A gradient-structured carbon fiber preform, its preparation method and application

By combining a gradient structure carbon fiber preform preparation method with needle punching and stitching processes, the problem of carbon fiber preforms being unable to simultaneously achieve ablation protection and mechanical properties was solved. This method realizes the gradient change of material properties and the improvement of strength, simplifies the production process, and produces high-performance ceramic-modified carbon fiber reinforced composite materials.

CN123104208APending Publication Date: 2026-11-17CENT SOUTH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611442984.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-17
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing carbon fiber preforms cannot simultaneously meet the dual requirements of excellent ablation protection performance and high mechanical load-bearing performance.

Method used

A gradient structure carbon fiber preform preparation method is adopted, which combines needle punching and stitching processes to control the density gradient of the material from top to bottom and the relative content of carbon fiber and pores. Combined with the tight bonding between different layers, a gradient change is formed.

Benefits of technology

This method achieves a balance between the ablation protection performance and high-temperature mechanical properties of the material, improves the interlayer bonding strength, simplifies the production process, shortens the process cycle, and produces a lightweight and high-performance ceramic-modified carbon fiber reinforced composite material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123104208A_ABST
    Figure CN123104208A_ABST
Patent Text Reader

Abstract

This invention discloses a gradient-structured carbon fiber preform, its preparation method, and its application, belonging to the field of carbon fiber preform preparation technology. The method includes the following steps: S1 using continuous fibers as stitching thread to perform Z-direction stitching on multi-layered stacked carbon fiber woven fabric to obtain a laminated stitched carbon fiber preform; S2 combining the laminated stitched carbon fiber preform with a 2.5D needle-punched carbon fiber preform, such that the laminated stitched carbon fiber preform is located below the 2.5D needle-punched carbon fiber preform; the 2.5D needle-punched carbon fiber preform is formed by alternating layers of non-woven fabric and a mesh layer connected by needle punching, and the thickness of the mesh layer gradually increases from bottom to top. This preform preparation method combines needle punching and stitching processes, resulting in a preform material with tight bonding between different layers, which can be applied to the preparation of ceramic-modified carbon fiber reinforced composite materials with both excellent ablation protection and high-temperature mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of carbon fiber preform preparation technology, specifically a gradient structure carbon fiber preform, its preparation method and application. Background Technology

[0002] Carbon fiber reinforced carbon matrix composites (C / C composites) are all-carbon composite materials with carbon fibers or their fabrics as reinforcement and carbon (resin carbon, pyrolytic carbon, or pitch carbon) as the matrix. C / C composites have advantages such as low density, high specific strength and specific modulus, small coefficient of thermal expansion, and good chemical stability. In particular, they have the characteristic that their strength increases with increasing temperature, and are widely used in the aerospace field, such as aircraft brake discs and rocket engine nozzle throat liners.

[0003] The properties of C / C composites are closely related to the fiber structure of the carbon fiber preform used. Currently, there are two main types of carbon fiber preform structures that are widely used: 2.5D needle-punched carbon fiber preforms and laminated and stitched carbon fiber preforms.

[0004] C / C composites made from 2.5D needle-punched carbon fiber preforms are primarily used as preforms for carbon fiber reinforced ceramic matrix modified composites for ablation protection. They mainly consist of a mesh layer composed of chopped fibers, a non-woven fabric layer (such as alternating 0° and 90° layups), and Z-direction fiber bundles introduced by needles during the needle-punching process. The Z-direction fiber bundles are formed by the transfer of chopped fibers from the mesh layer during needle-punching, increasing the fiber content in the thickness direction (Z-direction) of the carbon fiber preform, which helps improve the interlaminar shear strength of the material and simultaneously forms pore channels for fluid flow in the thickness direction. The fibers inside the mesh layer are randomly arranged, resulting in high porosity. During densification and ceramic phase introduction, fluid mainly diffuses through this region within the mesh layer, and the ceramic phase content in the mesh layer region is relatively higher after ceramic modification. The non-woven fabric layer, composed of continuous carbon fibers, is mainly used to enhance the in-plane (XY direction) mechanical properties of the composite material. However, the needle punching process can damage the continuous fibers in the non-woven fabric, and the mechanical properties of the mesh layer itself are limited. Therefore, the mechanical properties of composite materials prepared from this type of preform are usually limited.

