A Wide-Temperature-Range Creep-Controllable Interlayer Film for Laminated Glass, Its Preparation Method and Application
By optimizing the PVB resin structure and introducing compound plasticizers, combined with rapid cooling and shaping technology, the problems of easy bubbling of the interlayer film in laminated glass at high temperatures and the narrow production temperature window have been solved. Wide-temperature-range creep modulus control and quantitative design of surface micro-bump density have been achieved, making it suitable for the production of large-area and curved glass.
Patent Information
- Application Number
- CN202611394320.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-09
- Publication Date
- 2026-11-17
AI Technical Summary
Existing interlayer films in laminated glass are prone to bubbling and delamination at high temperatures, have unclear embossing designs, narrow production temperature windows, and are difficult to balance in terms of overall performance, making it impossible to meet the production needs of large-area and curved glass.
By optimizing the ternary structural unit ratio of PVB resin and introducing compound plasticizers, combined with rapid cooling and shaping technology, the creep modulus and surface micro-bump density over a wide temperature range can be precisely controlled, thereby achieving creep modulus control and surface morphology optimization across multiple temperature ranges.
It widens the pre-compression temperature window, improves the high-temperature stability and production adaptability of the interlayer film in laminated glass, and is suitable for large-area and curved glass, with high production yield and stability.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of polymer laminated glass materials technology, and in particular to a laminated glass interlayer with wide temperature range creep control, its preparation method and application. Background Technology
[0002] Laminated glass, as a safety glass product, is widely used in the automotive, construction, rail transportation, and photovoltaic industries. Common applications include automotive glass, building curtain walls, rail transportation glass, and photovoltaic modules. The performance of laminated glass depends on the comprehensive performance of the interlayer. Most existing interlayers use polyvinyl butyral (PVB) resin as the base material, and the degassing effect is improved by controlling the creep modulus at a single temperature of 60°C. The surface embossing texture is mostly designed based on experience and lacks quantitative standards.
[0003] PVB resin is a random copolymer composed of three structural units: vinyl alcohol (VA) units, vinyl butyral (VB) units, and vinyl acetate (VAc) units. VA units can form strong hydrogen bonds with the silanol groups on the glass surface, which is crucial for ensuring high adhesion strength between the PVB interlayer and the glass. However, excessive VA unit content can cause the PVB interlayer to absorb water easily and reduce its weather resistance. VB units improve the tensile strength, toughness, and compatibility with plasticizers in the PVB interlayer. Insufficient VB units will cause the resin to harden and reduce its impact resistance, while excessive VB units will weaken the adhesion between the PVB interlayer and the glass. VAc units impart a certain degree of water resistance to the PVB resin, but excessive residual amounts will significantly reduce the optical properties, weather resistance, and adhesion of the PVB interlayer. Current solutions lack systematic optimization of the proportions of each structural unit in the PVB resin, often focusing only on the single indicator of butyralization degree, making it difficult to balance adhesion, processability, and weather resistance. In addition, existing plasticizer systems mostly use a single plasticizer, making it difficult to balance plasticizing efficiency and migration resistance under wide temperature range conditions.
[0004] Based on the above background, existing interlayer films for laminated glass generally have the following defects: First, they only focus on the modulus below 60℃, and their high-temperature (70~80℃) stability is insufficient, making them prone to secondary bubbling and delamination; Second, the embossing design does not have a clear numerical range, making it prone to adhesion or poor degassing; Third, the pre-pressing temperature window is narrow, making it difficult to adapt to the production needs of large-area, curved glass; Fourth, it is difficult to balance the overall performance, and it cannot simultaneously meet the requirements of adhesion resistance, easy degassing, and high-temperature stability.
[0005] Therefore, developing a laminated glass interlayer with balanced performance across the entire temperature range, quantifiable design, and strong adaptability is an urgent problem to be solved in this field. Summary of the Invention
[0006] In view of this, the present invention provides a laminated glass interlayer with wide temperature range creep controllable, its preparation method and application. The laminated glass interlayer with wide temperature range creep controllable provided by the present invention has controllable creep modulus in multiple temperature ranges and excellent surface morphology.
