Modified bitumen waterproof membrane and its preparation method, waterproof system

By using a needle-punched geotextile reinforcement layer and maleic anhydride graft modifier in modified bitumen waterproof membranes, a strong composite between the modified bitumen waterproof membrane and the waterproof coating is achieved, solving the problem of poor adhesion between the membrane and the coating and improving the overall performance of the waterproof system.

CN123104203APending Publication Date: 2026-11-17BEIJING ORIENTAL YUHONG WATERPROOF TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611350517.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-02
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The existing modified bitumen waterproof membranes, after the strength of the intermediate layer is improved, result in a decrease in the bitumen penetration effect, making them prone to water seepage and water migration. In addition, the adhesion between the membrane and the waterproof coating is poor, making it difficult to meet the Class I waterproofing requirements of important buildings.

Method used

Needle-punched geotextile is used as the lower surface reinforcement layer. Its three-dimensional porous structure allows the waterproof coating to penetrate and form a mechanical bond with the modified asphalt. Maleic anhydride is added to the modified asphalt as a grafting modifier, which chemically bonds with the surface of the needle-punched geotextile fibers, enhancing the interfacial bonding.

Benefits of technology

It improves the strong bonding ability of modified bitumen waterproof membrane and waterproof coating, enhances the overall thickness and deformation resistance of the waterproof system, avoids the failure of the waterproof layer caused by interface peeling, and meets the waterproof requirements of important buildings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This invention proposes a modified bitumen waterproof membrane, its preparation method, and a waterproof system, belonging to the field of building insulation or other protection technology. The modified bitumen waterproof membrane comprises, sequentially arranged, an upper surface isolation layer, an upper surface modified bitumen coating layer, an intermediate reinforcement layer, a lower surface modified bitumen coating layer, and a lower surface reinforcement layer. The lower surface reinforcement layer is made of needle-punched geotextile with an equivalent pore size ≥0.1mm. The coating material for both the upper and lower surface modified bitumen coating layers is modified bitumen containing a grafting modifier, wherein the grafting modifier is maleic anhydride.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of building insulation or other protection technology, specifically to a modified bitumen waterproof membrane and its preparation method and waterproof system. Background Technology

[0002] Polymer-modified bitumen waterproof membranes improve the high-temperature anti-flow properties and low-temperature anti-brittleness properties of bitumen by adding modifiers such as styrene-butadiene-styrene block copolymer (SBS), styrene-isoprene-styrene block copolymer (SIS), and styrene-butadiene rubber (SBR). This allows them to be used in building waterproofing projects in various climate regions. Furthermore, when the modified bitumen is coated onto a long-fiber polyester reinforcing layer, it exhibits high tensile strength and good dimensional stability, making it suitable for various applications such as roofs, underground structures, bridge decks, and tunnels.

[0003] However, the modified bitumen waterproof membrane in related technologies still faces the following problems in its optimization and development: On the one hand, the strength of the intermediate layer increases with the increase of the fiber content and thickness of the base material (currently, the most commonly used highest specification polyester base material is 310g / m). 2 If the thickness is further increased, it will affect the asphalt penetration effect of the base layer, leading to a decrease in the density of the intermediate layer. This will easily cause water seepage and water leakage problems during application, affecting the waterproof performance of the membrane. On the other hand, taking roof waterproofing as an example, for important building waterproofing projects, to achieve Class I waterproofing, two layers of waterproofing materials must be used. The relevant technical solutions mainly include: membrane-to-membrane composite schemes, but the full adhesion of the membrane to the substrate has strict conditions and is difficult to achieve; membrane-to-asphalt coating composite schemes, but the asphalt coating layer lacks deformation resistance, and the permanent isolation layer on the membrane surface will form an isolation with the coating, resulting in poor adhesion strength; coating-reinforcement layer-to-coating composite schemes have better deformation resistance, but the operation is cumbersome and the construction period is long. In addition, when membranes are composited with polyurethane coatings, the adhesion effect is poor due to the large differences in the molecular structure of the main materials, making it difficult to meet the quality requirements of composite construction.

[0004] Therefore, how to improve the adhesion between the waterproof membrane and the waterproof coating while enhancing the mechanical properties of the waterproof membrane, and achieve a strong composite between the two, is a technical problem that urgently needs to be solved in this field. Summary of the Invention

[0005] In view of this, to solve at least one technical problem in related technologies and other aspects, the present invention proposes a modified bitumen waterproof membrane, comprising, sequentially arranged, an upper surface isolation layer, an upper surface modified bitumen coating layer, an intermediate reinforcement layer, a lower surface modified bitumen coating layer, and a lower surface reinforcement layer. The lower surface reinforcement layer is made of needle-punched geotextile with an equivalent pore size ≥ 0.1 mm. The coating material for the upper and lower surface modified bitumen coating layers is modified bitumen containing a grafting modifier, wherein the grafting modifier is maleic anhydride.

[0006] According to embodiments of the present invention, the needle-punched geotextile is selected from any one of polyester, polypropylene, high-density polyethylene, and glass fiber, wherein the density of the high-density polyethylene is 0.94~0.95 g / cm³. 3 The needle-punched geotextile has a fiber diameter of 8D~14D, a tensile strength greater than 110N / 50mm, and a unit area mass of 70g / m². 2 ~120g / m 2 .

[0007] According to an embodiment of the present invention, the bonding surface between the needle-punched geotextile and the lower surface modified asphalt coating layer has a surface-activated adhesive structure, which is a silica-modified surface formed by atomic layer deposition or a calendered surface formed by roller pressing.

[0008] According to an embodiment of the present invention, the material of the upper surface isolation layer is selected from any one of low-melting-point film, sand, mineral particles, and geotextile, wherein the melting point of the low-melting-point film is 60~140℃; the material of the intermediate reinforcement layer is selected from at least one of long-fiber polyester base, glass fiber base, and glass fiber reinforced polyester base, and the matrix mass per unit area of ​​the intermediate reinforcement layer material is 100~310g / m². 2 Among them, the fiber length of the long-fiber polyester base is not less than 60mm.

[0009] According to an embodiment of the present invention, the intermediate reinforcement layer is located in the middle of the thickness of the modified bitumen waterproof membrane, and the thickness of the upper surface modified bitumen coating layer is the same as that of the lower surface modified bitumen coating layer.

[0010] According to embodiments of the present invention, the modified asphalt is a temperature-adaptive modified asphalt, which is either a room-temperature / high-temperature type modified asphalt or a low-temperature type modified asphalt. The room-temperature / high-temperature type modified asphalt is suitable for environments with temperatures ≥25°C and comprises the following components by weight: 46-56 parts petroleum asphalt, 10-15 parts softener, 9-14 parts thermoplastic elastomer, 0.5-1 part antioxidant, 1-3 parts lubricant, 2-4 parts petroleum resin, 3-5 parts hard asphalt, 3-5 parts high-temperature modifier, 2-5 parts graft modifier, 10-20 parts inorganic filler, and a crosslinking agent. 0.5~1 part; Low-temperature modified asphalt is suitable for environments with temperatures ≤-25℃, and includes the following components by weight: 46~56 parts petroleum asphalt, 10~15 parts softener, 9~14 parts thermoplastic elastomer, 0.5~1 part antioxidant, 1~3 parts lubricant, 2~4 parts petroleum resin, 5~10 parts low-temperature modifier, 2~5 parts graft modifier, 10~20 parts inorganic filler, and 0.5~1 part crosslinking agent. Specifically, the softener is selected from at least one of base oil, reduced-density polyethylene, reduced-density polyethylene, naphthenic oil, aromatic oil, and rubber oil; the antioxidant is a hindered phenolic antioxidant; the crosslinking agent is di-tert-butyl peroxide; the high-temperature modifier is selected from at least one of atactic polypropylene, isotactic polypropylene, amorphous α-olefin copolymer, and polyvinyl chloride; and the low-temperature modifier is selected from at least one of dioctyl dicarboxylate and dioctyl sebacate.

