A three-layer biaxially stretched polymer dielectric composite film and its preparation method
By using a three-layer biaxially stretched polymer dielectric composite film, and combining BT@BNNs-g-PVDF, PCBM, and ALRB, the problem of interlayer separation in polymer film capacitors under mechanical stress was solved, achieving high breakdown strength and high energy storage density.
Patent Information
- Application Number
- CN202611269887.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-20
- Publication Date
- 2026-11-17
AI Technical Summary
Existing polymer film capacitors are prone to interlayer delamination under bending deformation or electric field-induced mechanical stress, leading to electrical failures, and their dielectric properties can only be improved to a limited extent.
A three-layer biaxially stretched polymer dielectric composite film is adopted, including a high polarization layer, an intermediate insulating layer, and a high polarization layer. By adding BT@BNNs-g-PVDF to the high polarization layer and adding PCBM and ALRB to the intermediate insulating layer, combined with biaxial stretching treatment, the interfacial adhesion and dielectric properties are improved.
It improves the breakdown strength, energy density and reliability of the film, reduces dielectric loss, enhances interlayer interface compatibility and interfacial diffusion behavior, and improves film quality and electrical stability.
Smart Images

Figure CN123104189A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of polymer composite capacitor film technology, and specifically discloses a three-layer biaxially stretched polymer dielectric composite film. Background Technology
[0002] As electronic power technology advances towards miniaturization, lightweighting, and integration, higher demands are being placed on the energy storage density and operational reliability of its core passive component—the capacitor. Polymer film capacitors are widely used due to their advantages such as high breakdown strength, self-healing, and high flexibility. In particular, high-dielectric-constant ferroelectric polymers, represented by polyvinylidene fluoride (PVDF), have shown great potential for high-energy-density device applications. To broaden their practical application areas, it is necessary to further improve their dielectric constant and breakdown strength while reducing dielectric loss.
[0003] Currently, to improve the dielectric properties of PVDF, two main approaches are taken: first, adding ceramic fillers with high dielectric constants to prepare nanocomposite materials to enhance the dielectric constant of PVDF; and second, using layered structures to design and compound linear dielectric polymers to improve the breakdown strength of PVDF and reduce its dielectric loss. For example, CN112185703A discloses a two-dimensional composite sandwich structure dielectric energy storage material, including an xBNNS / BP composite intermediate layer and xBNNS / yD-SNNS / BP composite upper and lower layers. It uses PVDF as the main organic matrix phase and PMMA as the modifying phase. By combining non-ferroelectric two-dimensional BNNS and ferroelectric two-dimensional SNNS and constructing a sandwich structure, it achieves both high dielectric breakdown strength and high energy storage density. Although the introduced BNNS improves the breakdown strength of the BP matrix and increases the energy storage density and charge / discharge efficiency, the modulus difference between different polymers can lead to interlayer separation and electrical failures under conditions such as bending deformation or electric field-induced mechanical stress. Furthermore, considering the biaxial stretching process used in industrial capacitor films, the mismatched moduli between layers hinder the coordinated deformation behavior during film formation, thus degrading the macroscopic film quality. In addition, filler agglomeration and interfacial electric field concentration lead to a decrease in overall breakdown strength, limiting the actual improvement in energy storage density. Therefore, it is urgent to develop a strategy to address the limited energy storage density and low reliability of PVDF dielectric composite films. Summary of the Invention
[0004] This invention provides a three-layer biaxially stretched polymer dielectric composite film and its preparation method. The composite film has high breakdown strength, high energy storage density, and high reliability.
[0005] This invention is achieved through the following technical solution: A three-layer biaxially oriented polymer dielectric composite film, wherein the composite film comprises a high polarization layer, an intermediate insulating layer and a high polarization layer in sequence; the raw materials of the high polarization layer include 100 parts PVDF, 0-10 parts PMMA and 10-20 parts BT@BNNs-g-PVDF by weight; the raw materials of the intermediate insulating layer include 100 parts PMMA, 0-10 parts PVDF, 1-5 parts PCBM and 1-5 parts ALRB by weight.
