1.3 mm;
[0025] The self-adhesive modified asphalt adhesive layer has a single-sided thickness of 0.8–1.3 mm; the multi-layer silicone oil release film is a PET or PE substrate, with modified silicone oil layers coated on the surface in two or more layers.
[0026] Preferably, the high-saturation softening oil has a saturation content ≥70% and a viscosity ≤10000mPa•s at 25℃; the viscosity-enhancing softening oil is a naphthenic oil with aromatics ≥55%.
[0027] Preferably, the linear SBS has a styrene content of 32% to 42%; the SBR is a powder with an ash content of ≤20%; and the antioxidant is one of B900, 168, and 1010.
[0028] Preferably, the silane coupling agent is one or a combination of two of KH550 and A171. Preferably, the addition method is to add the silane coupling agent after the modifier in the rubber compound has been activated and the filler has been added, by first adding the filler and continuously stirring to lower the temperature, and then adding the silane coupling agent simultaneously.
[0029] Preferably, the method for obtaining the high-adhesion self-adhesive modified bitumen waterproof membrane includes the following steps:
[0030] 1) Preparation of the asphalt base system: Add 70# asphalt, 200# asphalt, thickening softening oil, and high saturation softening oil to the reactor and heat to 180±5℃; add SBS and SBR, and shear at high speed for 30 min, then raise the temperature to 195±5℃ and shear at a constant temperature for 60 min.
[0031] 2) Cooling and adding coupling agent: Cool the system to below 180℃, add talc, antioxidant, and tackifying resin, stir for 30 minutes, then add silane coupling agent, continue stirring for 30 minutes, and then discharge the material;
[0032] 3) Roll forming: The base material is unwound, coated with self-adhesive material on both sides, covered with multiple layers of silicone oil release film, cooled, wound up, and slit to obtain the finished product.
[0033] Preferably, the coupling agent is added at a temperature of 165-180°C in step 2), more preferably 170-178°C, and even more preferably 175°C.
[0034] Beneficial effects
[0035] This application achieves the following technical effects through: designing the roll material structure as a base material + self-adhesive compound + multi-layer silicone oil release film; adjusting the self-adhesive compound formulation; adding coupling agent in a specific manner; and combining the release film with a unique preparation process:
[0036] 1. Significantly improved adhesion: The coupling effect of silane coupling agent increases the peel strength of aluminum plates by 50%~80%; the adhesion of galvanized plates, color steel plates, and cement-based surfaces is simultaneously optimized;
[0037] 2. Formula optimization: Reduce the amount of SBR and tackifying resin, and use SBS + coupling agent as the main component, while taking into account both low-temperature flexibility at -30℃ and full adhesion to metals;
[0038] 3. Good stability: Low-temperature coupling agent is added to avoid high-temperature failure, ensuring stable performance;
[0039] 4. Construction-friendly: Multi-layer silicone oil release film, easy to tear in summer;
[0040] 5. Controllable costs: Reducing the use of expensive tackifying resins and SBR lowers overall costs. Detailed Implementation
[0041] The preparation steps of the waterproof membrane in the specific implementation are roughly as follows:
[0042] 1) Preparation of the asphalt base system: Add 70# asphalt, 200# asphalt, thickening softening oil, and high saturation softening oil to the reactor and heat to 180±5℃; add SBS and SBR, and shear at high speed for 30 min, then raise the temperature to 195±5℃ and shear at a constant temperature for 60 min.
[0043] 2) Cooling and adding coupling agent: Cool the system to below 180℃, add talc, antioxidant, and tackifying resin, stir for 30 minutes, then add silane coupling agent, continue stirring for 30 minutes, and then discharge the material;
[0044] 3) Roll forming: The base material is unwound, coated with self-adhesive material on both sides, covered with multiple layers of silicone oil release film, cooled, wound up, and slit to obtain the finished product.
[0045] Example 1
[0046] Self-adhesive compound formulation (parts by weight):
[0047] 70# asphalt 100
[0048] 200# Asphalt 50
[0049] Naphthenic oil 20
[0050] Highly saturated oil 25
[0051] Terpene resin 8
[0052] SBR 5
[0053] SBS 12
[0054] Talc 22
[0055] Antioxidant 1.0
[0056] KH550 2‰;
[0057] Process: 195℃ shearing → 175℃ coupling agent addition; Base material: 1.0mm polyester base; Release film: PET silicone oil film; Performance: Low temperature flexibility -32℃, aluminum plate peeling 1.8N / mm (55% improvement), color steel plate 1.6N / mm, cement-based surface 1.4N / mm, easy-tear film in summer.
[0058] Example 2
[0059] Self-adhesive compound formulation:
[0060] 70# asphalt 100
[0061] 200# Asphalt 55
[0062] Naphthenic oil 22
[0063] Highly saturated oil 22
[0064] Rosin Resin 6
[0065] SBR 4
[0066] SBS 14
[0067] Talc 23
[0068] Antioxidant 1.0
[0069] A171 3‰;
[0070] Performance: Low temperature gentleness -33℃, aluminum plate peeling 2.1N / mm (70% improvement), color steel plate 1.8N / mm, cement base surface 1.5N / mm.
[0071] Example 3
[0072] Self-adhesive compound formulation:
[0073] 70# asphalt 100
[0074] 200# Asphalt 60
[0075] Naphthenic oil 25
[0076] Highly saturated oil 28
[0077] DSPD Resin 7
[0078] SBR 3
[0079] SBS 15
[0080] Talc 24
[0081] Antioxidant 1.0
[0082] KH550 2‰ + A171 2‰;
[0083] Performance: Low temperature gentleness -34℃, aluminum plate peeling 2.4N / mm (80% improvement), color steel plate 2.0N / mm, cement base surface 1.7N / mm.