[0011] In another aspect of the present invention, a method for preparing the aforementioned modified bitumen waterproof membrane is also proposed, comprising: firstly providing an intermediate reinforcing layer, then coating modified bitumen containing maleic anhydride as a grafting modifier onto both sides of the intermediate reinforcing layer to form an upper surface modified bitumen coating layer and a lower surface modified bitumen coating layer respectively; then covering the surface of the upper surface modified bitumen coating layer with an isolation material to form an upper surface isolation layer; then performing atomic layer deposition treatment or roll pressing treatment on one side of the needle-punched geotextile to form a surface-activated adhesive structure, and covering the surface of the lower surface modified bitumen coating layer with the needle-punched geotextile having the surface-activated adhesive structure to form a lower surface isolation layer, thereby obtaining the modified bitumen waterproof membrane.

[0012] According to an embodiment of the present invention, the conditions for atomic layer deposition include: using oxygen as plasma, silicon dioxide as precursor, a deposition temperature of 80~100℃, and a film thickness of 1~10nm; the conditions for roll pressing include: a roll pressing temperature of 80~140℃, and the bonding surfaces of the needle-punched geotextile and the lower surface modified asphalt coating layer being in contact with a high-temperature roller to form a surface-activated adhesive structure, while the opposing surfaces of the needle-punched geotextile and the lower surface modified asphalt coating layer being in contact with a low-temperature roller.

[0013] According to an embodiment of the present invention, the coating temperature of the temperature-adaptive modified asphalt is 180~190℃; the covering temperature of the upper surface isolation layer is 90~140℃; and the covering temperature of the needle-punched geotextile is 70~140℃, reaching the instantaneous swelling temperature of the needle-punched geotextile.

[0014] In another aspect of the invention, a waterproofing system is also provided, comprising a waterproof coating and the aforementioned modified bitumen waterproof membrane. The waterproof coating is applied to one side of the lower surface reinforcement layer of the modified bitumen waterproof membrane, and the waterproof coating penetrates into the needle-punched geotextile. The waterproof coating is at least one of bitumen-based waterproof coating, polyurethane waterproof coating, or silane-modified polyether waterproof coating.

[0015] According to an embodiment of the present invention, the lower surface reinforcement layer uses a needle-punched geotextile with high permeability (equivalent pore size not less than 0.1 mm), allowing the waterproof coating to penetrate the three-dimensional pore structure of the needle-punched geotextile during construction. After curing, the coating forms a mechanical bond with the needle-punched geotextile fibers, thereby establishing a physical bonding effect between the coating and the modified bitumen waterproof membrane. Simultaneously, maleic anhydride added to the modified bitumen formulation acts as a grafting modifier. Under the process temperature conditions of covering the needle-punched geotextile, the anhydride groups on its molecular chain can undergo a grafting reaction with the polar groups on the surface of the needle-punched geotextile fibers, forming a chemical bond between the modified bitumen and the needle-punched geotextile, significantly enhancing the interfacial bonding strength between the needle-punched geotextile and the modified bitumen. Through the synergistic effect of physical riveting and chemical bonding, needle-punched geotextile firmly bonds the modified bitumen waterproof membrane body and the waterproof coating into a continuous composite structure. After the waterproof coating cures, it forms a reinforced composite layer on the underside of the modified bitumen waterproof membrane together with the needle-punched geotextile. This composite layer increases the overall thickness and deformation resistance of the waterproof system while preventing waterproof layer failure caused by interfacial delamination between different materials. Furthermore, the maleic anhydride graft modifier introduced into the modified bitumen improves the interfacial compatibility between the modified bitumen and polar materials, enabling the underside of the modified bitumen waterproof membrane to form a strong bond with various types of waterproof coatings. Detailed Implementation

[0016] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to specific embodiments.

[0017] The endpoints and any values ​​of the ranges disclosed in this invention are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of the various ranges, the endpoint values ​​of the various ranges and individual point values, and individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this invention.

[0018] The terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the invention. The terms “comprising,” “including,” etc., as used herein indicate the presence of the stated features, steps, operations, and / or components, but do not exclude the presence or addition of one or more other features, steps, operations, or components.

[0019] All terms used herein (including technical and scientific terms) have the meanings commonly understood by those skilled in the art, unless otherwise defined. It should be noted that the terms used herein are to be interpreted in a manner consistent with the context of this specification, and not in an idealized or overly rigid way.

[0020] Similarly, to simplify the invention and aid in understanding one or more of the various disclosed aspects, in the above description of exemplary embodiments of the invention, various features of the invention are sometimes grouped together into a single embodiment or description thereof. The use of terms such as "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., indicates that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the invention. In this specification, illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.

[0021] Furthermore, the technical solutions of the various embodiments can be combined with each other, but only if they are feasible for those skilled in the art. If the combination of technical solutions is contradictory or cannot be implemented, it should be considered that such combination of technical solutions does not exist and is not within the scope of protection claimed by this invention.

[0022] In the process of realizing this invention, it was found that the fundamental reason for the poor composite effect of waterproof membrane and coating in related technologies lies mainly in two aspects: First, although the permanent isolation layer (such as polyethylene film, sanding surface, etc.) on the lower surface of the membrane plays a role in preventing the membrane from self-adhesive, it also blocks the direct contact between the coating and the main body of the membrane, causing the coating to only adhere to the surface of the isolation layer and unable to form an effective bond; Second, even if the isolation layer is replaced with a non-woven fabric material with a certain degree of permeability, due to the large difference in interfacial polarity between modified bitumen and non-polar polymer materials, the combination of the two is still mainly physical interlocking, lacking chemical bonding, and is prone to interfacial peeling under stress.

[0023] Based on the above understanding, this invention proposes to set needle-punched geotextile as a reinforcing layer on the lower surface of modified bitumen waterproof membrane. Its three-dimensional porous structure provides a penetration channel for the coating, allowing the coating to penetrate the needle-punched geotextile and contact the lower surface of the modified bitumen waterproof membrane. Simultaneously, maleic anhydride is added as a grafting modifier to the modified bitumen formulation. The maleic anhydride groups react with the active groups on the surface of the needle-punched geotextile fibers, thereby establishing a chemical bond between the modified bitumen and the needle-punched geotextile, achieving a strong adhesion between the two.