[0007] This invention provides a laminated glass interlayer with wide-temperature-range creep control, and the creep modulus is as follows: creep modulus at 20℃ is 120~250 g / cm³. 2 The creep modulus at 40℃ is 70~150 g / cm³. 2 The creep modulus at 60℃ is 50~120 g / cm³. 2 The creep modulus at 80℃ is 40~90 g / cm³. 2 The density of surface microbumps in the wide-temperature-range creep-controllable interlayer glass film is 150~350 per cm. 2 .
[0008] Preferably, the raw materials for the wide-temperature-range creep-controllable interlayer glass include polyvinyl butyral resin and a plasticizer; the polyvinyl butyral resin includes high molecular weight polyvinyl butyral resin and low molecular weight polyvinyl butyral resin; the high molecular weight polyvinyl butyral resin has a number average molecular weight of not less than 100,000 Daltons and a weight average molecular weight of 175,000 to 210,000 Daltons; the low molecular weight polyvinyl butyral resin has a degree of polymerization of 1800 to 2500 and a weight average molecular weight of less than 50,000 Daltons; the content of low molecular weight polyvinyl butyral resin in the polyvinyl butyral resin is not less than 10 wt%; the degree of butyralization of the polyvinyl butyral resin is 66 to 70 mol%; in the polyvinyl butyral resin, the mass fraction of vinyl alcohol (hydroxyl unit) is 17% to 22%, the mass fraction of vinyl butyral (butyral group unit) is 75% to 80%, and the mass fraction of vinyl acetate (acetyl group unit) is 1% to 3%.
[0009] Preferably, the mass ratio of the polyvinyl butyral resin to the plasticizer is 100:35~45.
[0010] Preferably, the raw materials of the interlayer of the laminated glass with wide temperature range creep control also include functional additives; the functional additives include one or more of ultraviolet absorbers, antioxidants, heat stabilizers and adhesion modifiers.
[0011] Preferably, the mass ratio of the polyvinyl butyral resin to the ultraviolet absorber is 100:0.2~0.5; and the mass ratio of the polyvinyl butyral resin to the adhesive modifier is 100:0.02~0.2.
[0012] The present invention also provides a method for preparing the interlayer film of laminated glass with wide temperature range creep control as described above, comprising the following steps: (1) Mix PVB resin, plasticizer and functional additives to obtain a mixture; (2) The mixture is melted and kneaded and then extruded into a film to obtain a film preform; (3) After the preform is rapidly cooled and shaped, it is embossed and shaped to obtain the interlayer film of the laminated glass with wide temperature range creep control.
[0013] Preferably, the melt mixing method is twin-screw extrusion; the barrel temperature of the twin-screw extrusion is sequentially divided into a feeding section, a melting section, and a homogenization section; the temperature of the feeding section is 100~120℃; the temperature of the melting section is 135~155℃; the temperature of the homogenization section is 160~175℃; the die temperature of the twin-screw extrusion is 165~175℃; the screw speed of the twin-screw extrusion is 200~350 r / min; and the feeding rate of the twin-screw extrusion is based on a melt pressure of 5~8 MPa.
[0014] Preferably, the rapid cooling and shaping includes the following steps: the preform is drawn into the rapid cooling roller group under the traction of the traction roller for cooling and shaping; the ratio of the traction speed to the linear speed of the twin-screw extrusion is 1.05~1.15:1; the surface temperature of the rapid cooling roller in the rapid cooling roller group is 55~65℃.
[0015] The present invention also provides the application of the wide-temperature-range creep-controllable interlayer film of laminated glass described in the above-described scheme or the wide-temperature-range creep-controllable interlayer film of laminated glass obtained by the preparation method described in the above-described scheme in the fields of laminated glass, automotive, construction or photovoltaic.
[0016] The present invention also provides a laminated glass comprising two surface glass sheets and a wide-temperature-range creep-controllable interlayer film disposed between the two surface glass sheets, wherein the wide-temperature-range creep-controllable interlayer film is the wide-temperature-range creep-controllable interlayer film described in the above-described scheme or the wide-temperature-range creep-controllable interlayer film obtained by the preparation method described in the above-described scheme.