[0006] A method for preparing a three-layer biaxially stretched polymer dielectric composite film includes the following steps: S1 involves melting and mixing PVDF, PMMA, and BT@BNNs-g-PVDF to obtain a high polarization layer material; PMMA, PVDF, PCBM and ALRB are melt-mixed to obtain the intermediate insulation layer material; The high polarization layer raw material and the intermediate insulating layer raw material are respectively molded into high polarization layer film and intermediate insulating layer film; S2 After plasma treatment, PMMA is grafted onto the surface of the high polarization layer film. Then, the high polarization layer film and the intermediate insulating layer film are stacked and hot-pressed in an ABA manner to obtain a hot-pressed base film. S3 involves biaxially stretching the hot-pressed base film to obtain a three-layer biaxially stretched polymer dielectric composite film.
[0007] The technical solution of the present invention has at least the following advantages and beneficial effects: 1. This invention incorporates BT@BNNs-g-PVDF into a highly polarizable layer, using modified boron nitride nanosheets as the primary carrier. The hydroxyl groups of these nanosheets effectively load and disperse high-dielectric barium titanate nanosheets. After high-temperature treatment, the dispersed barium titanate nanosheets are immobilized within the boron nitride nanosheets. Secondly, PVDF polymer is grafted onto the surface of BT@BNNs using irradiation grafting, thereby enhancing the compatibility between the hybrid filler and the PVDF matrix, and further improving the overall dispersion of the dielectric filler in the polymer matrix. Simultaneously, the long-chain polymer on the surface of BT@BNNs can form chain entanglements with the polymer matrix, reducing the modulus mismatch at the filler-polymer interface, improving the interfacial bonding force, and reducing interfacial voids and defects during the biaxial stretching film formation process.
[0008] 2. This invention incorporates PCBM and ALRB into the intermediate insulating layer. PCBM traps high-energy electrons through deep-trap chemical confinement, while ALRB dissipates electron energy and suppresses electrical treeing through self-excitation. The synergistic effect of these two molecules suppresses carrier transport and improves insulation performance, thus addressing the reliability shortcomings of the intermediate layer relying solely on physical barrier mechanisms under long-term service conditions. Simultaneously, both organic molecules can achieve molecular-level dispersion within the polymer matrix, minimizing filler agglomeration and weak interfacial bonding, thereby avoiding defects such as localized electric field distortion and early breakdown.
[0009] 3. This invention, by adding a small amount of PMMA to the PVDF in the highly polarizable layer and a small amount of PVDF to the PMMA in the intermediate insulating layer, enhances the entropy-driven interfacial diffusion behavior during high-temperature annealing while maintaining the performance advantages of each component, thereby increasing the thickness of the interfacial phase in the ABA structure. The surface of the highly polarizable layer film is in-situ grafted with PMMA polymer through plasma modification, significantly improving its compatibility with the intermediate insulating layer and its van der Waals interactions. These multiple effects enhance the intralayer tensile stress transfer capacity and interlayer shear synergistic deformation capacity during the biaxial stretching process of the film.
[0010] 4. The high-ratio biaxial stretching process employed in this invention can enhance the polymer matrix modulus, while simultaneously inducing the arrangement of microcrystals and fillers along the stress direction, suppressing electrical tree development. The nano-barium titanate coated with wide-bandgap boron nitride significantly reduces interfacial electric field concentration, thereby improving the film's breakdown strength. Furthermore, the enhanced interlayer diffusion behavior reduces porosity and defects that may be induced during the stretching process, improving the stability of the film's breakdown strength. Additionally, boron nitride nanosheets can improve the material's thermal conductivity, thus reducing heat loss during charging and discharging. The introduction of a high-dielectric-constant filler into the high-polarization layer, combined with the PVDFβ-type high-polarization crystallization induced by biaxial stretching, enhances the film's polarization capability. Attached Figure Description
[0011] Figure 1 SEM images of the hot-pressed base film and composite film in Example 1 of the present invention.
[0012] Figure 2 The images show the stretched film of the composite films of Examples 1-2 and Comparative Example 1 provided by the present invention.
[0013] Figure 3 A schematic diagram of the dielectric constant of the composite thin film of Examples 1-2 and Comparative Example 1 provided by the present invention.
[0014] Figure 4 The dielectric loss diagrams of the composite films of Examples 1-2 and Comparative Example 1 provided by the present invention are shown.
[0015] Figure 5A schematic diagram of the breakdown strength of the composite films of Examples 1-2 and Comparative Example 1 provided by the present invention.