[0024] This invention proposes a modified bitumen waterproof membrane, comprising, sequentially arranged, an upper surface isolation layer, an upper surface modified bitumen coating layer, an intermediate reinforcement layer, a lower surface modified bitumen coating layer, and a lower surface reinforcement layer. The lower surface reinforcement layer is made of needle-punched geotextile with an equivalent pore size ≥ 0.1 mm. The coating material for both the upper and lower surface modified bitumen coating layers is modified bitumen containing a grafting modifier, wherein the grafting modifier is maleic anhydride.

[0025] According to an embodiment of the present invention, the lower surface reinforcement layer uses a needle-punched geotextile with high permeability (equivalent pore size not less than 0.1 mm), allowing the waterproof coating to penetrate the three-dimensional pore structure of the needle-punched geotextile during construction. After curing, the coating forms a mechanical bond with the needle-punched geotextile fibers, thereby establishing a physical bonding effect between the coating and the modified bitumen waterproof membrane. Simultaneously, maleic anhydride added to the modified bitumen formulation acts as a grafting modifier. Under the process temperature conditions of covering the needle-punched geotextile, the anhydride groups on its molecular chain can undergo a grafting reaction with the polar groups on the surface of the needle-punched geotextile fibers, forming a chemical bond between the modified bitumen and the needle-punched geotextile, significantly enhancing the interfacial bonding strength between the needle-punched geotextile and the modified bitumen. Through the synergistic effect of physical riveting and chemical bonding, needle-punched geotextile firmly bonds the modified bitumen waterproof membrane body and the waterproof coating into a continuous composite structure. After the waterproof coating cures, it forms a reinforced composite layer on the underside of the modified bitumen waterproof membrane together with the needle-punched geotextile. This composite layer increases the overall thickness and deformation resistance of the waterproof system while preventing waterproof layer failure caused by interfacial delamination between different materials. Furthermore, the maleic anhydride graft modifier introduced into the modified bitumen improves the interfacial compatibility between the modified bitumen and polar materials, enabling the underside of the modified bitumen waterproof membrane to form a strong bond with various types of waterproof coatings.

[0026] In some specific embodiments, an overlap edge is provided on one side of the lower surface of the modified bitumen waterproof membrane, which is isolated by an isolation film. If the upper surface is a non-low melting point film surface, an overlap edge is provided on the upper surface on the other side of the overlap edge on the lower surface.

[0027] According to embodiments of the present invention, the needle-punched geotextile is selected from any one of polyester, polypropylene, high-density polyethylene, and glass fiber, wherein the density of the high-density polyethylene is 0.94~0.95 g / cm³. 3 The needle-punched geotextile has a fiber diameter of 8D~14D, a tensile strength greater than 110N / 50mm, and a unit area mass of 70g / m². 2 ~120g / m 2 .

[0028] According to embodiments of the present invention, polyester, polypropylene, high-density polyethylene, or glass fiber are selected as needle-punched geotextiles. This is beneficial in ensuring that the needle-punched geotextiles possess heat resistance and dimensional stability to adapt to the production and application environment of modified bitumen waterproof membranes. Specifically, the physical properties of the fibers are defined to ensure that the needle-punched geotextiles themselves possess high mechanical load-bearing capacity, thereby sharing part of the load when the modified bitumen waterproof membrane is subjected to external forces. Appropriate unit area mass ensures that the needle-punched geotextiles have sufficient fiber density to guarantee mechanical strength while retaining ample three-dimensional pore space for waterproof coating penetration.

[0029] In some specific embodiments, if the unit area mass of the needle-punched geotextile is less than 70 g / m² 2 The fiber layer of needle-punched geotextile is too sparse. Although it has good permeability, its mechanical properties are insufficient, and it cannot effectively reinforce the modified bitumen waterproof membrane. If the unit area mass is higher than 120g / m², 2 Excessive fiber packing leads to over-compression of the three-dimensional pores. While the equivalent pore size may still meet the requirement of not less than 0.1 mm, the connectivity and permeability of the pores decrease. This makes it difficult for the waterproof coating to fully penetrate the needle-punched geotextile and form effective contact with the underside of the modified bitumen waterproof membrane during construction. The physical bonding effect weakens, and the peel strength actually decreases. If the fibers in the needle-punched geotextile are too fine, the tensile strength will be insufficient; if they are too coarse, the interlacing points between the fibers will decrease, reducing the overall integrity and tear resistance of the needle-punched geotextile.

[0030] According to an embodiment of the present invention, the bonding surface between the needle-punched geotextile and the lower surface modified asphalt coating layer has a surface-activated adhesive structure, which is a silica-modified surface formed by atomic layer deposition or a calendered surface formed by roller pressing.

[0031] According to embodiments of the present invention, the bonding surface of the needle-punched geotextile has a surface-activated adhesive structure to improve the interfacial bonding between the needle-punched geotextile and the modified asphalt. Due to the significant polarity difference between the needle-punched geotextile fiber material (such as polypropylene, polyester, etc.) and the modified asphalt, the interfacial bonding is weak when they are directly compounded, and they are prone to peeling under external force. The surface-activated adhesive structure, by constructing a transitional interface layer on the bonding surface of the needle-punched geotextile, increases the chemical affinity and physical contact area at the interface, allowing the modified asphalt to more fully wet the surface of the needle-punched geotextile during the coating process.

[0032] In some specific embodiments, the silica-modified surface formed by atomic layer deposition can introduce a thin layer of highly polar silica on the surface of needle-punched geotextile fibers, thereby interacting with the polar groups in the modified bitumen and enhancing the interfacial adhesion. At the same time, because atomic layer deposition has atomic-level thickness control precision, the modified layer is thin and will not block the pores between the needle-punched geotextile fibers, thus ensuring the original permeability of the needle-punched geotextile.

[0033] In some specific embodiments, the calendered surface formed by roller pressing causes the fibers of the needle-punched geotextile bonding surface to undergo plastic deformation through the combined action of heat and pressure. The gaps between the fibers are partially compressed, and the surface tends to be flat, which significantly increases the actual contact area between the needle-punched geotextile and the modified asphalt. At the same time, the micro-coarsening structure of the fiber surface during the calendering process is beneficial to the mechanical anchoring of the modified asphalt.

[0034] According to an embodiment of the present invention, the material of the upper surface isolation layer is selected from any one of low-melting-point film, sand, mineral particles, and geotextile, wherein the melting point of the low-melting-point film is 60~140℃; the material of the intermediate reinforcement layer is selected from at least one of long-fiber polyester base, glass fiber base, and glass fiber reinforced polyester base, and the matrix mass per unit area of ​​the intermediate reinforcement layer material is 100~310g / m². 2 Among them, the fiber length of the long-fiber polyester base is not less than 60mm.