[0017] Compared with the prior art, the present invention has achieved the following beneficial effects: This invention achieves precise control over the creep modulus of a wide-temperature-range creep-controlled interlayer glass membrane at four key temperature points: 20℃, 40℃, 60℃, and 80℃, through rapid cooling and shaping. It also controls the density of surface micro-bumps in the wide-temperature-range creep-controlled interlayer glass membrane, enabling it to balance room-temperature adhesion resistance, mid-temperature degassing efficiency, and high-temperature sealing stability, while significantly widening the pre-compression temperature window. Based on multi-temperature-range creep modulus control, this invention solves the technical problems of existing products, such as high-temperature blistering, ambiguous embossing design, narrow production temperature window, and unbalanced overall performance. This makes the wide-temperature-range creep-controlled interlayer glass membrane suitable for the automotive, construction, and laminated glass industries, especially for large-area or curved laminated glass, and offers advantages such as high production yield and good stability.
[0018] Specifically, the mechanism of rapid cooling and shaping in this invention is as follows: This invention controls the surface temperature of the rapid cooling roller used for rapid cooling and shaping, and the cooling rate is linked and matched with the rate of twin-screw extrusion. By adjusting the cooling crystallization rate, the size distribution of the microcrystalline region in the film material is adjusted.
[0019] This invention further achieves a systematic balance between adhesion, processability, and weather resistance by optimizing the ternary structural unit ratio of PVB resin (VA unit 15%~22%, VB unit 75%~80%, VAc unit 1%~3%). By limiting the number average molecular weight of high molecular weight PVB resin to not less than 100,000 Daltons and the weight average molecular weight to 175,000~210,000 Daltons, and combining it with a bimodal molecular weight distribution design (containing up to 10 wt% low molecular weight PVB resin), it balances melt processing fluidity and the mechanical strength of the PVB interlayer. By introducing a compound plasticizer system and functional additives such as antioxidants and heat stabilizers, it further improves plasticizing efficiency, migration resistance, and processing thermal stability under a wide temperature range. Detailed Implementation
[0020] This invention provides a laminated glass interlayer with wide-temperature-range creep control, and the creep modulus is as follows: creep modulus at 20℃ is 120~250 g / cm³. 2 The creep modulus at 40℃ is 70~150 g / cm³. 2 The creep modulus at 60℃ is 50~120 g / cm³. 2 The creep modulus at 80℃ is 40~90 g / cm³. 2 The density of surface microbumps in the wide-temperature-range creep-controllable interlayer glass film is 150~350 per cm. 2 .
[0021] In this invention, the raw materials for the wide-temperature-range creep-controllable interlayer glass film may include polyvinyl butyral resin and plasticizer.
[0022] In this invention, the polyvinyl butyral resin may include high molecular weight polyvinyl butyral resin and low molecular weight polyvinyl butyral resin; the high molecular weight polyvinyl butyral resin may have a number average molecular weight of not less than 100,000 Daltons, specifically 150,000 Daltons or 200,000 Daltons, and a weight average molecular weight of 175,000 to 210,000 Daltons, specifically 200,000 Daltons; the low molecular weight polyvinyl butyral resin may have a degree of polymerization of 1800 to 2500, specifically 1900, 2000, 2100, 2200, 2300 or 2400, and a weight average molecular weight of less than 50,000 Daltons, specifically 2,000 Daltons or 4,000 Daltons; the polyvinyl butyral resin may have a number average molecular weight of not less than 100,000 Daltons, specifically 150,000 Daltons or 200,000 Daltons; the low molecular weight ...0 Daltons; the low molecular weight polyvinyl butyral resin may have a number average molecular weight of not less than 100,000 Daltons, specifically 150,000 Daltons or 2000 Daltons; the low molecular weight polyvinyl butyral resin may have a number average molecular weight of not less than 100,000 Daltons, specifically 150, The content of low molecular weight polyvinyl butyral resin in the polyvinyl butyral resin can be no less than 10 wt%, specifically 15 wt% or 25 wt%; the degree of butyralization of the polyvinyl butyral resin can be 66-70 mol%, specifically 67 mol%, 68 mol%, or 69 mol%; in the polyvinyl butyral resin, the mass fraction of vinyl alcohol (hydroxyl unit) can be 17%-22%, specifically 18%, 20%, or 21%, the mass fraction of vinyl butyral (butyral group unit) can be 75%-80%, specifically 76%, 77%, 78%, or 79%, and the mass fraction of vinyl acetate (acetyl group unit) can be 1%-3%, specifically 1.5%, 2%, or 2.5%. The polyvinyl butyral resin used in this invention has a bimodal molecular weight distribution, which is beneficial for improving melt processing performance without sacrificing the strength and impact resistance of the interlayer of the laminated glass.