[0005] Lamination and stitching of carbon fiber preforms mainly involves stacking carbon fabrics (such as satin weave, plain weave, and spread weave) in a certain direction and sequence, and then stitching them together with continuous fibers along the thickness direction (Z-direction). This type of preform has a high fiber volume fraction (up to 40%~50%), resulting in a denser structure and superior mechanical properties in the prepared C / C composites. However, due to the high carbon fiber volume fraction, the preform contains a large amount of continuous matrix carbon in the thickness direction after densification. This makes it easy for the continuous matrix carbon to oxidize and be lost during service in ablation environments, forming channels for high-temperature gases to diffuse inwards. Therefore, the ablation protection performance of this type of composite material is usually limited.

[0006] However, in practical applications, while requiring materials to possess excellent ablation resistance, sufficient mechanical load-bearing capacity is also necessary. This presents a dual requirement for materials to achieve both ablation resistance and load-bearing capacity. However, due to the limitations of the carbon fiber preform structure, the dual requirements of ablation protection and mechanical load-bearing capacity are often difficult to meet simultaneously with a single-structure carbon fiber preform. Therefore, starting with the structural design of the carbon fiber preform, developing a gradient-type, designable carbon fiber preform is expected to lay a solid material design foundation for the subsequent preparation of multifunctional gradient carbon fiber reinforced composite materials that combine excellent ablation resistance and high mechanical load-bearing capacity. Summary of the Invention

[0007] In view of the problems that existing carbon fiber preforms cannot simultaneously achieve mechanical properties and ablation protection properties, the first objective of this invention is to provide a gradient structure carbon fiber preform in which different layers of the material are tightly bonded, and can be applied to the preparation of ceramic modified carbon fiber reinforced composite materials with both excellent ablation protection properties and high-temperature mechanical properties.

[0008] The second objective of this invention is to provide a method for preparing a gradient-structured carbon fiber preform. This method combines needle punching and stitching processes to effectively control the density gradient of the overall material from top to bottom, as well as the relative content of carbon fibers and pores, in order to achieve the goal of gradient change in performance.

[0009] The third objective of this invention is to provide an application of a gradient structure carbon fiber preform. Using this preform as a raw material to prepare gradient structure ceramic modified carbon fiber reinforced composite materials not only simplifies the process and allows for one-time molding, thus improving production efficiency, but also results in a composite material that is lighter and has a lower density than existing composite materials, while simultaneously meeting the dual requirements of mechanical properties and ablation protection properties of ceramic modified carbon fiber reinforced composite materials.

[0010] To achieve the above technical objectives, the present invention provides a method for preparing a gradient-structured carbon fiber preform, the method comprising:

[0011] S1 uses continuous fibers as stitching thread to stitch multiple layers of stacked carbon fiber woven fabric in the Z direction to obtain a laminated and stitched carbon fiber preform.

[0012] S2 combines the laminated and stitched carbon fiber preform with the 2.5D needle-punched carbon fiber preform, such that the laminated and stitched carbon fiber preform is located below the 2.5D needle-punched carbon fiber preform; the 2.5D needle-punched carbon fiber preform is formed by alternating layers of non-woven fabric and mesh layer and then needle-punching them together.

[0013] The composite method is as follows: the laminated and stitched carbon fiber preform and the 2.5D needle-punched carbon fiber preform are prepared separately in advance and then laminated; or the non-woven fabric and the mesh layer are alternately laid on one side of the laminated and stitched carbon fiber preform and needle-punched and connected; then, continuous carbon fiber is used to stitch the composite whole in the Z direction.