[0035] According to embodiments of the present invention, low-melting-point films, sand surfaces, mineral particles, or geotextiles are selected as surface isolation layers. These layers will not soften prematurely at high temperatures (above room temperature), leading to isolation failure, nor will they affect the isolation effect at normal storage temperatures. The intermediate reinforcement layer, serving as the skeleton of the modified bitumen waterproof membrane, needs to possess high tensile strength, good dimensional stability, and the ability to impregnate the bitumen coating. The long-fiber polyester base has a fiber length of not less than 60 mm and sufficient interweaving between fibers, providing high tensile strength and tear resistance. Fiberglass and fiberglass-reinforced polyester bases have excellent dimensional stability and heat resistance, suitable for scenarios with high requirements for the dimensional change rate of the modified bitumen waterproof membrane. Controlling the unit area mass of the base layer ensures sufficient mechanical properties while allowing the bitumen coating to completely penetrate the base layer during pre-impregnation and oiling processes, preventing the formation of seepage channels due to an excessively thick base layer that is not impregnated by bitumen.

[0036] In some specific embodiments, if the unit area mass of the intermediate reinforcement layer exceeds 310 g / m² 2 If the base layer thickness is too large, the asphalt coating material cannot completely penetrate the interior of the base layer during pre-impregnation and coating processes. This results in unfilled pores within the base layer, allowing moisture to seep into the modified bitumen waterproof membrane through these pores during use, causing water seepage and leakage problems. If the thickness is below 100g / m², further issues may occur. 2 If the fiber length of the long-fiber polyester base is less than 60mm, the degree of interweaving and entanglement between the fibers decreases, and the tensile strength and dimensional stability of the base will both decrease.

[0037] According to an embodiment of the present invention, the intermediate reinforcement layer is located in the middle of the thickness of the modified bitumen waterproof membrane, and the thickness of the upper surface modified bitumen coating layer is the same as that of the lower surface modified bitumen coating layer.

[0038] According to an embodiment of the present invention, the intermediate reinforcing layer is located at the midpoint of the thickness of the modified bitumen waterproof membrane. This allows the intermediate reinforcing layer to act as a neutral layer to withstand tensile stress when the modified bitumen waterproof membrane is subjected to tensile or bending forces. The upper and lower coating layers then evenly distribute the compressive and tensile stresses, resulting in a balanced overall stress state for the modified bitumen waterproof membrane. This avoids asymmetrical deformation of the modified bitumen waterproof membrane under stress due to the reinforcing layer being off-center. The identical thickness of the upper and lower coating layers further ensures the symmetry of the modified bitumen waterproof membrane, ensuring consistent deformation of the upper and lower surfaces during thermal expansion and contraction caused by temperature changes, thus reducing the risk of warping.

[0039] In some specific embodiments, if the intermediate reinforcement layer is off-center or the thickness of the upper and lower coating layers is different, the stress generated on the upper and lower surfaces of the modified bitumen waterproof membrane will be uneven when heated or subjected to force. The modified bitumen waterproof membrane is prone to warping and deformation, which affects the flatness of the laying and the sealing effect of the overlapping edges during construction. In severe cases, it may cause hollow areas between the modified bitumen waterproof membrane and the substrate, reducing the reliability of the waterproof system.

[0040] According to embodiments of the present invention, the modified asphalt is a temperature-adaptive modified asphalt, which is either a room-temperature / high-temperature type modified asphalt or a low-temperature type modified asphalt. The room-temperature / high-temperature type modified asphalt is suitable for environments with temperatures ≥25°C and comprises the following components by weight: 46-56 parts petroleum asphalt, 10-15 parts softener, 9-14 parts thermoplastic elastomer, 0.5-1 part antioxidant, 1-3 parts lubricant, 2-4 parts petroleum resin, 3-5 parts hard asphalt, 3-5 parts high-temperature modifier, 2-5 parts graft modifier, 10-20 parts inorganic filler, and a crosslinking agent. 0.5~1 part; Low-temperature modified asphalt is suitable for environments with temperatures ≤-25℃, and includes the following components by weight: 46~56 parts petroleum asphalt, 10~15 parts softener, 9~14 parts thermoplastic elastomer, 0.5~1 part antioxidant, 1~3 parts lubricant, 2~4 parts petroleum resin, 5~10 parts low-temperature modifier, 2~5 parts graft modifier, 10~20 parts inorganic filler, and 0.5~1 part crosslinking agent. Specifically, the softener is selected from at least one of base oil, reduced-density polyethylene, reduced-density polyethylene, naphthenic oil, aromatic oil, and rubber oil; the antioxidant is a hindered phenolic antioxidant; the crosslinking agent is di-tert-butyl peroxide; the high-temperature modifier is selected from at least one of atactic polypropylene, isotactic polypropylene, amorphous α-olefin copolymer, and polyvinyl chloride; and the low-temperature modifier is selected from at least one of dioctyl dicarboxylate and dioctyl sebacate.

[0041] In some specific embodiments, the petroleum asphalt is at least one of 70# petroleum asphalt, 90# petroleum asphalt, and 150# petroleum asphalt.

[0042] In some specific embodiments, the thermoplastic elastomer is at least one of linear styrene-butadiene-styrene block copolymer (SBS), styrene-isoprene-styrene block copolymer (SIS), and hydrogenated styrene-butadiene block copolymer (SEBS).

[0043] In some specific embodiments, the petroleum resin is at least one of C5 petroleum resin and C9 petroleum resin.

[0044] In some specific embodiments, the lubricant is at least one of polyethylene wax, polypropylene wax, and maleic anhydride-grafted polyethylene wax.

[0045] In some specific embodiments, the filler is at least one of heavy calcium carbonate, mineral powder, light calcium carbonate, and talc, with a mesh size of 100-200 mesh.

[0046] Hard asphalt is one or more of the following: residual oil asphalt, coal ash asphalt, No. 10 asphalt, etc.

[0047] According to embodiments of the present invention, the modified bitumen formulation of the waterproof membrane is differentiated for different ambient temperatures. The room temperature / high temperature formulation improves the softening point and heat resistance of the modified bitumen by adding hard bitumen and a high-temperature modifier, enabling it to maintain good dimensional stability and anti-flow properties in room temperature / high temperature (especially temperatures ≥35℃) scenarios, preventing slippage or deformation of the modified bitumen waterproof membrane due to bitumen softening in high-temperature environments. The low-temperature formulation improves the low-temperature anti-brittleness properties of the modified bitumen by adding a low-temperature modifier, enabling it to maintain good flexibility in ambient temperatures not exceeding -25℃, preventing brittleness of the modified bitumen waterproof membrane in low-temperature environments. Furthermore, both formulations contain maleic anhydride graft modifiers and di-tert-butyl peroxide crosslinking agents. The crosslinking agents can crosslink with the rubber-like modifiers in the modified bitumen, forming a three-dimensional network structure and improving the fatigue resistance of the modified bitumen.

[0048] In some specific embodiments, if the content of hard asphalt or high-temperature modifier in the room temperature / high temperature type formulation exceeds the range of 3 to 5 parts, if the content is too low, the improvement in heat resistance will not be significant, and if the content is too high, it will lead to excessive viscosity of the modified asphalt, affecting the uniformity of the coating process and the penetration effect on the base material; if the content of low temperature modifier in the low temperature type formulation exceeds the range of 5 to 10 parts, if the content is too low, the improvement in low temperature anti-brittleness performance will be insufficient, and if the content is too high, the heat resistance of the modified asphalt will be significantly reduced, and the modified asphalt waterproof membrane may flow at slightly higher temperatures.