[0023] In this invention, the plasticizer can be triethylene glycol di(2-ethylhexanoate) (3GO) or a compound plasticizer; the compound plasticizer can include at least two of triethylene glycol di(2-ethylhexanoate), triethylene glycol diisooctanoate (3G8), di(butoxyethoxyethyl) adipic acid ester (DBEEA), and benzoate plasticizers; the benzoate plasticizers can include diethylene glycol dibenzoate (DEDB), dipropylene glycol dibenzoate (DPGDB), tripropylene glycol dibenzoate, 2,2,4-trimethyl-1,3-pentanediol dibenzoate, etc. The compound plasticizer comprises one or more of benzyl benzoate, isodecanyl benzoate, and 2-ethylhexyl benzoate; in the compound plasticizer, the mass ratio of triethylene glycol di(2-ethylhexanoate) to benzoate plasticizer can be 1~3:1, specifically 2:1; the mass ratio of triethylene glycol diisooctanoate to di(butoxyethoxyethyl) adipate can be 20~30:5~10, specifically 25:7 or 25:8; the mass ratio of di(butoxyethoxyethyl) adipate to benzoate plasticizer can be 5~10:1~5, specifically 7:2, 7:3 or 7:4. The compounding method of the plasticizer in this invention can achieve a balance between plasticizing efficiency and migration resistance, and has a synergistic effect on widening the pre-compression temperature window.
[0024] In this invention, the mass ratio of polyvinyl butyral resin to plasticizer can be 100:35~45, specifically 100:37, 100:39, 100:41 or 100:43.
[0025] In this invention, the raw materials of the interlayer glass with wide temperature range creep control may also include functional additives; the functional additives may include one or more of ultraviolet absorbers, antioxidants, heat stabilizers and adhesion modifiers.
[0026] In this invention, the ultraviolet absorber can be a benzotriazole ultraviolet absorber; the benzotriazole ultraviolet absorber can be UV-571 ultraviolet absorber or UV-5411 ultraviolet absorber.
[0027] In this invention, the mass ratio of the polyvinyl butyral resin and the ultraviolet absorber can be 100:0.2~0.5, specifically 100:0.3 or 100:0.4.
[0028] In this invention, the antioxidant may be one or more of hindered phenolic antioxidants and phosphite antioxidants; the hindered phenolic antioxidant may be Irganox 1010; and the phosphite antioxidant may be Irgafos168.
[0029] In this invention, the mass ratio of polyvinyl butyral resin to antioxidant can be 100:0.1 to 1.0, specifically 100:0.3, 100:0.5 or 100:0.8.
[0030] In this invention, the heat stabilizer may include one or both of organotin stabilizers and calcium-zinc stabilizers; the organotin stabilizers may include one or more of methyltin thiols (e.g., grades YT181, MS1928), octyltin thiols, and dibutyltin dilaurate; the calcium-zinc stabilizers may include a compound of calcium stearate and zinc stearate; the calcium-zinc stabilizers may also include one or more of β-diketone stabilizers, polyols, epoxy compounds, and hydrotalcite; the β-diketone stabilizers may include one or more of dibenzoylmethane and stearoylbenzoylmethane; the polyol may be pentaerythritol; and the epoxy compound may be epoxidized soybean oil. This invention uses heat stabilizers to inhibit thermal degradation during processing.
[0031] In this invention, the mass ratio of the polyvinyl butyral resin and the heat stabilizer can be 100:0.1 to 0.5, specifically 100:0.2, 100:0.3 or 100:0.4.
[0032] In this invention, the adhesive modifier can be one or both of magnesium acetate solution and potassium formate solution; based on metal ions, the total proportion of potassium ions and / or sodium ions in the adhesive modifier (the proportion of the mass of potassium ions and / or sodium ions to the total mass of polyvinyl butyral resin, plasticizer, and functional additives) can not exceed 80 ppm, specifically 70 ppm, 50 ppm, or 40 ppm. This invention achieves precise control of adhesive strength through the adhesive modifier of the above specifications.