[0014] The gradient carbon fiber preform preparation method of this invention combines needle punching and Z-axis stitching processes. This method not only tightly binds different layers through the dual mechanisms of needle punching and stitching, avoiding the risk of interlayer delamination, but also places the laminated and stitched carbon fiber preform in the lower layer. This facilitates the overall forming process of the material and, in application, the lower layer, located on the inside, serves as the main mechanical load-bearing component. The upper 2.5D needle-punched structure, located on the outside, acts as an ablation protection layer, achieving a unity of structure and function. Furthermore, this invention achieves ceramic modification only in the outer needle-punched layer, while the inner laminated and stitched layer remains in a pure C / C state, significantly reducing the overall density. The ceramic phase infiltrates the needle-punched fiber network rather than being a pure coating, and the carbon fiber toughening improves thermal shock resistance. Since both the inner and outer layers are carbon fiber reinforcements, the gradient transition and fiber synergy effectively mitigate the difference in thermal expansion coefficients, avoiding the delamination failure caused by the brittleness and interface mismatch of traditional coatings. Moreover, the integrated preform of this invention only requires one co-densification and partitioned modification step for one-step forming, significantly shortening the process cycle.

[0015] A further preferred method of composite assembly is to directly lay layers of non-woven fabric and mesh layer alternately on one side of the stacked carbon fiber preform and then needle-punch them together; then, continuous carbon fiber is used to suture the composite assembly in the Z direction.

[0016] As a preferred embodiment, the thickness of the mesh layer gradually increases from bottom to top. This invention further sets the thickness of the mesh layer into a gradient structure, utilizing the fact that the gradient increase in mesh layer thickness does not change the density of the mesh layer unit structure itself, but makes the preform exhibit a characteristic of decreasing density and increasing porosity from bottom to top, thus achieving gradient control of carbon fiber and pore content. The lower layer of laminated preform provides a high-strength continuous fiber skeleton, achieving the goal of excellent mechanical load-bearing capacity. The upper 2.5D needle-punched structure preform and the pore structure gradient caused by the gradual increase in mesh layer thickness from bottom to top impart a gradient change in material from dense to porous, thereby forming a continuous change in performance in the thickness direction. Moreover, this gradient structure can effectively control the content distribution of ceramic phase—the thicker outer mesh layer can accommodate more ceramic phase to provide excellent ablation protection, while the thinner inner mesh layer has less ceramic phase, which can match the thermal expansion coefficient of the laminated structure, thereby significantly alleviating interfacial thermal stress concentration and improving interlayer bonding strength. Therefore, it can further significantly improve the ablation protection capability and high-temperature mechanical properties of the material, and realize the integration of ablation and load bearing.

[0017] As a preferred embodiment, the multi-layered stacked carbon fiber woven fabric is a carbon fiber fabric using different weaving methods.

[0018] As a preferred embodiment, the carbon fiber cloth is at least one of satin fabric, spread fabric, and plain weave fabric, and the corresponding carbon fiber cloth is laid in the required position according to the specific needs.

[0019] As a preferred embodiment, the thickness of the laminated and stitched carbon fiber preform is 3~30mm.

[0020] As a preferred embodiment, in S1, the continuous fiber is a 1k or 3k carbon fiber bundle.

[0021] As a preferred embodiment, in S1, the suture density of the Z-direction suture is between 3mm×3mm and 15mm×15mm.

[0022] As a preferred embodiment, in S2, the needle density of each layer in the 2.5D needled structure ranges from 15 to 30 needles / cm along the direction from contact with the laminated and stitched carbon fiber preform to the direction away from it. 2 Decrease to 8 or more stitches per cm and less than 15 stitches per cm 2This invention further utilizes a gradient change in needled density to effectively form Z-direction fibers and Z-direction interconnecting channels in both needled and laminated stitched structures. Through a unidirectional reactive melting and infiltration method, after modifying the 2.5D needled structure preform with ultra-high temperature ceramics, a portion of the molten metal can infiltrate into the laminated stitched structure through the Z-direction interconnecting channels formed by needled insertion. This portion of the ceramic phase can also produce pinning and mechanical bonding effects, thereby improving the interfacial bonding strength of the composite material with its two different structures: the needled structure and the laminated stitched structure.

[0023] A further preferred configuration is 15-25 stitches / cm. 2 Decrease to 8-12 stitches / cm 2 .