[0049] In another aspect of the present invention, a method for preparing the aforementioned modified bitumen waterproof membrane is also proposed, comprising: firstly providing an intermediate reinforcing layer, then coating modified bitumen containing maleic anhydride as a grafting modifier onto both sides of the intermediate reinforcing layer to form an upper surface modified bitumen coating layer and a lower surface modified bitumen coating layer respectively; then covering the surface of the upper surface modified bitumen coating layer with an isolation material to form an upper surface isolation layer; then performing atomic layer deposition treatment or roll pressing treatment on one side of the needle-punched geotextile to form a surface-activated adhesive structure, and covering the surface of the lower surface modified bitumen coating layer with the needle-punched geotextile having the surface-activated adhesive structure to form a lower surface isolation layer, thereby obtaining the modified bitumen waterproof membrane.

[0050] According to an embodiment of the present invention, modified asphalt is first coated on both sides of the intermediate reinforcement layer to form upper and lower coating layers. The modified asphalt is allowed to fully impregnate and penetrate the intermediate reinforcement layer at the coating temperature. After the coating layers are formed, a release material is applied to the upper surface. Finally, a surface-activated needle-punched geotextile is applied to the lower modified asphalt coating layer. The needle-punched geotextile application step is performed last, allowing the geotextile to contact the still-warm modified asphalt coating layer at a higher temperature. At this temperature, the maleic anhydride graft modifier in the modified asphalt has high reactivity and can undergo a grafting reaction with the polar groups on the surface of the needle-punched geotextile fibers, achieving chemical bonding. Furthermore, the coating process is completed before the needle-punched geotextile application step, ensuring that the thickness and uniformity of the upper and lower coating layers are not affected by subsequent processes.

[0051] In some specific embodiments, if the covering temperature of the needle-punched geotextile is too low or the covering time is too early, the grafting reaction activity of maleic anhydride is insufficient, the chemical bonding effect is poor, and the adhesion between the needle-punched geotextile and the modified asphalt mainly relies on physical interlocking, resulting in low peel strength.

[0052] In some specific embodiments, providing an intermediate reinforcement layer includes sequentially unfolding, drying, pre-impregnating, and oiling the tire base.

[0053] According to an embodiment of the present invention, the conditions for atomic layer deposition include: using oxygen as plasma, silicon dioxide as precursor, a deposition temperature of 80~100℃, and a film thickness of 1~10nm; the conditions for roll pressing include: a roll pressing temperature of 80~140℃, and the bonding surfaces of the needle-punched geotextile and the lower surface modified asphalt coating layer being in contact with a high-temperature roller to form a surface-activated adhesive structure, while the opposing surfaces of the needle-punched geotextile and the lower surface modified asphalt coating layer being in contact with a low-temperature roller.

[0054] According to an embodiment of the present invention, atomic layer deposition (ALD) pretreatment of the bonding surface of needle-punched geotextile using oxygen plasma activates the fiber surface of the needle-punched geotextile and introduces active sites. Subsequently, a silica-modified layer with a thickness of 1-10 nm is formed using silica as a precursor at a deposition temperature of 80-100°C. This temperature range ensures sufficient chemical adsorption and reaction of the precursor on the surface of the needle-punched geotextile without causing thermal damage to thermoplastic fibers such as polypropylene. The film thickness of 1-10 nm is sufficient to change the polarity and chemical properties of the needle-punched geotextile surface without clogging the pores between the needle-punched geotextile fibers.

[0055] In this invention, the term "high temperature roller" refers to a heated roller used for calendering the bonding surface of geotextile, for example, the roller surface temperature can be 80~140°C; the term "low temperature roller" refers to a roller with a roller surface temperature lower than that of the high temperature roller, used for cooling and supporting the back surface of geotextile to prevent the geotextile from overheating and deforming as a whole.

[0056] In some specific embodiments, if the atomic layer deposition temperature is below 80°C, the chemical reaction rate of the precursor is insufficient to form a continuous and dense silica-modified layer; if it is above 100°C, the needle-punched geotextile fibers may experience thermal shrinkage or local melting, affecting the three-dimensional pore structure. If the silica film thickness is less than 1 nm, the modification effect is not obvious; if it is greater than 10 nm, it may fill the microscopic rough structure on the fiber surface, which is detrimental to the wetting of the modified asphalt.

[0057] According to an embodiment of the present invention, the roll pressing process is carried out at 80~140°C. The bonding surface of the needle-punched geotextile contacts the high-temperature roller to form a calendered surface to increase the contact area, while the backing surface contacts the low-temperature roller to prevent the needle-punched geotextile from being overheated and deformed.

[0058] In some specific embodiments, if the rolling temperature is below 80°C, the surface of the needle-punched geotextile cannot undergo effective plastic deformation, resulting in poor calendering effect; if it is above 140°C, the needle-punched geotextile fibers may excessively melt and adhere, affecting the pore structure.

[0059] According to an embodiment of the present invention, the coating temperature of the temperature-adaptive modified asphalt is 180~190℃; the covering temperature of the upper surface isolation layer is 90~140℃; and the covering temperature of the needle-punched geotextile is 70~140℃, reaching the instantaneous swelling temperature of the needle-punched geotextile.

[0060] According to embodiments of the present invention, the coating temperature of the temperature-adaptive modified asphalt is within this range. The modified asphalt has a low viscosity, which allows it to fully wet the intermediate reinforcement layer and penetrate into its interior, ensuring a tight bond between the coating layer and the base material. The application temperature of the upper surface isolation layer is within this temperature range, allowing it to adhere well to the surface of the coating layer without melting or deforming due to excessive temperature. Limiting the covering temperature of the needle-punched geotextile to reach its instantaneous swelling temperature activates the surface of the needle-punched geotextile fibers. This facilitates the grafting reaction between the maleic anhydride grafting modifier in the modified asphalt and the fibers, and also allows the modified asphalt to partially penetrate between the surface fibers of the needle-punched geotextile, forming a physical interlocking.

[0061] In some specific embodiments, if the coating temperature of the temperature-adaptive modified asphalt is below 180°C, the viscosity of the modified asphalt is too high, making it difficult to completely penetrate the base layer. Unwetted areas may exist between the base layer and the coating layer, affecting the compactness and waterproofing effect of the modified asphalt waterproof membrane. If the temperature is above 190°C, the thermoplastic elastomers and grafting modifiers in the modified asphalt may undergo thermal oxidative degradation, affecting their mechanical properties and grafting reactivity. If the covering temperature of the needle-punched geotextile is below 70°C, the movement of fiber molecular chain segments is restricted, resulting in poor instantaneous swelling and hindering the effective grafting reaction of maleic anhydride. If the temperature exceeds 140°C and the instantaneous swelling temperature is reached, prolonged heating may cause the needle-punched geotextile fibers to become structurally loose due to excessive swelling, leading to a decrease in strength. If the covering temperature of the needle-punched geotextile does not reach its instantaneous swelling temperature, the fiber surface is not sufficiently activated, resulting in insufficient grafting reaction and affecting the interfacial bonding strength.