[0033] In this invention, the mass ratio of the polyvinyl butyral resin and the adhesive modifier can be 100:0.02~0.2, specifically 100:0.05, 100:0.07, 100:0.09, 100:0.11, 100:0.15 or 100:0.17.
[0034] In this invention, the density of surface microbumps in the wide-temperature-range creep-controllable interlayer glass film is 150~350 per cm. 2 Specifically, it can be 170 pieces / cm 2 190 pieces / cm 2 210 pieces / cm 2 230 pieces / cm 2 250 pieces / cm 2 270 pieces / cm 2 290 pieces / cm 2310 pieces / cm 2 Or 330 pieces / cm 2 .
[0035] In this invention, the shape of a single surface micro-bump can be hemispherical (dot-like protrusion), and the height of the micro-bump (i.e., embossing depth) can be 30~100μm; the arrangement of the surface micro-bump can be regular, and the regular arrangement can be a parallel arrangement with equal spacing, a parallel arrangement with partially unequal spacing, a grid arrangement with equal spacing, or a grid arrangement with partially unequal spacing.
[0036] In this invention, the thickness of the interlayer film of the laminated glass with wide temperature range creep control can be 0.7~0.8mm, specifically 0.76mm.
[0037] The core of the wide-temperature-range creep-controllable interlayer glass membrane provided by this invention lies in the precise control of the four-segment creep modulus and the quantitative design of the surface micro-bump density, which enables it to possess the aforementioned excellent properties. Specifically, the creep modulus at 20℃ (room temperature) is 120~250 g / cm³. 2 This ensures that the interlayer film of the laminated glass exhibits controllable creep over a wide temperature range, preventing adhesion and facilitating operation; the creep modulus at 40℃ (initial pre-compression stage) is 70~150 g / cm³. 2 It can prevent premature sealing of the edges and avoid air retention; the creep modulus at 60℃ (core degassing zone) is 50~120g / cm³. 2 It has a good balance of softness and hardness, which is conducive to the collapse of embossing and the expulsion of air; the creep modulus at 80℃ (high-temperature sealed zone) is 40~90g / cm. 2 The material is moderately softened to form a dense sealing layer, preventing secondary bubbling. The density of surface micro-bumps is controlled at 150~350 per cm³. 2 It can simultaneously provide both an exhaust channel and anti-adhesion support.
[0038] The present invention also provides a method for preparing the interlayer film of laminated glass with wide temperature range creep control as described above, comprising the following steps: (1) Mix PVB resin, plasticizer and functional additives to obtain a mixture; (2) The mixture is melted and kneaded and then extruded into a film to obtain a film preform; (3) After the preform is rapidly cooled and shaped, it is embossed and shaped to obtain the interlayer film of the laminated glass with wide temperature range creep control.
[0039] This invention involves mixing PVB resin, plasticizer, and functional additives to obtain a mixture. In this invention, the mixing can be achieved through stirring.
[0040] After obtaining the mixture, the present invention melts and kneads the mixture to form a film, thereby obtaining a film preform. In the present invention, the melt kneading method can be twin-screw extrusion; the twin-screw extrusion equipment can be a twin-screw extruder; the barrel temperature of the twin-screw extrusion can be sequentially divided into a feeding section, a melting section, and a homogenization section; the temperature of the feeding section can be 100~120℃, specifically 105℃, 110℃, or 115℃; the temperature of the melting section can be 135~155℃, specifically 140℃, 145℃, or 150℃; the temperature of the homogenization section can be 160~175℃, specifically 165℃ or 170℃; the die head temperature of the twin-screw extruder can be 165~175℃, specifically 168℃, 170℃, or 172℃.
[0041] In this invention, the screw speed of the twin-screw extruder can be 200~350 r / min, specifically 250 r / min or 300 r / min.
[0042] In this invention, the feeding rate of the twin-screw extruder can be based on a melt pressure of 5-8 MPa, specifically 6 MPa or 7 MPa.
[0043] After obtaining the preform, the present invention rapidly cools and shapes the preform, followed by embossing and shaping, to obtain the interlayer film of laminated glass with wide temperature range creep control. In the present invention, the rapid cooling and shaping may include the following steps: the preform is drawn into a rapid cooling roller group under the traction of traction rollers for cooling and shaping.