[0024] As a preferred embodiment, the thickness of the mesh layer gradually increases from 0.2-0.6 mm at the bottom to 0.8-2 mm at the top. The thickness of the mesh layer and the needle-punching density in this invention exhibit opposite trends, which synergistically results in more Z-axis fibers within the preform, leading to a relatively higher interlayer bonding strength. After melt infiltration, a thicker mesh layer results in a higher ceramic phase content in the composite material, and vice versa. The ceramic phase content significantly affects ablation protection performance and the coefficient of thermal expansion. This invention uses a thicker mesh layer in the outer layer to accommodate more ceramic phase and achieve superior ablation protection performance, while using a thinner mesh layer in the inner layer to reduce the ceramic phase content. This aims to reduce the coefficient of thermal expansion of this portion of the material, alleviate shear stress concentration at the interface, and improve the interlayer bonding strength of the two composite materials with different structures.

[0025] As a preferred embodiment, the density of the laminated and stitched carbon fiber preform is 0.7~1 g / cm³. 3 In this invention, the laminated and stitched carbon fiber preform has a high density, resulting in a high proportion of carbon fiber content after densification, thereby achieving excellent mechanical properties.

[0026] As a preferred embodiment, the density per unit thickness of the 2.5D needle-punched structure ranges from 0.5 to 0.8 g / cm³ from bottom to top. 3 Reduced to 0.3~0.5 g / cm³ 3 .

[0027] As a preferred embodiment, the total thickness of the 2.5D needle-punched carbon fiber preform is 3~30mm.

[0028] As a preferred embodiment, the adjacent non-woven fabrics in the 2.5D needle-punched carbon fiber preform are placed at an angle of 0 to 90°.

[0029] As a preferred embodiment, the needle insertion depth can be set to a constant or variable depth between 2 mm and 15 mm as required.

[0030] As a preferred embodiment, in S2, the continuous fiber is a 1k or 3k carbon fiber bundle.

[0031] As a preferred embodiment, the Z-direction suture lines in S1 and S2 coincide, or the suture position of S2 is located at the exact center of the suture line in the laminated carbon fiber preform. This invention reduces damage to the carbon fibers in the laminated preform by aligning the suture lines, while aligning them at the exact center of the suture line improves the interlaminar bonding strength of the composite material. More preferably, the Z-direction suture lines in S1 and S2 coincide.

[0032] As a preferred embodiment, after laying a non-woven fabric layer and chopped fibers on the top of the laminated and stitched preform, it is impregnated with low-flow resin and then needle-punched, or a resin-coated non-woven fabric layer is laid on the surface of the laminated and stitched carbon fiber preform, and then a layer of chopped fibers is laid and needle-punched.

[0033] This invention also provides a gradient-structured carbon fiber preform obtained by the above-described preparation method. This material exhibits tight bonding between different layers and possesses excellent ablation protection and high-temperature mechanical properties.

[0034] Finally, this invention also provides an application of gradient structure carbon fiber preforms, which are used as raw materials in gradient structure ceramic modified carbon fiber reinforced composites. This not only simplifies the process and improves production efficiency, but also makes the preforms lighter and lower in density than existing ceramic modified carbon fiber reinforced composites, while simultaneously possessing excellent high-temperature mechanical properties and ablation protection properties.

[0035] Compared with the prior art, the present invention has at least the following beneficial effects:

[0036] (1) The gradient structure carbon fiber preform provided by the present invention has a tight bond between different layers and can be used to prepare ceramic modified carbon fiber reinforced composite materials with excellent ablation protection performance and high temperature mechanical properties.

[0037] (2) The present invention combines needle punching and suturing processes to ensure tight bonding between different layers and avoid the risk of detachment, thereby improving the bonding strength between different structural layers.

[0038] (3) Furthermore, the present invention can effectively control the relative content of carbon fiber and pores by changing the thickness of the mesh layer in the 2.5D needle-punched carbon fiber preform, thereby achieving gradient changes in the preform structure and gradient changes in the properties of the prepared carbon fiber reinforced composite material.