[0062] In some more specific embodiments, the preparation method of room temperature / high temperature modified asphalt includes: stirring petroleum asphalt uniformly at a temperature of 130~140℃; adding thermoplastic elastomer to petroleum asphalt and stirring or grinding to homogenize for 1.5~2 hours at a temperature of 180~190℃; adding petroleum resin and antioxidant to the mixture and stirring uniformly for 15~20 minutes at a temperature of 180~190℃; adding hard asphalt and high temperature modifier to the mixture and stirring uniformly for 25~35 minutes at a temperature of 180~190℃; adding filler to the mixture and stirring uniformly for 25~35 minutes at a temperature of 180~190℃; adding grafting agent to the mixture and stirring uniformly for 25~35 minutes at a temperature of 180~190℃; adding crosslinking agent to the mixture and stirring uniformly before discharging.

[0063] In some more specific embodiments, the preparation method of low-temperature modified asphalt includes: stirring petroleum asphalt uniformly at a temperature of 130~140℃; adding thermoplastic elastomer to petroleum asphalt and stirring or grinding to homogenize for 1.5~2 hours at a temperature of 180~190℃; adding petroleum resin and antioxidant to the mixture and stirring uniformly for 15~20 minutes at a temperature of 180~190℃; adding low-temperature modifier to the mixture and stirring uniformly for 10~15 minutes at a temperature of 180~190℃; adding filler to the mixture and stirring uniformly for 25~35 minutes at a temperature of 180~190℃; adding crosslinking agent to the mixture and stirring uniformly before discharging.

[0064] In another aspect of the invention, a waterproofing system is also provided, comprising a waterproof coating and the aforementioned modified bitumen waterproof membrane. The waterproof coating is applied to one side of the lower surface reinforcement layer of the modified bitumen waterproof membrane, and the waterproof coating penetrates into the needle-punched geotextile. The waterproof coating is at least one of bitumen-based waterproof coating, polyurethane waterproof coating, or silane-modified polyether waterproof coating.

[0065] According to an embodiment of the present invention, in a waterproofing system, after curing, the waterproof coating forms an integrated reinforced composite layer with the needle-punched geotextile. The coating fills the three-dimensional pores of the needle-punched geotextile and forms a mechanical bond with the fibers of the geotextile. The needle-punched geotextile then firmly bonds to the lower surface of the modified bitumen waterproof membrane through grafting reaction and physical wetting, ultimately forming a continuous waterproof structure consisting of three layers: the modified bitumen waterproof membrane, the needle-punched geotextile, and the coating. In this structure, the needle-punched geotextile simultaneously serves multiple functions: reinforcing the modified bitumen waterproof membrane, connecting the coating, and transferring loads. This allows the originally independent modified bitumen waterproof membrane and coating waterproof layers to form a collaborative whole through the bridging effect of the needle-punched geotextile, avoiding interlayer separation failure caused by interface isolation or poor adhesion when traditional modified bitumen waterproof membranes and coatings are combined.

[0066] In some specific embodiments, the waterproof coating is limited to asphalt-based waterproof coating, polyurethane waterproof coating, or silane-modified polyether waterproof coating. Due to the penetration effect of needle-punched geotextile and the improvement of interfacial polarity by maleic anhydride graft modifier, the lower surface of the modified asphalt waterproof membrane has good adhesion to the above-mentioned types of waterproof coatings.

[0067] It should be noted that the described embodiments are merely some, not all, of the embodiments of the present invention. Other embodiments obtained by those skilled in the art based on the embodiments of the present invention without inventive effort are all within the scope of protection of the present invention.

[0068] Example 1

[0069] This embodiment 1 provides a modified bitumen waterproof membrane, the formulation components, content and process of which are shown in Table 1-1 below.

[0070] Table 1-1

[0071]

[0072] The modified bitumen waterproof membrane prepared in Example 1 was subjected to performance testing, and the results are recorded in Tables 1-2 below.

[0073] Table 1-2

[0074]

[0075] As can be seen from Table 1-2, the lower surface of the modified bitumen waterproof membrane in Example 1 is coated with an 80g / m² layer that has undergone atomic layer deposition and high-temperature roll pressing. 2 After the polypropylene needle-punched geotextile is coated, the bitumen-based waterproof coating can completely penetrate into the interior of the geotextile. Its peel strength to the substrate reaches 3.5 N / mm, with the peel section showing separation between the coating and the substrate, indicating that the interfacial bonding strength between the needle-punched geotextile and the roll material, and between the coating and the needle-punched geotextile, is higher than the bonding strength between the coating and the substrate. In terms of mechanical properties, the composite of the needle-punched geotextile improves the tensile strength and tear resistance of the composite roll material and coating, achieving a watertightness rating in terms of puncture resistance.

[0076] Example 2

[0077] This embodiment 2 provides a modified bitumen waterproof membrane, the formulation components, content and process parameters of which are shown in Table 2-1 below.

[0078] Table 2-1

[0079]

[0080] The modified bitumen waterproof membrane prepared in Example 2 was subjected to performance testing, and the results are recorded in Table 2-2 below.

[0081] Table 2-2

[0082]

[0083] As shown in Table 2-2, Example 2 uses a high-temperature modified asphalt formulation (with the addition of atactic polypropylene (APP) and residual oil asphalt). Compared with the ordinary formulation in Example 1, the heat resistance of the membrane increases from 105℃ to 130℃, making it suitable for waterproofing projects in hot regions. The lower surface is coated with an 80g / m² layer treated with atomic layer deposition and high-temperature roll pressing. 2 After the polypropylene needle-punched geotextile is coated, the bitumen-based waterproof coating can also completely penetrate into the interior of the needle-punched geotextile, achieving a peel strength of 3.5 N / mm, with the peel section showing separation between the coating and the base layer. In terms of mechanical properties, the tensile strength after composite coating is 1400 N / 50 mm, the tear strength is 600 N, and the puncture resistance reaches the impermeability level.

[0084] Example 3

[0085] This embodiment 3 provides a modified bitumen waterproof membrane, the formulation components, content and process parameters of which are shown in Table 3-1 below.

[0086] Table 3-1

[0087]

[0088] The modified bitumen waterproof membrane prepared in Example 3 was subjected to performance testing, and the results are recorded in Table 3-2 below.

[0089] Table 3-2

[0090]

[0091] As can be seen from Table 3-2, Example 3 uses a unit area mass of 130 g / m². 2 When polypropylene needle-punched geotextile is used as the lower surface reinforcement layer, although the needle-punched geotextile itself has higher mechanical properties, with a tensile strength of 1600 N / 50 mm and a tear strength of 700 N after composite, the high unit area mass and dense fiber packing of the needle-punched geotextile make it difficult for the bitumen-based waterproof coating to fully penetrate into the interior of the needle-punched geotextile. This causes the interface between the needle-punched geotextile and the roll material to fail first in the peel test, with a peel strength of only 1.0 N / mm. This indicates that there is an optimal upper limit to the unit area mass of the needle-punched geotextile; exceeding this range will affect the interfacial bonding effect due to insufficient penetration.

[0092] Example 4

[0093] This embodiment 4 provides a modified bitumen waterproof membrane, the formulation components, content and process parameters of which are shown in Table 4-1 below.