[0044] In this invention, the ratio of the traction speed to the linear speed of the twin-screw extrusion can be 1.05 to 1.15:1, specifically 1.08:1, 1.1:1, or 1.13:1.
[0045] In this invention, the surface temperature of the quenching rollers in the quenching roller assembly can be 55~65℃, specifically 60℃. This invention controls the surface temperature of the quenching rollers used for quenching and shaping, linking the cooling rate with the twin-screw extrusion rate, and adjusts the microcrystalline region size distribution within the film material by regulating the cooling crystallization rate.
[0046] In this invention, the embossing and shaping equipment may include an embossing roller.
[0047] In this invention, the embossing and shaping process may also include cooling and then winding.
[0048] The present invention also provides the application of the wide-temperature-range creep-controllable interlayer film of laminated glass described in the above-described scheme or the wide-temperature-range creep-controllable interlayer film of laminated glass obtained by the preparation method described in the above-described scheme in the fields of laminated glass, automotive, construction or photovoltaic.
[0049] The present invention also provides a laminated glass comprising two surface glass sheets and a wide-temperature-range creep-controllable interlayer film disposed between the two surface glass sheets, wherein the wide-temperature-range creep-controllable interlayer film is the wide-temperature-range creep-controllable interlayer film described in the above-described scheme or the wide-temperature-range creep-controllable interlayer film obtained by the preparation method described in the above-described scheme.
[0050] To further illustrate the present invention, the technical solutions of the present invention will be clearly and completely described below in conjunction with the embodiments thereof.
[0051] Example 1: 1) Raw material mixing: Weigh 100 parts by weight of PVB resin (degree of butyralization 68 mol%, of which ethylene alcohol unit mass fraction 18%, ethylene alcohol butyral unit mass fraction 79%, vinyl acetate unit mass fraction 3%; high molecular weight PVB resin number average molecular weight 120,000 Daltons, weight average molecular weight 190,000 Daltons; low molecular weight PVB resin weight average molecular weight less than 50,000 Daltons, degree of polymerization 2000, content in PVB resin 12 wt%), 40 parts of 3GO plasticizer, 0.3 parts of UV-571 ultraviolet absorber, 0.021 parts of potassium formate solution (potassium ions account for 70 ppm of all raw materials), 0.3 parts of Irganox 1010 antioxidant and 0.2 parts of calcium zinc heat stabilizer, stir evenly to obtain the mixture.
[0052] 2) Melt extrusion: The mixture is added to a twin-screw extruder. The temperature of each section of the twin-screw extruder is controlled. From the feed port to the die head, the temperature is as follows: feed section 110℃, melting section 145℃, homogenization section 168℃, die head temperature 170℃, screw speed 280r / min. The feed rate is adjusted to stabilize the melt pressure in the range of 5~8MPa. Melt mixing is carried out, and the mixture is extruded into a film to obtain a film preform.
[0053] 3) Rapid cooling and shaping: The preform is drawn into the rapid cooling roller group under the traction of the traction roller. The surface temperature of the rapid cooling roller is controlled at 60℃. The cooling rate is linked and matched with the extrusion rate (the ratio of the traction speed to the linear speed of the twin-screw extrusion is 1.1:1). 4) Embossing and shaping: The density of micro-embossing dots is controlled to 220 dots / cm by embossing with embossing rollers. 2 The micro-bumps are hemispherical in shape, with a height of 65μm, and are arranged in parallel at equal intervals. After cooling and winding, a wide-temperature-range creep-controlled interlayer film of laminated glass with a thickness of 0.76mm is obtained.
[0054] Example 2: The preparation method of this embodiment is the same as that of Example 1, except that: the degree of butyralization of the PVB resin is 67 mol%, the mass fraction of the vinyl alcohol unit is 20%, the mass fraction of the vinyl alcohol butyral unit is 77%, and the mass fraction of the vinyl acetate unit is 3%; the degree of polymerization of the low molecular weight PVB resin is 2200, and its content in the PVB resin is 11 wt%; the number average molecular weight of the high molecular weight PVB resin is 135,000 Daltons, and the weight average molecular weight is 200,000 Daltons; 38 parts of 3GO plasticizer are used; the surface temperature of the quench roll is controlled at 58°C; the ratio of the traction speed to the linear speed of the twin-screw extrusion is 1.08:1; and the micro-bump density is 280 bumps / cm². 2 .