[0039] (4) The present invention effectively alleviates the difference in thermal expansion coefficient through gradient transition and fiber synergy, avoiding the peeling failure caused by the brittleness and interface mismatch of traditional coatings; at the same time, the integrated preform of the present invention only needs one co-densification and partition modification to be formed in one step, which can greatly shorten the process cycle, eliminate the need for multiple steps, and improve production efficiency. Attached Figure Description

[0040] Figure 1 The cross-sectional SEM morphology of the gradient structure carbon fiber preform prepared in Example 1 of the present invention is shown.

[0041] Figure 2 This is a schematic diagram of the gradient structure carbon fiber preform prepared in Example 1 of the present invention.

[0042] Figure 3 This is a SEM cross-sectional microstructure image of the C / C composite material after the gradient structure carbon fiber preform prepared in Example 1 was densified by chemical vapor infiltration. Detailed Implementation

[0043] The technical solution of the present invention will be clearly and completely described below through specific embodiments. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0044] The present invention will be further described below by way of examples, but the scope of protection of the present invention is not limited to these embodiments. Unless otherwise stated, the raw materials and reagents used in the following examples are commercially available products or can be prepared by known methods.

[0045] Example 1

[0046] (1) A layered and stitched carbon fiber preform was prepared by progressively laying down eight-end satin-weave carbon fiber fabric to a thickness of 10 mm, followed by stitching with 1 kJ continuous carbon fiber at a Z-direction spacing of 10 mm × 10 mm. After preparation, the density of the stitched carbon fiber preform was 0.85 g / cm³. 3 .

[0047] (2) Prepare needle-punched carbon fiber preforms separately. A layer of 0.8 mm thick chopped fibers is laid as the bottom layer. Then, a 0° non-woven fabric is laid on top of the chopped fibers, followed by another layer of chopped fibers of the same thickness. Needling is then performed. This alternating layering of chopped fibers and non-woven fabric is repeated, maintaining a needle-punching depth of 5 mm and a needle-punching density of 8 needles / cm². 2The thickness of the mesh layer is maintained at 0.8 mm, and adjacent non-woven fabric layers are laid alternately at 0° and 90°, and needled after each layup. The above work is repeated until the thickness of the 2.5D needled carbon fiber preform reaches 10 mm, thus obtaining a 2.5D needled carbon fiber preform with uniform structure.

[0048] (3) The 2.5D needle-punched carbon fiber preform prepared above is stacked on top of the laminated and stitched carbon fiber preform, and continuous fibers (polyacrylonitrile (PAN) based carbon fiber, 1K) are integrally stitched in the Z direction. The stitching spacing is 10mm×10mm, and the carbon fiber lines are located at the center of the stitching of the laminated and stitched preform. Finally, a gradient structure carbon fiber preform is obtained.

[0049] Example 2

[0050] (1) A layered and stitched carbon fiber preform was prepared by progressively laying down eight-end satin-weave carbon fiber fabric to a thickness of 10 mm, followed by stitching with 1 kJ continuous carbon fiber at a Z-direction spacing of 10 mm × 10 mm. After preparation, the density of the stitched carbon fiber preform was 0.85 g / cm³. 3 .

[0051] (2) First, lay a 0° non-woven fabric, then lay a layer of chopped fibers on the non-woven fabric to a thickness of 0.3 mm. Next, lay a 90° non-woven fabric on top of the chopped fiber mesh layer, and then continue laying chopped fibers to a thickness of 0.3 mm. Then, perform needle punching with a needle to a depth of 3 mm. Repeat the above process until the thickness of the 2.5D needle-punched carbon fiber preform reaches 3 mm. Then, increase the thickness of the chopped fiber layer to 1 mm, performing needle punching after each layer of chopped fibers, until the total thickness of the 2.5D needle-punched carbon fiber preform is 10 mm. The density per unit thickness of the preform increases from 0.6 g / cm³ from bottom to top. 3 Reduced to 0.4 g / cm³ 3 The needle-punching density increases from 15 needles / cm along the direction from where it meets the laminated carbon fiber preform to the direction away from it. 2 2 needles / cm 2 Decrease to 9 stitches / cm 2 .