[0016] Figure 6 Electric field-electric displacement curves of the composite thin films of Examples 1-2 and Comparative Example 1 provided by the present invention. Detailed Implementation
[0017] The present invention will be further described below with reference to specific embodiments, but the embodiments do not limit the present invention in any way. Unless otherwise stated, the raw materials and reagents used in the embodiments of the present invention are conventionally purchased raw materials and reagents.
[0018] For layered polymer capacitor films, the modulus differences between different polymers can lead to interlayer separation and electrical faults under conditions such as bending deformation or electric field-induced mechanical stress. Furthermore, considering the biaxial stretching process used in industrial capacitor film fabrication, the mismatched modulus between layers hinders the coordinated deformation behavior during film formation, thus degrading the macroscopic film quality. Therefore, the applicant addresses the interlayer interface problem of three-layer capacitor films by controlling interfacial diffusion and capacitance enhancement to overcome the above-mentioned issues. The specific technical solution is as follows.
[0019] In a first aspect, the present invention provides a three-layer biaxially oriented polymer dielectric composite film, wherein the composite film comprises a high polarization layer, an intermediate insulating layer and a high polarization layer in sequence; the raw materials of the high polarization layer include 100 parts PVDF, 0-10 parts PMMA and 10-20 parts BT@BNNs-g-PVDF by weight; the raw materials of the intermediate insulating layer include 100 parts PMMA, 0-10 parts PVDF, 1-5 parts PCBM and 1-5 parts ALRB by weight.
[0020] By adding a small amount of PMMA to the PVDF in the highly polarizable layer and a small amount of PVDF to the PMMA in the intermediate insulating layer, the entropy-driven interfacial diffusion behavior during high-temperature annealing can be enhanced while maintaining the performance advantages of each component, thereby increasing the thickness of the interfacial phase in the ABA structure.
[0021] Barium titanate (BT) nanoparticles can improve the dielectric constant of PVDF, but they are prone to aggregation, leading to a decrease in the breakdown strength of the samples. By preparing a hybrid filler with boron nitride nanosheets (BNNs), BT is loaded onto the surface of the BNNs filler to improve its dispersibility. Furthermore, PVDF is grafted onto the BNNs surface to improve the compatibility of the hybrid filler in the matrix. Hierarchical interface design prevents filler aggregation and mitigates premature breakdown caused by interfacial electric field concentration. In addition, BNNs have a wide band gap, good insulation properties, and high electrical breakdown strength, which can compensate for the intrinsic low breakdown strength defect of BT.
[0022] [6,6]-Phenyl-C 61methyl butyrate (PCBM) traps high-energy electrons through deep-trap chemical confinement, while 4-propenoxy-2-hydroxybenzophenone (ALRB) captures high-energy electrons through high electron affinity and a narrow bandgap, dissipating energy through self-excitation. Selectively distributing PCBM and ALRB into the intermediate insulating layer allows them to synergistically enhance the insulation performance of the intermediate PMMA layer, addressing the reliability limitations of relying solely on physical barriers under long-term service conditions. Furthermore, it avoids the problem of PCBM and ALRB competing for space with BT@BNNs-g-PVDF filler in the same matrix, which could lead to filler aggregation and a decline in overall mechanical properties.
[0023] In this invention, the raw materials of the high polarization layer include 100 parts PVDF, 1-8 parts PMMA and 12-18 parts BT@BNNs-g-PVDF by weight; the raw materials of the intermediate insulating layer include 100 parts PMMA, 1-8 parts PVDF, 1-3 parts PCBM and 2-4 parts ALRB by weight.
[0024] In this invention, the weight-average molecular weight of PVDF is 280,000-320,000, and the density is 1.78 g / cm³. 3 PMMA has a weight-average molecular weight of 65,000-70,000 and a density of 1.19 g / cm³. 3 .
[0025] In this invention, the preparation method of BT@BNNs-g-PVDF includes the following steps: 1) Disperse BNNs powder in a mixed solvent of deionized water and ethanol to obtain a BNNs suspension; transfer the BNNs suspension to an aqueous sodium hydroxide solution for hydrothermal reaction to obtain a hydroxylated BNNs suspension; 2) BT powder was dispersed in a mixed solvent of deionized water and ethanol, then hydroxylated BNNs suspension was added and mixed, followed by calcination to obtain BT@BNNs; 3) BT@BNNs were mixed with PVDF solution and reacted by γ-ray irradiation to obtain BT@BNNs-g-PVDF.