[0055] Example 3: The preparation method of this embodiment is the same as that of Example 1, except that: the degree of butyralization of the PVB resin is 69 mol%, the mass fraction of vinyl alcohol unit is 16%, the mass fraction of vinyl alcohol butyral unit is 80%, and the mass fraction of vinyl acetate unit is 4%; the degree of polymerization of the low molecular weight PVB resin is 1800, and its content in the PVB resin is 10 wt%; the number average molecular weight of the high molecular weight PVB resin is 105,000 Daltons, and the weight average molecular weight is 180,000 Daltons; 42 parts of 3GO plasticizer are used; the surface temperature of the quench roll is controlled at 62°C; the ratio of the traction speed to the linear speed of the twin-screw extrusion is 1.12:1; and the micro-bump density is 180 bumps / cm². 2 .
[0056] Comparative Example 1 (Traditional Narrow Modulus Range): The preparation method of this comparative example is the same as that of Example 1, except that: the degree of polymerization of the PVB resin is 2000, the degree of butyralization is 68 mol%, and the proportion and molecular weight distribution of the ternary structural units are not limited; 40 parts of 3GO plasticizer are used; the surface temperature of the quench roll is controlled at 70°C; the ratio of the traction speed to the linear speed of the twin-screw extrusion is 1.02:1; and the micro-bump density is 100 bumps / cm². 2 Modulus at 60℃: 40 g / cm³ 2 .
[0057] Comparative Example 2 (High Hardness Overmodulus): The preparation method of this comparative example is the same as that of Example 1, except that: the degree of polymerization of the PVB resin is 2500, the degree of butyralization is 65 mol%, and the proportion and molecular weight distribution of the ternary structural units are not limited; 35 parts of 3GO plasticizer are used; the surface temperature of the quench roll is controlled at 50°C; the ratio of the traction speed to the linear speed of the twin-screw extrusion is 1.2:1; and the micro-bump density is 400 bumps / cm². 2 Modulus at 60℃: 130 g / cm³ 2 .
[0058] Test Example 1: The performance of the interlayer films with wide temperature range creep control prepared in Examples 1-3 and the interlayer films prepared in Comparative Examples 1-2 were tested, as follows: 1) Creep modulus: Tested according to JIS K 7115; 2) Micro-bump density: counted using an optical microscope; 3) Pre-compression window: Temperature range where foaming rate ≤ 3%; 4) Number of bubbles: After baking at 145℃ for 2 hours, count the number of bubbles in 100 pieces of interlayer glass with wide temperature range creep control. 5) Self-adhesive peel force: 180° peel force after stacking at 20℃ for 24 hours.
[0059] Table 1. Performance data of Examples 1-3 and Comparative Examples 1-2:
[0060] As shown in Table 1, the interlayer film for laminated glass with wide-temperature-range creep control provided by this invention exhibits uniform modulus across the entire temperature range, meets the high-temperature performance criteria at 80℃, completely solves the problem of secondary bubbling at high temperatures, and demonstrates excellent long-term stability. The surface micro-bump density is quantified, precisely balancing venting efficiency and anti-adhesion properties, and is easy to operate. The pre-compression temperature window is widened to 55~90℃, making it suitable for large-area, curved glass, with a production yield ≥99%. The core range of creep modulus is 50~120 g / cm³. 2 It expands the creep performance of the interlayer film in laminated glass; with excellent comprehensive performance, it can be used in the automotive, construction, laminated glass or photovoltaic fields, and is suitable for multiple application scenarios such as automotive windshields / side windows, building curtain walls, large-area curved glass, photovoltaic laminated glass, etc., with broad application prospects.
[0061] The embodiments of the present invention have been described above. However, these embodiments are for illustrative purposes only and are not intended to limit the scope of the present invention. All other embodiments obtained by those skilled in the art based on the above embodiments of the present invention without inventive effort are within the protection scope of the present invention.
Claims
1. A laminated glass interlayer with wide-temperature-range creep control, characterized in that, The creep modulus is as follows: 120~250 g / cm³ at 20℃. 2 The creep modulus at 40℃ is 70~150 g / cm³. 2 The creep modulus at 60℃ is 50~120 g / cm³. 2 The creep modulus at 80℃ is 40~90 g / cm³. 2 The density of surface microbumps in the wide-temperature-range creep-controllable interlayer glass film is 150~350 per cm. 2 .