[0052] (3) The 2.5D needle-punched carbon fiber preform prepared above is stacked on top of the laminated and stitched carbon fiber preform, and continuous fibers (polyacrylonitrile (PAN) based carbon fiber, 1K) are integrally stitched in the Z-direction. The side with a mesh layer thickness of 0.3 mm is attached to the laminated and stitched carbon fiber preform. The stitching spacing is 10 mm × 10 mm, and the carbon fiber lines are located at the center of the stitching of the laminated and stitched preform. Finally, a gradient structure carbon fiber preform is obtained.

[0053] The gradient-structured carbon fiber preform prepared in Example 2 was used as a reinforcement in gradient carbon fiber reinforced ceramic modified composite materials. The specific application process is as follows:

[0054] The gradient-structured carbon fiber preform and the needle-punched preform are wrapped with graphite paper without gaps, exposing only the top surface of the laminated and stitched structure. The wrapped carbon fiber preform is then clamped in a deposition fixture. The deposition fixture consists of a solid graphite plate and a porous graphite plate stacked on top of each other, with the carbon fiber preform clamped in a cavity formed between the solid and porous graphite plates. During clamping, one side of the laminated and stitched carbon fiber preform is positioned on the side of the porous graphite plate, where the cavity area of ​​the porous graphite plate is arrayed with vent holes, each 10 mm in diameter, and the distance between the central axes of adjacent vent holes is one time the diameter of the vent hole.

[0055] Subsequently, four deposition fixtures containing carbon fiber preforms were placed at intervals in the chemical vapor deposition furnace, with the spacing between adjacent fixtures controlled at 30 mm, and the porous graphite plates in any two fixtures facing the same direction. Then, using propylene as the carbon source gas and nitrogen as the diluent gas, the carbon fiber preforms were periodically densified using chemical vapor deposition. The propylene flow rate was 30±5 L / min, the nitrogen flow rate was 10±2 L / min, the deposition temperature was 930 ℃, the furnace pressure was controlled between 0.6-1.0 kPa, and the single deposition time was 100 h. After each deposition, the furnace temperature was lowered to below 100℃ before removal from the furnace. The fixtures were removed, and the C / C composite material was taken out. The C / C composite material on one side of the porous graphite fixture was then subjected to surface removal processing to open the closed pores. Afterwards, the fixture clamping, sample placement, and unidirectional CVI process were repeated according to the above procedure. After a total deposition time of 500 hours, an average density of 1.31 g / cm³ was obtained. 3 It is a C / C porous body with a density gradient along its thickness. The density of the C / C porous body on the side in contact with the porous graphite plate can reach 1.48 g / cm³. 3 The C / C porous body density on the side in contact with the solid graphite plate is maintained at 1.24 g / cm³. 3 .

[0056] After completing the unidirectional CVI, the thickness on one side of the laminated stitch structure is maintained at 5.5 mm, and the thickness on the other side of the needle-punched structure is maintained at 3 mm. Then, part of it is cut into carbon porous bodies with a planar size of 100×130 mm, which are used as preforms for unidirectional RMI.

[0057] A carbon-carbon porous body is placed in a graphite crucible of suitable size, with the lower 2.5D needle-punched C / C porous body facing upwards and the layered stitched C / C porous body facing downwards. Small graphite blocks are used to elevate the bottom surface of the graphite crucible and the high-density surface of the carbon-carbon porous body, or the body is placed in a graphite crucible with a stepped bottom, creating pores of 5 mm in height between the high-density surface and the bottom of the graphite crucible. Then, graphite paper is used to fill the gaps between the sidewalls of the graphite crucible and the sides of the carbon-carbon porous body to fix the C / C porous body within the inner cavity of the graphite crucible. A bottomless graphite frame is placed above the low-density surface of the carbon-carbon porous body. The outer diameter of the graphite frame is equal to the area of ​​the C / C porous body used for melting and infiltration, which is 100 × 130 mm. The thickness of the graphite frame is set to 10 mm, and the height is set according to the height of the melting and infiltration material to be filled. The graphite frame and the inner wall of the graphite crucible are filled with graphite paper or graphite blocks and graphite paper to fix the graphite frame in the graphite crucible, keeping the relative positions of the crucible, C / C porous body, and graphite frame relatively fixed. Then, Zr-Hf-Ti mixed powder is placed inside the graphite frame, and the thickness of the Zr-Hf-Ti mixed powder is controlled to be 9 mm. After completion, the graphite crucible is sealed and transferred to the melting and infiltration furnace. After the melting and infiltration furnace is closed, the furnace is evacuated and the sealing performance is measured. After the sealing performance meets the standard, the temperature is increased to 2000 °C at a rate of 10 °C / min, and the reaction melting and infiltration is carried out. During the melting and infiltration process, the furnace was kept at 300 ℃ and 1300 ℃ for 30 min to ensure uniform temperature inside the furnace. After holding at 2000 ℃ for 20 min, heating was stopped and the furnace was cooled down. After the temperature dropped below 300 ℃, argon gas was filled into the furnace and the temperature was further cooled down to below 100 ℃ before the sample was removed from the furnace.