[0084] Example 4
[0085] Self-adhesive compound formulation:
[0086] 70# asphalt 100
[0087] 200# Asphalt 45
[0088] Naphthenic oil 18
[0089] High saturated oil 30
[0090] Terpene resin 5
[0091] SBR3
[0092] SBS15
[0093] Talc 25
[0094] Antioxidant 1.2
[0095] KH550 5‰;
[0096] Performance: Low temperature gentleness -31℃, aluminum sheet peeling 2.2N / mm (75% improvement), optimal cost.
[0097] Comparative Example 1
[0098] Formulation: Same as Example 3, except that the coupling agent is removed, the tackifying resin is increased to 12 parts, and the SBR is increased to 8 parts;
[0099] Results: Aluminum plate peeling 1.3 N / mm, low temperature flexibility -30℃, high design cost, high temperature slippage.
[0100] Comparative Example 2
[0101] Formulation: Same as in Example 3, except the coupling agent is added at 190°C;
[0102] Result: Aluminum plate peeling was 1.5 N / mm, an improvement of only 20%, which is poor.
[0103] Comparative Example 3
[0104] Formulation: Same as Example 3, with coupling agent 1‰;
[0105] Result: Aluminum plate peeling was 1.4 N / mm, an increase of 15%, but the effect did not meet the standard.
[0106] Comparative Example 4
[0107] Formulation: Same as Example 3, except that the separator is made of ordinary PE film;
[0108] Result: High temperatures in summer caused the film to adhere, making it difficult to remove and resulting in low construction efficiency.
[0109] Performance Comparison Table
[0110]
[0111] This invention designs a self-adhesive modified bitumen waterproof membrane that utilizes the coupling effect of a silane coupling agent to enhance the peel strength of the adhesive on aluminum plates. Compared to a reference system, this design can improve the peel strength of aluminum plates by 50% to 80%. In practical applications, it optimizes adhesion to galvanized steel sheets, color steel sheets, and cement-based surfaces. It reduces the amount of SBR and tackifying resin used, primarily using SBS + coupling agent, while also meeting the high and low temperature performance requirements of the product design and ensuring adhesion to metal substrates. The addition of a coupling agent at low temperatures prevents high-temperature failure and ensures stable performance. A multi-layer silicone oil release film is used, making it easy to peel off in summer. The reduction in the addition of expensive tackifying resin and SBR lowers the overall cost.
[0112] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the essence and scope of the technical solutions of the present invention.
Claims
1. A highly adhesive self-adhesive modified bitumen waterproof membrane, characterized in that, Including structures that are compounded sequentially: The middle layer is the tire base; Both the upper and lower sides of the tire base are coated with a self-adhesive modified asphalt rubber layer; The self-adhesive modified asphalt adhesive layer is covered with a multi-layer silicone oil release film on the underside and a PE film or a multi-layer silicone oil release film on the top side. The self-adhesive modified asphalt compound, by weight, comprises: 100 parts of 70# petroleum asphalt, 40-70 parts of 200# petroleum asphalt, 10-30 parts of tackifying softening oil, 15-30 parts of high-saturation softening oil, 5-10 parts of tackifying resin, 3-6 parts of styrene-butadiene rubber (SBR), 8-15 parts of linear SBS, 20-25 parts of talc, 0.5-1.5 parts of antioxidant, and 2‰-5‰ of silane coupling agent; The silane coupling agent is one or a combination of two of KH550 and A171; during the preparation of the rubber compound, the silane coupling agent must be added after the asphalt system has cooled to below 180°C, and the subsequent temperature must be controlled not to exceed 180°C.
2. The high-adhesion self-adhesive modified bitumen waterproof membrane according to claim 1, characterized in that: The base material is polyester or glass fiber reinforced polyester, with a thickness of 0.8–1.3 mm; the self-adhesive modified asphalt adhesive layer has a single-sided thickness of 0.8–1.3 mm; the multi-layer silicone oil release film is a PET or PE substrate, with modified silicone oil layers coated on the surface in two or more layers.
3. The high-adhesion self-adhesive modified bitumen waterproof membrane according to claim 1, characterized in that: The high-saturation softening oil has a saturation content ≥70% and a viscosity ≤10000mPa•s at 25℃; the thickening softening oil is a naphthenic oil with aromatics ≥55%; the linear SBS has a styrene content of 32%~42%; the SBR is a powder with an ash content ≤20%; and the antioxidant is one of B900, 168, and 1010.
4. The high-adhesion self-adhesive modified bitumen waterproof membrane according to claim 1, characterized in that: The silane coupling agent is one or a combination of two of KH550 and A171. It is added after the modifier in the rubber compound has been activated and the filler has been added. The filler is added first and the mixture is stirred continuously to reduce the temperature. Then the silane coupling agent is added simultaneously.
5. A method for preparing the high-adhesion self-adhesive modified bitumen waterproof membrane according to any one of claims 1 to 4, characterized in that, Includes the following steps: 1) Preparation of the asphalt base system: Add 70# asphalt, 200# asphalt, tackifying softening oil, and high-saturation softening oil to the reactor and heat to 180±5℃; add SBS and SBR, and shear at high speed for 30 min, then raise the temperature to 195±5℃ and shear at a constant temperature for 60 min; 2) Cooling and adding coupling agent: Cool the system to below 180℃, add talc, antioxidant, and tackifying resin, stir for 30 min, then add silane coupling agent, continue stirring for 30 min, and discharge the material; 3) Roll forming: Unwind the base material, coat both sides with self-adhesive material, cover with multiple layers of silicone oil release film, cool, rewind, and slit to obtain the finished product.