[0026] BT@BNNs-g-PVDF uses modified boron nitride nanosheets as the primary carrier, utilizing their hydroxyl groups to achieve effective loading and dispersion of high-dielectric barium titanate nanosheets. After high-temperature treatment, the dispersed barium titanate nanosheets are immobilized within the boron nitride nanosheets. Next, PVDF polymer is grafted onto the surface of BT@BNNs using irradiation grafting, thereby enhancing the compatibility between the hybrid filler and the PVDF matrix, and further improving the overall dispersion of the dielectric filler in the polymer matrix. Simultaneously, the long-chain polymer on the surface of BT@BNNs can form chain entanglements with the polymer matrix, reducing the modulus mismatch at the filler-polymer interface, improving the interfacial bonding force, and reducing interfacial voids and defects during the biaxial stretching film formation process.
[0027] In this invention, during the hydrothermal reaction, the temperature is 100-120℃ and the time is 10-12h; and / or, during the calcination treatment, the temperature is 700-800℃ and the time is 2-5h; and / or, during the irradiation reaction, the irradiation is carried out under vacuum and room temperature conditions of a 5-45 kGy cobalt source for 16-20h.
[0028] In this invention, the total thickness of the composite film is 8-15 μm, and the thickness ratio of the high polarization layer to the intermediate insulating layer is 1:0.5-1.
[0029] Secondly, the present invention provides a method for preparing a three-layer biaxially stretched polymer dielectric composite film, comprising the following steps: S1 involves melting and mixing PVDF, PMMA, and BT@BNNs-g-PVDF to obtain a high polarization layer material; PMMA, PVDF, PCBM and ALRB are melt-mixed to obtain the intermediate insulation layer material; The high polarization layer raw material and the intermediate insulating layer raw material are respectively molded into high polarization layer film and intermediate insulating layer film; S2 After plasma treatment, PMMA is grafted onto the surface of the high polarization layer film. Then, the high polarization layer film and the intermediate insulating layer film are stacked and hot-pressed in an ABA manner to obtain a hot-pressed base film. S3 involves biaxially stretching the hot-pressed base film to obtain a three-layer biaxially stretched polymer dielectric composite film.
[0030] In the past, the reliability of interfacial bonding between different layers in multilayer composite thin film materials produced by simple hot pressing or co-extrusion was relatively low. This invention firstly introduces a small amount of PMMA inside the highly polarizable layer and a small amount of PVDF inside the intermediate insulating layer. This entropy-driven method enhances interfacial molecular diffusion during the hot pressing process between the AB layers, increasing the interfacial phase thickness while maintaining the matrix properties essentially unchanged. Secondly, grafting PMMA onto the surface of the highly polarizable layer enhances its van der Waals interaction with the intermediate insulating layer, strengthening the interfacial bonding strength. Furthermore, biaxial stretching is employed to significantly increase the interfacial area of the film while reducing its thickness, thereby increasing the interfacial area per unit volume. This stretching-induced interfacial reconstruction further enhances the reliability of the layer structure.
[0031] High-ratio biaxial stretching enhances the polymer matrix modulus and induces the alignment of microcrystals and fillers along the stress direction, suppressing electrical tree development. The nano-barium titanate coated with wide-bandgap boron nitride significantly reduces interfacial electric field concentration, thereby improving film breakdown strength. Furthermore, the enhanced interlayer diffusion behavior reduces porosity and defects that may be induced during stretching, improving the stability of film breakdown strength. Additionally, boron nitride nanosheets improve the material's thermal conductivity, reducing heat loss during charge and discharge. The introduction of high-dielectric-constant fillers into the high-polarization layer, combined with the PVDFβ-type high-polarization crystallization induced by biaxial stretching, significantly enhances the film's polarization capability.
[0032] In this invention, during step S1, the temperature for melting and mixing is 200-210℃ and the time is 5-10 min; during molding, the temperature is 190-220℃ and the pressure is 10-20 MPa.