[0058] After melt infiltration, the density of the resulting gradient carbon fiber reinforced ceramic modified composite material is 2.96 g / cm³. 3 Using a plasma ablation device with an output power of 48 kW for 60 s, the linear ablation rate was -3.85 μm / s, and the mass ablation rate was 3.15 mg / s. The flexural strength of the laminated and stitched carbon fiber reinforced composite material at 2000 ℃ was 271 MPa.

[0059] Example 3

[0060] (1) A layered carbon fiber eight-end satin fabric was laid up to a thickness of 12 mm, and then 1 kJ continuous carbon fiber was sewn together in the Z direction at a spacing of 10 mm × 10 mm to prepare a laminated and sewn carbon fiber preform. After preparation, the density of the laminated and sewn carbon fiber preform was 0.9 g / cm³. 3 .

[0061] (2) Lay a 0° non-woven fabric on one side of the laminated carbon fiber preform, then lay a 0.5 mm thick layer of chopped fibers on top of the non-woven fabric, and then use a needle to puncture the fibers to a depth of 3 mm and a puncture density of 15 needles / cm. 2 After needle punching, a 90° non-woven fabric is laid on top of the chopped fiber layer, followed by a 0.5mm layer of chopped fibers, and then needle punched again using the same needle punching parameters. This process is repeated until the needle-punched carbon fiber preform reaches a thickness of 2mm.

[0062] (3) Increase the thickness of the chopped fiber layup to 1 mm, and then needle-punch using the same needle-punching process parameters until the thickness of the needle-punched carbon fiber preform reaches 10 mm. The final result is a carbon fiber preform with a gradient structure where the thickness of the mesh layer increases from bottom to top. The density per unit thickness of the mesh layer increases from 0.6 g / cm³ from bottom to top. 3 Reduced to 0.4 g / cm³ 3 .

[0063] (4) After needle punching, the gradient carbon fiber preform is stitched together with 1K continuous fiber. The stitching spacing is consistent with the spacing of the stacked preform, but the stitching line is located at the center of the stitching line of the stacked preform.

[0064] Example 4

[0065] It is basically the same as Example 2, except that the two layers of satin fabric connecting the laminated and sewn carbon fiber preform and the 2.5D needle-punched structure preform are replaced with spread fabric.

[0066] The gradient-structured carbon fiber preform prepared in Example 4 was used as a reinforcement in the gradient carbon fiber reinforced ceramic modified composite material, and the specific application process was the same as in Example 2; the density of the obtained gradient carbon fiber reinforced ceramic modified composite material was measured to be 2.09 g / cm³. 3 .

[0067] Using a plasma ablation device with an output power of 48 kW, a 60-second ablation test was conducted. The linear ablation rate was -1.37 μm / s, the mass ablation rate was 8.25 mg / s, and the surface response temperature during stable ablation was above 2600℃.

[0068] In addition, the gradient carbon fiber reinforced ceramic modified composite material has a flexural strength of 284.30 MPa and a flexural modulus of 26049 MPa at 2000 ℃.

[0069] Example 5

[0070] It is basically the same as Example 2, except that the integrated stitching line of the gradient structure carbon fiber preform and the stitching line of the laminated stitching structure carbon fiber preform coincide in position.

[0071] Example 6

[0072] It is basically the same as Example 2, except that the outermost 7cm satin fabric on one side of the laminated carbon fiber preform is replaced with a regular weave fabric.