[0094] Table 4-1

[0095]

[0096] The modified bitumen waterproof membrane prepared in Example 4 was subjected to performance testing, and the results are recorded in Table 4-2 below.

[0097] Table 4-2

[0098]

[0099] As shown in Table 4-2, when Example 4 used a polypropylene needle-punched geotextile with a unit area mass of 60 g / m² as the lower surface reinforcement layer, the asphalt-based waterproof coating could completely penetrate to the surface of the roll material due to the low unit area mass and thin fiber layer of the needle-punched geotextile. The peel strength reached 3.6 N / mm, and the peel section was the separation between the coating and the base layer. However, due to the low fiber density of the needle-punched geotextile itself, the enhancement effect on the mechanical properties of the roll material was limited. The tensile strength after composite was 1250 N / 50 mm, and the tear strength was 500 N, which was a small improvement in mechanical properties compared with Example 2.

[0100] Example 5

[0101] This embodiment 5 provides a modified bitumen waterproof membrane, the formulation components, content and process parameters of which are shown in Table 5-1 below.

[0102] Table 5-1

[0103]

[0104] The modified bitumen waterproof membrane prepared in Example 5 was subjected to performance testing, and the results are recorded in Table 5-2 below.

[0105] Table 5-2

[0106]

[0107] As shown in Table 5-2, Example 5 uses a low-temperature modified asphalt formulation (with dioctyl sebacate (DOS) added as a low-temperature modifier), achieving a low-temperature flexibility limit of -50℃, making it suitable for waterproofing projects in extremely cold regions. Compared to the ordinary formulation of Example 1 (low-temperature flexibility limit -30℃), the low-temperature performance is significantly improved, while the heat resistance remains at 105℃. The lower surface is covered with 80g / m²... 2 After the polypropylene needle-punched geotextile is exposed, the asphalt-based waterproof coating can completely penetrate into the interior of the needle-punched geotextile, with a peel strength of 3.4 N / mm and a peel section where the coating peels off from the base layer.

[0108] Example 6

[0109] This embodiment 6 provides a modified bitumen waterproof membrane, the formulation components, content and process parameters of which are shown in Table 6-1 below.

[0110] Table 6-1

[0111]

[0112] The modified bitumen waterproof membrane prepared in Example 6 was subjected to performance testing, and the results are recorded in Table 6-2 below.

[0113] Table 6-2

[0114]

[0115] As shown in Table 6-2, Example 6 uses a composite of silane-modified polyether waterproof coating and modified bitumen waterproof membrane. Due to the high cohesive strength and good interfacial adhesion of the silane-modified polyether waterproof coating, and its ability to completely penetrate the needle-punched geotextile, the tensile strength of the composite membrane reaches 1500 N / 50 mm, and the tear strength reaches 800 N. This represents a significant improvement in mechanical properties compared to the bitumen-based waterproof coating system, with a peel strength of 4.5 N / mm. This indicates that the combination of needle-punched geotextile and maleic anhydride-grafted modified bitumen is also applicable to non-bitumen-based waterproof coating systems, effectively addressing the compatibility issues between different waterproof materials.

[0116] Comparative Example 1

[0117] Comparative Example 1 provides a modified bitumen waterproof membrane, the formulation components, content and process parameters of which are shown in Table 7-1 below.

[0118] Table 7-1

[0119]

[0120] The modified bitumen waterproof membrane prepared in Comparative Example 1 was subjected to performance tests, and the results are recorded in Table 7-2 below.

[0121] Table 7-2

[0122]

[0123] As shown in Table 7-2, in Comparative Example 1, a polyethylene film was used as the lower surface isolation layer. The asphalt-based waterproof coating could not penetrate into the interior of the roll material and only adhered to the surface of the polyethylene film. The adhesion strength between the two was low, with a peel strength of only 1.5 N / mm. The peel section showed separation between the coating and the polyethylene film. In this scheme, the polyethylene film lacked permeability and reinforcing properties. The tensile strength after composite was 1200 N / 50 mm, the tear strength was 400 N, and the puncture resistance test result was penetration.

[0124] Comparative Example 2

[0125] Comparative Example 2 provides a modified bitumen waterproof membrane, the formulation components, content and process parameters of which are shown in Table 8-1 below.

[0126] Table 8-1

[0127]

[0128] The performance of the modified bitumen waterproof membrane prepared in Comparative Example 2 was tested, and the results are recorded in Table 8-2 below.

[0129] Table 8-2

[0130]

[0131] As can be seen from Table 8-2, Comparative Example 2 uses 80 g / m³ material without atomic layer deposition and high-temperature rolling treatment. 2Polypropylene needle-punched geotextile was used as the lower surface reinforcement layer. Asphalt-based waterproof coatings could penetrate into the interior of the needle-punched geotextile, but the peeling section showed a separation between the modified asphalt membrane and the needle-punched geotextile, with a peel strength of only 1.0 N / mm. This indicates that although the three-dimensional porous structure of the needle-punched geotextile allows for coating penetration, the lack of chemical bonding and sufficient physical combination at the interface between the needle-punched geotextile and the modified asphalt results in insufficient adhesion strength, causing the needle-punched geotextile to detach from the membrane surface under external force. Compared to Comparative Example 1, the composite of needle-punched geotextile still improved mechanical properties, with tensile strength increasing from 1200 N / 50 mm to 1400 N / 50 mm, tear strength from 400 N to 600 N, and puncture resistance improving from penetration to impermeability; however, the interfacial adhesion problem remained unresolved.

[0132] Based on the test results of Examples 1-6 and Comparative Examples 1-2, the following conclusions can be drawn.

[0133] In Comparative Example 1, when a polyethylene film was used as the lower surface isolation layer, the waterproof coating could not penetrate into the interior of the roll material, only adhering to the surface of the polyethylene film. This resulted in low peel strength, limited improvement in the mechanical properties of the laminated roll material, and insufficient puncture resistance. Comparative Example 2, although replacing the polyethylene film with an 80g / m² waterproof coating… 2 Polypropylene needle-punched geotextile: The three-dimensional porous structure of needle-punched geotextile allows waterproof coatings to penetrate into its interior. However, due to the lack of chemical bonding between the needle-punched geotextile and modified bitumen and the absence of interface activation treatment, the bond strength between the needle-punched geotextile and the roll material is insufficient. The peel section is the separation between the needle-punched geotextile and the roll material, and the peel strength is even lower than that of the polyethylene film system.

[0134] Examples 1-6 all used maleic anhydride-grafted modified asphalt formulations, and the needle-punched geotextiles underwent atomic layer deposition and high-temperature roll pressing treatments. The unit area mass of the needle-punched geotextiles in Examples 1-2 and Examples 4-6 was 60-80 g / m². 2Within the specified range, the waterproof coating can completely penetrate into the needle-punched geotextile, and the interface between the needle-punched geotextile and the roll material is firmly bonded. The peel sections are all between the coating and the substrate, with a peel strength of 3.4~4.5 N / mm, representing an improvement of approximately 127%~200% compared to Comparative Example 1 and approximately 240%~350% compared to Comparative Example 2. Example 3 shows that when the unit area mass of the needle-punched geotextile increases to 130 g / m², the fiber packing becomes too dense, making it difficult for the coating to fully penetrate, resulting in decreased interfacial adhesion and a peel strength reduction to 1.0 N / mm. A comparison between Example 2 and Example 1 shows that the high-temperature modified bitumen formulation can increase the heat resistance from 105℃ to 130℃; Example 5 shows that the low-temperature modified bitumen formulation can reduce the low-temperature flexibility limit from -30℃ to -50℃; Example 6 shows that the technical solution of this invention is also applicable to non-bitumen-based waterproof coating systems such as silane-modified polyether.