[0033] In this invention, step S2, the step of grafting PMMA onto the surface of the highly polarizable film material after plasma treatment, includes: 1) The high polarization layer film material is subjected to surface plasma treatment under inert gas. The plasma power is 15-25W, the radio frequency power is 8-12MHz, the treatment time is 60-120s, and the treated film material is exposed to air for 8-10min to obtain the pretreated film material. 2) Immerse the pretreated membrane material in a 10% (v / v) aqueous solution of methacrylic acid, vacuum treat for 20-40 min, and then heat to 80℃ for 1-2 h to obtain a high polarization layer membrane material with PMMA grafted on the surface.
[0034] In this invention, during step S2, the stacking hot pressing is performed at a temperature of 150-160°C, a pressure of 5-8 MPa, and a time of 20-30 min, followed by static annealing at 180°C for 30-60 min.
[0035] In this invention, in step S3, the cavity temperature for biaxial stretching is 160-170℃, the stretching rate is 20-100mm / s, the stretching ratio is 4-4.5 times, and then it is annealed at 160℃ for 10-20min.
[0036] Example 1 A three-layer biaxially stretched polymer dielectric composite film is prepared by the following method: Preparation of BT@BNNs-g-PVDF packing material: 1) Place BNNs powder in a mixed solvent of deionized water and ethanol and sonicate for 7 h. The volume ratio of deionized water to ethanol is 70:30. After centrifugation, take the upper suspension to obtain BNNs suspension. Transfer the BNNs suspension to sodium hydroxide aqueous solution and keep it at 120℃ for 10 h in a hydrothermal reactor. After cooling, repeat the centrifugation and washing operation with deionized water to obtain hydroxylated BNNs suspension. 2) Place BT powder in a mixed solvent of deionized water and ethanol and ultrasonically disperse for 50 min. The volume ratio of deionized water to ethanol is 70:30. Then add hydroxylated BNNs suspension and continue ultrasonic mixing for 5 h. After filtration and washing, calcine at 780℃ for 4 h to obtain BT@BNNs. 3) Dissolve BT@BNNs and PVDF in N,N-dimethylformamide (DMF) solution, sonicate for 2 h, then heat in an oven to remove DMF solvent, and transfer the resulting mixture to a self-sealing bag for vacuum treatment; irradiate the above mixture at room temperature with a 25-45 kGy cobalt source for 18 h, and use DMF to dissolve and centrifuge the obtained sample to remove free PVDF. After multiple washings, place it in a vacuum oven for drying to obtain BT@BNNs-g-PVDF filler.
[0037] Preparation of composite thin films: S1 100 parts by weight of PVDF, 5 parts by weight of PMMA and 15 parts by weight of BT@BNNs-g-PVDF were premixed and then added to an internal mixer for melt blending. The internal mixing temperature was 210℃, the internal mixing time was 10min, and the rotor speed was 60rpm to obtain a high polarization layer raw material. S2 premixes 100 parts by weight of PMMA, 5 parts by weight of PVDF, 3 parts by weight of PCBM and 4 parts by weight of ALRB, then adds them to an internal mixer for melt blending and processes them under the same process conditions to obtain the intermediate insulation layer raw material. S3 The high polarization layer material and the intermediate insulating layer material are molded separately, and the molding temperature is controlled at 200℃, the pressure is 15MPa, and the thickness is 70μm to obtain the high polarization layer film and the intermediate insulating layer film. S4 The highly polarizable layer film was fixed on a glass plate and subjected to surface plasma treatment in an argon atmosphere. The plasma power was 20W, the radio frequency power was 10MHz, and the treatment time was 100s. After treatment, it was exposed to air for 10min to obtain the pretreated film. The pretreated film was then immersed in a 10% methacrylic acid aqueous solution and vacuum treated for 30min. Subsequently, the temperature was raised to 80℃ and reacted for 2h to obtain a highly polarizable layer film with PMMA grafted on the surface. S5 Then, the high polarization layer film material grafted with PMMA on the surface and the intermediate insulating layer film material are stacked and hot-pressed in the ABA manner. The hot-pressing temperature is 155℃, the pressure is 7MPa, and the hot-pressing time is 25min. Then, the pressure is removed and static annealing is performed at 180℃ for 40min to obtain the hot-pressed base film. S6 The hot-pressed base film is subjected to biaxial stretching treatment. The biaxial stretching cavity temperature is 165℃, the stretching rate is 50mm / s, and the biaxial stretching ratio is 4.5 times, resulting in a three-layer biaxially stretched polymer dielectric composite film with a total thickness of 12μm. Among them, the single-layer thickness of the high polarization layer is 4μm, and the thickness of the intermediate insulating layer is 4μm.