[0073] Example 7

[0074] Similar to Example 2, except that after laying a non-woven fabric layer and chopped fibers on top of the laminated sewn blank, it is impregnated with low-flow resin and then needle-punched, so that the resin can penetrate to a limited extent between the non-woven fabric and the laminated sewn blank below, thereby improving the bonding strength between the interfaces of the two different structural blanks.

[0075] Example 8

[0076] The procedure is essentially the same as in Example 2, except that a resin-coated nonwoven fabric layer is laid on the surface of the laminated and stitched carbon fiber preform, followed by a layer of chopped fibers for needle punching. This process is repeated three times for a total of four times, using resin-coated nonwoven fabric for both layering and needle punching.

[0077] Example 9

[0078] The example is basically the same as Example 2, except that the needle density of each layer of the mesh layer is 15 needles / cm. 2 , rather than gradient.

[0079] Comparative Example 1

[0080] It is basically the same as Example 2, except that the thickness gradient trend of the mesh layer in the 2.5D needle-punched structure is opposite to that in Example 2, that is, it decreases from bottom to top, and the thickness of each layer is the same as in Example 2.

[0081] The above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit it. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a gradient structure carbon fiber preform, characterized by: step include: S1 uses continuous fibers as stitching thread to stitch multiple layers of stacked carbon fiber woven fabric in the Z direction to obtain a laminated and stitched carbon fiber preform. S2 combines the laminated and stitched carbon fiber preform with the 2.5D needle-punched carbon fiber preform, such that the laminated and stitched carbon fiber preform is located below the 2.5D needle-punched carbon fiber preform; the 2.5D needle-punched carbon fiber preform is formed by alternating layers of non-woven fabric and mesh layer and then needle-punching them together. The composite method is as follows: the laminated and stitched carbon fiber preform and the 2.5D needle-punched carbon fiber preform are prepared separately in advance and then laminated; or the non-woven fabric and the mesh layer are alternately laid on one side of the laminated and stitched carbon fiber preform and needle-punched and connected; then the composite is stitched in the Z direction using continuous carbon fiber.

2. The method for preparing a gradient structure carbon fiber preform according to claim 1, characterized in that: The continuous fiber is a 1k or 3k carbon fiber bundle; The suture density of the Z-direction suture is between 3mm×3mm and 15mm×15mm; The thickness of the laminated and stitched carbon fiber preform is 3~30mm; The thickness of the mesh layer increases gradually from bottom to top.

3. The method for preparing a gradient structure carbon fiber preform according to claim 2, characterized in that: In S2, the needle density of each layer in the 2.5D needled structure ranges from 15 to 30 needles / cm along the direction from contact with the laminated and stitched carbon fiber preform to the direction away from it. 2 Decrease to 8 or more stitches per cm and less than 15 stitches per cm 2 .

4. The method for preparing a gradient structure carbon fiber preform according to claim 2, characterized in that: The thickness of the mesh layer increases gradually from bottom to top from 0.2~0.6mm to 0.8~2mm.

5. The method for preparing a gradient structure carbon fiber preform according to claim 4, characterized in that: The density per unit thickness of the 2.5D needle-punched structure ranges from 0.5 to 0.8 g / cm³ from bottom to top. 3 Reduced to 0.3~0.5 g / cm³ 3 ; The density of the laminated and stitched carbon fiber preform is 0.7~1 g / cm³. 3 .

6. The method for preparing a gradient structure carbon fiber preform according to claim 1, characterized in that: In the 2.5D needle-punched carbon fiber preform, adjacent non-woven fabrics are placed at an angle of 0~90°.

7. The method for preparing a gradient structure carbon fiber preform according to claim 6, characterized in that: The Z-direction suture lines in S1 and S2 coincide, or the suture position of S2 is located at the exact center of the suture line of the laminated carbon fiber preform.

8. A gradient-structured carbon fiber preform, characterized in that: It is obtained by the preparation method according to any one of claims 1 to 7.

9. An application of the gradient structure carbon fiber preform as described in claim 8, characterized in that: It is used as a raw material in ceramic-modified carbon fiber reinforced composites with gradient structures.