[0135] In terms of mechanical properties, the method of using needle-punched geotextile as the lower surface reinforcement layer in this invention significantly improves the tensile strength and tear resistance after composite compared to the traditional polyethylene film method, and the puncture resistance is improved from penetration resistance to water impermeability. The needle-punched geotextile has a unit area mass of 80 g / m². 2 At the same time, it can ensure that the coating can fully penetrate and achieve good adhesion, and also provide effective mechanical reinforcement for the roll material. The tensile strength after composite reaches 1400~1500N / 50mm, and the tear strength reaches 600~800N, with excellent overall performance.

[0136] The specific embodiments described above further illustrate the purpose, technical solution, and beneficial effects of the present invention. It should be understood that the above descriptions are merely specific embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A modified bitumen waterproof membrane, characterized in that, It includes, in sequence, an upper surface isolation layer, an upper surface modified bitumen coating layer, an intermediate reinforcement layer, a lower surface modified bitumen coating layer, and a lower surface reinforcement layer; wherein, The material of the lower surface reinforcement layer is needle-punched geotextile, and the equivalent pore size of the needle-punched geotextile is ≥0.1mm; The coating material for the upper and lower surface modified asphalt coating layers is modified asphalt containing a grafting modifier, wherein the grafting modifier is maleic anhydride.

2. The modified bitumen waterproof membrane according to claim 1, characterized in that, The needle-punched geotextile is selected from any one of polyester, polypropylene, high-density polyethylene, and glass fiber, wherein the density of the high-density polyethylene is 0.94~0.95 g / cm³. 3 ; The needle-punched geotextile has fibers with a diameter of 8D to 14D, a tensile strength greater than 110N / 50mm, and a unit area mass of 70g / m². 2 ~120g / m 2 .

3. The modified bitumen waterproof membrane according to claim 2, characterized in that, The bonding surface between the needle-punched geotextile and the lower surface modified asphalt coating layer has a surface-activated adhesive structure, which is a silica-modified surface formed by atomic layer deposition or a calendered surface formed by roller pressing.

4. The modified bitumen waterproof membrane according to claim 1, characterized in that, The material of the upper surface isolation layer is selected from any one of low melting point film, sand, mineral particles, and geotextile, wherein the melting point of the low melting point film is 60~140℃; The intermediate reinforcement layer is made of at least one of long-fiber polyester matrix, glass fiber matrix, and glass fiber reinforced polyester matrix, and the matrix mass per unit area of ​​the intermediate reinforcement layer is 100~310 g / m². 2 The fiber length of the long-fiber polyester base is not less than 60 mm.

5. The modified bitumen waterproof membrane according to claim 1, characterized in that, The intermediate reinforcement layer is located in the middle of the thickness of the modified bitumen waterproof membrane, and the upper surface modified bitumen coating layer and the lower surface modified bitumen coating layer have the same thickness.

6. The modified bitumen waterproof membrane according to claim 1, characterized in that, The modified asphalt is a temperature-adaptive modified asphalt, which is either a normal temperature / high temperature type modified asphalt or a low temperature type modified asphalt. The aforementioned room temperature / high temperature modified asphalt is suitable for environments with temperatures ≥25℃, and comprises the following components by weight: 46-56 parts petroleum asphalt, 10-15 parts softener, 9-14 parts thermoplastic elastomer, 0.5-1 part antioxidant, 1-3 parts lubricant, 2-4 parts petroleum resin, 3-5 parts hard asphalt, 3-5 parts high temperature modifier, 2-5 parts graft modifier, 10-20 parts inorganic filler, and 0.5-1 part crosslinking agent; The low-temperature modified asphalt is suitable for environments with temperatures ≤-25℃, and comprises the following components by weight: 46-56 parts petroleum asphalt, 10-15 parts softener, 9-14 parts thermoplastic elastomer, 0.5-1 part antioxidant, 1-3 parts lubricant, 2-4 parts petroleum resin, 5-10 parts low-temperature modifier, 2-5 parts graft modifier, 10-20 parts inorganic filler, and 0.5-1 part crosslinking agent; wherein, The softener is selected from at least one of base oil, reduced-strength ester, reduced-strength ester, naphthenic oil, aromatic oil, and rubber oil; the antioxidant is a hindered phenolic antioxidant; the crosslinking agent is di-tert-butyl peroxide; the high-temperature modifier is selected from at least one of atactic polypropylene, isotactic polypropylene, amorphous α-olefin copolymer, and polyvinyl chloride; and the low-temperature modifier is selected from at least one of dioctyl dicarboxylate and dioctyl sebacate.

7. A method for preparing a modified bitumen waterproof membrane as described in any one of claims 1 to 6, characterized in that, include: Provide intermediate reinforcement layers; Modified asphalt containing maleic anhydride as a grafting modifier is coated on both sides of the intermediate reinforcement layer to form an upper surface modified asphalt coating layer and a lower surface modified asphalt coating layer, respectively. An isolation material is applied to the surface of the modified asphalt coating layer on the upper surface to form an upper surface isolation layer; Atomic layer deposition or roll forming is performed on one side of the needle-punched geotextile to form a surface-activated adhesive structure. The needle-punched geotextile with the surface-activated adhesive structure is then covered onto the surface of the lower modified bitumen coating layer to form a lower surface isolation layer, thereby obtaining a modified bitumen waterproof membrane.

8. The preparation method according to claim 7, characterized in that, The conditions for the atomic layer deposition process include: using oxygen as plasma, silicon dioxide as precursor, deposition temperature of 80~100℃, and film thickness of 1~10nm. The conditions for the roll pressing process include: the roll pressing temperature is 80~140℃, and the bonding surfaces of the needle-punched geotextile and the lower surface modified asphalt coating layer are in contact with the high-temperature roller to form the surface activated adhesive structure, while the opposing surfaces of the needle-punched geotextile and the lower surface modified asphalt coating layer are in contact with the low-temperature roller.

9. The preparation method according to claim 7, characterized in that, The coating temperature of the modified asphalt is 180~190℃; The temperature at which the upper surface isolation layer is applied is 90~140℃; The covering temperature of the needle-punched geotextile is 70~140℃, and it reaches the instantaneous swelling temperature of the needle-punched geotextile.

10. A waterproofing system, characterized in that, Includes waterproof coatings and modified bitumen waterproof membranes as described in any one of claims 1 to 6; The waterproof coating is applied to one side of the lower surface reinforcement layer of the modified bitumen waterproof membrane, and the waterproof coating penetrates into the needle-punched geotextile of the modified bitumen waterproof membrane; the waterproof coating is at least one of bitumen-based waterproof coating, polyurethane waterproof coating, and silane-modified polyether waterproof coating.