[0038] Example 2 A three-layer biaxially stretched polymer dielectric composite film is prepared by the following method: S1 100 parts by weight of PVDF, 8 parts by weight of PMMA and 12 parts by weight of BT@BNNs-g-PVDF were premixed and then added to an internal mixer for melt blending. The internal mixing temperature was 210℃, the internal mixing time was 10min, and the rotor speed was 60rpm to obtain a high polarization layer raw material. S2 premixes 100 parts by weight of PMMA, 8 parts by weight of PVDF, 3 parts by weight of PCBM and 2 parts by weight of ALRB, then adds them to an internal mixer for melt blending and processes them under the same process conditions to obtain the intermediate insulation layer raw material. S3 The high polarization layer material and the intermediate insulating layer material are molded separately, and the molding temperature is controlled at 200℃, the pressure is 15MPa, and the thickness is 100μm to obtain the high polarization layer film and the intermediate insulating layer film. S4 The highly polarizable layer film was fixed on a glass plate and subjected to surface plasma treatment in an argon atmosphere. The plasma power was 20W, the radio frequency power was 10MHz, and the treatment time was 100s. After treatment, it was exposed to air for 10min to obtain the pretreated film. The pretreated film was then immersed in a 10% methacrylic acid aqueous solution and vacuum treated for 30min. Subsequently, the temperature was raised to 80℃ and reacted for 2h to obtain a highly polarizable layer film with PMMA grafted on the surface. S5 Then, the high polarization layer film and the intermediate insulating layer film are stacked and hot-pressed in the ABA manner. The hot-pressing temperature is 155℃, the pressure is 7MPa, and the hot-pressing time is 25min. Then, the pressure is removed and static annealing is performed at 180℃ for 40min to obtain the hot-pressed base film. S6 The hot-pressed base film is subjected to biaxial stretching treatment. The biaxial stretching cavity temperature is 165℃, the stretching rate is 50mm / s, and the biaxial stretching ratio is 4.5 times, resulting in a three-layer biaxially stretched polymer dielectric composite film with a total thickness of 15μm. Among them, the single-layer thickness of the high polarization layer is 5μm, and the thickness of the intermediate insulating layer is 5μm.
[0039] Example 3 A three-layer biaxially oriented polymer dielectric composite film is disclosed, comprising a highly polarizable layer, an intermediate insulating layer, and a highly polarizable layer in sequence. The highly polarizable layer comprises, by weight, 100 parts PVDF, 10 parts PMMA, and 20 parts BT@BNNs-g-PVDF. The intermediate insulating layer comprises, by weight, 100 parts PMMA, 10 parts PVDF, 5 parts PCBM, and 5 parts ALRB. The preparation method is the same as in Example 1.
[0040] Example 4 A three-layer biaxially oriented polymer dielectric composite film is disclosed. The composite film comprises a highly polarized layer, an intermediate insulating layer, and a highly polarized layer in sequence. The raw materials of the highly polarized layer include 100 parts by weight of PVDF, 1 part by weight of PMMA, and 10 parts by weight of BT@BNNs-g-PVDF. The raw materials of the intermediate insulating layer include 100 parts by weight of PMMA, 1 part by weight of PVDF, 1 part by weight of PCBM, and 1 part by weight of ALRB. The preparation method is the same as in Example 1.
[0041] Comparative Example 1 The difference between this comparative example and Example 1 is that PMMA was not grafted onto the surface of the highly polarized layer.
[0042] Comparative Example 2 The difference between this comparative example and Example 1 is that the high polarization layer is PVDF and BT@BNNs-g-PVDF, and the intermediate insulating layer is PMMA, PCBM and ALRB.
[0043] Comparative Example 3 The difference between this comparative example and Example 1 is that the BT@BNNs filler was not grafted with PVDF.
[0044] Comparative Example 4 The difference between this comparative example and Example 1 is that no PCBM and ALRB were added to the intermediate insulating layer.