2. The interlayer film of laminated glass with wide temperature range creep control according to claim 1, characterized in that, The raw materials for the wide-temperature-range creep-controllable interlayer glass include polyvinyl butyral resin and plasticizer; the polyvinyl butyral resin includes high molecular weight polyvinyl butyral resin and low molecular weight polyvinyl butyral resin; the high molecular weight polyvinyl butyral resin has a number average molecular weight of not less than 100,000 Daltons and a weight average molecular weight of 175,000~210,000 Daltons; the low molecular weight polyvinyl butyral resin has a degree of polymerization of 1800~2500 and a weight average molecular weight of less than 50,000 Daltons; the content of low molecular weight polyvinyl butyral resin in the polyvinyl butyral resin is not less than 10 wt%; the degree of butyralization of the polyvinyl butyral resin is 66~70 mol%; in the polyvinyl butyral resin, the mass fraction of ethylene alcohol is 17%~22%, the mass fraction of ethylene butyral is 75%~80%, and the mass fraction of vinyl acetate is 1%~3%.
3. The interlayer film of laminated glass with wide temperature range creep control according to claim 2, characterized in that, The mass ratio of polyvinyl butyral resin to plasticizer is 100:35~45.
4. The interlayer film of laminated glass with wide temperature range creep control according to claim 1, characterized in that, The raw materials for the wide-temperature-range creep-controllable interlayer glass also include functional additives, which include one or more of ultraviolet absorbers, antioxidants, heat stabilizers, and adhesion modifiers.
5. The interlayer film of laminated glass with wide temperature range creep control according to claim 4, characterized in that, The mass ratio of polyvinyl butyral resin to ultraviolet absorber is 100:0.2~0.5, and the mass ratio of polyvinyl butyral resin to adhesive modifier is 100:0.02~0.
2.
6. A method for preparing a laminated glass interlayer with wide-temperature-range creep control, characterized in that, The wide-temperature-range creep-controlled interlayer glass film is the wide-temperature-range creep-controlled interlayer glass film according to any one of claims 1 to 5, comprising the following steps: (1) Mix PVB resin, plasticizer and functional additives to obtain a mixture; (2) The mixture is melted and kneaded and then extruded into a film to obtain a film preform; (3) After the preform is rapidly cooled and shaped, it is embossed and shaped to obtain the interlayer film of the laminated glass with wide temperature range creep control.
7. The preparation method according to claim 6, characterized in that, The melt mixing method is twin-screw extrusion; the barrel temperature of the twin-screw extrusion is divided into a feeding section, a melting section, and a homogenization section in sequence; the temperature of the feeding section is 100~120℃; the temperature of the melting section is 135~155℃; the temperature of the homogenization section is 160~175℃; the die temperature of the twin-screw extrusion is 165~175℃; the screw speed of the twin-screw extrusion is 200~350 r / min; the feeding rate of the twin-screw extrusion is based on a melt pressure of 5~8 MPa.
8. The preparation method according to claim 6, characterized in that, The rapid cooling and shaping process includes the following steps: the preform is drawn into the rapid cooling roller group under the traction of the traction roller for cooling and shaping; the ratio of the traction speed to the linear speed of the twin-screw extrusion is 1.05~1.15:1; the surface temperature of the rapid cooling roller in the rapid cooling roller group is 55~65℃.
9. An application of a wide-temperature-range creep-controllable interlayer film for laminated glass in the fields of laminated glass, automotive, construction, or photovoltaic, characterized in that, The wide-temperature-range creep-controllable interlayer glass film is the wide-temperature-range creep-controllable interlayer glass film according to any one of claims 1 to 5 or the wide-temperature-range creep-controllable interlayer glass film obtained by the preparation method according to any one of claims 6 to 8.
10. A laminated glass, characterized in that, It includes two surface glass sheets and a wide-temperature-range creep-controllable interlayer glass film disposed between the two surface glass sheets. The wide-temperature-range creep-controllable interlayer glass film is the wide-temperature-range creep-controllable interlayer glass film according to any one of claims 1 to 5 or the wide-temperature-range creep-controllable interlayer glass film obtained by the preparation method according to any one of claims 6 to 8.