[0045] Comparative Example 5 The difference between this comparative example and Example 1 is that PCBM and ALRB are added to the high polarization layer, that is, the high polarization layer includes PVDF, PMMA, BT@BNNs-g-PVDF, PCBM and ALRB, and the intermediate insulating layer includes PMMA and PVDF.
[0046] Test case (1) The hot-pressed base film and the three-layer biaxially stretched polymer dielectric composite film prepared in Example 1 were observed by scanning electron microscopy (SEM), and the results are as follows: Figure 1 As shown, a is a composite film and b is a hot-pressed base film.
[0047] according to Figure 1 It can be seen that after biaxial stretching, the three-layer structure modified by the layer interface exhibits a relatively uniform texture in the composite film, without obvious interface pores or defects.
[0048] (2) Compare Examples 1-2 and Comparative Example 1, such as... Figure 2 The image shown is a photograph of the composite films prepared in Examples 1-2 and Comparative Example 1, after stretching.
[0049] according to Figure 2 It can be seen that the interlayer interface effect in Comparative Example 1 is weak, and the film surface is uneven with wrinkles after stretching. In Examples 1 and 2, the interlayer interface effect is strong, and the film surface is smooth. This indicates that introducing a small amount of PMMA into the highly polarizable layer and a small amount of PVDF into the intermediate insulating layer can enhance interfacial molecular diffusion between the AB layers based on entropy-driven processes. Grafting PMMA onto the surface of the highly polarizable layer film material can enhance interlayer van der Waals interactions, thereby improving film quality and interlayer reliability.
[0050] (3) The composite films of the examples and comparative examples were subjected to performance tests. The dielectric constant was measured using a broadband dielectric spectrometer (Concept50, Novocontrol GmbH), the dielectric breakdown strength was measured using an electrical insulation strength tester (DDJ-100KV, guance), and the energy density was measured using a ferroelectric testing system (Premier II, Radiant Technologies). The results are shown in Table 1.
[0051] Table 1 Performance test results of Examples 1-2 and Comparative Examples 1-5
[0052] As shown in Table 1, the composite film of the embodiment exhibits higher dielectric constant, breakdown strength, energy density, and discharge efficiency, while exhibiting lower dielectric loss. This indicates that the material performance can be improved by optimizing the composition and filler of the high polarization layer and intermediate insulating layer.
[0053] according to Figure 3It can be seen that the dielectric constant of the composite films of Examples 1-2 and Comparative Example 1 decreases with increasing frequency, and the dielectric constant of Comparative Example 1, which has poor interfacial interaction, decreases more at high frequencies.
[0054] according to Figure 4 It can be seen that the dielectric loss of the composite films of Examples 1-2 and Comparative Example 1 initially remains almost unchanged, but increases at high frequencies. Furthermore, Comparative Example 1, with its weaker interfacial interactions, exhibits weaker carrier confinement and higher dielectric loss. This indicates that at high frequencies, the dielectric constant of the examples decreases less, resulting in lower dielectric loss.
[0055] according to Figure 5 It can be seen that the breakdown strength of Example 1 is 847.5 kV / mm, the breakdown strength of Example 2 is 823.2 kV / mm, and the breakdown strength of Comparative Example 1 is 796.6 kV / mm. Examples 1 and 2 have good breakdown stability, while Comparative Example 1 has poor breakdown stability due to interface defects.
[0056] according to Figure 6 It can be seen that, compared with Comparative Example 1, Examples 1 and 2 have better energy density and discharge efficiency. This indicates that the examples have higher energy density and discharge efficiency.
[0057] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A three-layer biaxially oriented polymer dielectric composite film, characterized in that, The composite film comprises, in sequence, a high polarization layer, an intermediate insulating layer, and a high polarization layer; the raw materials of the high polarization layer include, by weight, 100 parts PVDF, 0-10 parts PMMA, and 10-20 parts BT@BNNs-g-PVDF; the raw materials of the intermediate insulating layer include, by weight, 100 parts PMMA, 0-10 parts PVDF, 1-5 parts PCBM, and 1-5 parts ALRB.
2. The three-layer biaxially oriented polymer dielectric composite film according to claim 1, characterized in that, The raw materials for the high polarization layer include 100 parts PVDF, 1-8 parts PMMA and 12-18 parts BT@BNNs-g-PVDF by weight; the raw materials for the intermediate insulation layer include 100 parts PMMA, 1-8 parts PVDF, 1-3 parts PCBM and 2-4 parts ALRB by weight.
3. The three-layer biaxially oriented polymer dielectric composite film according to claim 1, characterized in that, PVDF has a weight-average molecular weight of 280,000-320,000 and a density of 1.78 g / cm³. 3 PMMA has a weight-average molecular weight of 65,000-70,000 and a density of 1.19 g / cm³. 3 .
4. The three-layer biaxially oriented polymer dielectric composite film according to claim 1, characterized in that, The preparation method of BT@BNNs-g-PVDF includes the following steps: 1) Disperse BNNs powder in a mixed solvent of deionized water and ethanol to obtain a BNNs suspension; transfer the BNNs suspension to an aqueous sodium hydroxide solution for hydrothermal reaction to obtain a hydroxylated BNNs suspension; 2) BT powder was dispersed in a mixed solvent of deionized water and ethanol, then hydroxylated BNNs suspension was added and mixed, followed by calcination to obtain BT@BNNs; 3) BT@BNNs were mixed with PVDF solution and reacted by γ-ray irradiation to obtain BT@BNNs-g-PVDF.
5. The three-layer biaxially oriented polymer dielectric composite film according to claim 4, characterized in that, During hydrothermal reaction, the temperature is 100-120℃ and the time is 10-12h; and / or, during calcination treatment, the temperature is 700-800℃ and the time is 2-5h; and / or, during irradiation reaction, irradiation is carried out under vacuum at room temperature conditions with a 5-45 kGy cobalt source for 16-20h.
6. The three-layer biaxially oriented polymer dielectric composite film according to claim 1, characterized in that, The total thickness of the composite film is 8-15 μm, and the thickness ratio of the high polarization layer to the intermediate insulating layer is 1:0.5-1.
7. The method for preparing a three-layer biaxially oriented polymer dielectric composite film according to any one of claims 1-6, characterized in that, Includes the following steps: S1 involves melting and mixing PVDF, PMMA, and BT@BNNs-g-PVDF to obtain a high polarization layer material; PMMA, PVDF, PCBM and ALRB are melt-mixed to obtain the intermediate insulating layer material; the high polarization layer material and the intermediate insulating layer material are respectively molded into high polarization layer film and intermediate insulating layer film. S2 After plasma treatment, PMMA is grafted onto the surface of the high polarization layer film. Then, the high polarization layer film and the intermediate insulating layer film are stacked and hot-pressed in an ABA manner to obtain a hot-pressed base film. S3 involves biaxially stretching the hot-pressed base film to obtain a three-layer biaxially stretched polymer dielectric composite film.
8. The method for preparing a three-layer biaxially stretched polymer dielectric composite film according to claim 7, characterized in that, Step S2, the step of grafting PMMA onto the surface of the highly polarizable film material after plasma treatment, includes: 1) The high polarization layer film material is subjected to surface plasma treatment under inert gas. The plasma power is 15-25W, the radio frequency power is 8-12MHz, the treatment time is 60-120s, and the treated film material is exposed to air for 8-10min to obtain the pretreated film material. 2) Immerse the pretreated membrane material in a 10% (v / v) aqueous solution of methacrylic acid, vacuum treat for 20-40 min, and then heat to 80℃ for 1-2 h to obtain a high polarization layer membrane material with PMMA grafted on the surface.
9. The method for preparing a three-layer biaxially oriented polymer dielectric composite film according to claim 7, characterized in that, In step S1, the temperature during melt mixing is 200-210℃ and the time is 5-10 min; during compression molding, the temperature is 190-220℃ and the pressure is 10-20 MPa. And / or, in step S2, during hot pressing of the stack, the temperature is 150-160℃, the pressure is 5-8MPa, and the time is 20-30min, followed by static annealing at 180℃ for 30-60min; And / or, in step S3, the cavity temperature for biaxial stretching is 160-170℃, the stretching rate is 20-100mm / s, the stretching ratio is 4-4.5 times, and then it is annealed at 160℃ for 10-20min.
Citation Information
Patent Citations
High-breakdown and high-energy-storage-density two-dimensional composite sandwich structure polymer-based dielectric energy storage material and preparation method and application thereof
CN112185703A