A magnesium-based hydrogen storage material with multi-center relay catalysis and its preparation method

By constructing a multi-center relay catalytic system inside magnesium-based hydrogen storage materials and utilizing the synergistic effect of Mg2Ni phase, REHx and nano Mo2C spheres, the problems of high hydrogen release temperature and slow kinetics in magnesium-based hydrogen storage materials were solved, achieving efficient hydrogen storage and release.

CN123105544APending Publication Date: 2026-11-17NORTHWEST INSTITUTE FOR NONFERROUS METAL RESEARCH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611448001.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-17
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing magnesium-based hydrogen storage materials struggle to balance hydrogen absorption/desorption kinetics and desorption temperature, and suffer from insufficient cycle stability. Current modifications are mostly limited to a single mechanism or a single catalytic center, failing to effectively construct multiple complementary and synergistic catalytic centers.

Method used

By constructing Mg2Ni phase and REHx catalytic centers inside the material through alloying design, and externally doping with nano-Mo2C spheres, three functionally complementary catalytic centers are formed, realizing a multi-center relay catalytic system, reducing the hydrogen desorption temperature and improving the hydrogen absorption and desorption kinetics.

Benefits of technology

Significantly reduce the hydrogen release temperature to 150℃~170℃, improve hydrogen absorption and release kinetics, maintain high hydrogen storage capacity, and realize the coupling utilization of medium and low temperature waste heat and cycle stability of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123105544A_ABST
    Figure CN123105544A_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing a magnesium-based hydrogen storage material with multi-center relay catalysis. The preparation method includes the following steps: 1. Mixing ammonium molybdate solution and dopamine hydrochloride ethanol solution, adding ammonia water and stirring, collecting the precipitate, and calcining the precipitate under an inert atmosphere to obtain nano-Mo2C spheres; 2. Mg 100‑a‑ b Ni a RE b The matrix alloy is crushed and then ball-milled with nano-Mo2C balls to obtain a magnesium-based hydrogen storage material with multi-center relay catalysis. This invention also discloses a magnesium-based hydrogen storage material with multi-center relay catalysis. This invention constructs an in-situ Mg2Ni phase and REH phase internally through alloying design. x Two catalytic centers are introduced, and a third catalytic center is introduced through external doping with nano-Mo2C spheres. The three centers complement each other and work synergistically to form a multi-center relay catalytic system inside the material, thereby significantly reducing the hydrogen desorption temperature and improving the hydrogen absorption and desorption kinetics, making it suitable for the energy field.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of hydrogen storage material technology, and in particular relates to a magnesium-based hydrogen storage material with multi-center relay catalysis and its preparation method. Background Technology

[0002] The hydrogen energy industry chain involves hydrogen production, storage, transportation, and end-use applications. Currently, the safe and efficient storage and transportation of hydrogen has become a critical issue that the hydrogen energy industry urgently needs to overcome. Solid-state hydrogen storage technology is considered one of the key technologies to overcome the material and cost bottlenecks in hydrogen storage and transportation due to its advantages such as good safety, high volumetric hydrogen storage density, and high purity of released hydrogen. Among them, magnesium-based solid-state hydrogen storage materials have become a highly cost-effective choice due to their advantages such as high hydrogen storage capacity, low material preparation cost, and good reversibility of hydrogen absorption and desorption. However, the slow hydrogen absorption and desorption kinetics and the excessively high hydrogen desorption temperature still limit the practical application of magnesium-based hydrogen storage materials.

[0003] Currently, the optimization strategies for magnesium-based solid-state hydrogen storage materials mainly include nano-sizing, external catalysis, and alloying design. Nano-sizing primarily improves hydrogen absorption and desorption kinetics by reducing particle size and shortening the diffusion path of hydrogen atoms within the matrix. However, nanoparticles are prone to aggregation, growth, and surface oxidation during cyclic hydrogen absorption and desorption. Furthermore, the preparation cost of nanoparticles is high, and their safety in air is poor, making it difficult to meet the needs of large-scale storage and transportation applications. External catalysis typically involves introducing transition metals, metal compounds, or carbon-based materials into magnesium-based materials to lower the hydrogen desorption temperature and accelerate the absorption and desorption rates. However, external doping of a single catalyst often provides only a limited number of surface active sites, and the catalytic mechanism is singular. Alloying design introduces other elements to form crystal defects and an active second phase, promoting hydrogen transport within the material. However, existing technologies lack effective synergy between the second phases, making it difficult to achieve relay catalysis for the entire process of "hydrogen dissociation - hydrogen atom diffusion - Mg / MgH2 reversible phase transition."

[0004] In summary, existing modifications of magnesium-based hydrogen storage materials are mostly limited to a single mechanism or a single catalytic center, failing to effectively construct multiple functionally complementary and synergistic catalytic centers within the material. This results in a difficulty in balancing hydrogen absorption / desorption kinetics and hydrogen desorption temperature, as well as insufficient cycle stability. Therefore, there is an urgent need for a magnesium-based hydrogen storage material and its preparation method that can construct a multi-center, relay-style catalytic system within the material to synergistically address the problems of sluggish kinetics and excessively high hydrogen desorption temperature. Summary of the Invention

[0005] The purpose of this invention is to overcome the shortcomings of the prior art and provide a method for preparing magnesium-based hydrogen storage materials with multi-center relay catalysis. This preparation method utilizes alloying design to construct the Mg2Ni phase in situ within the material and form REH during hydrogen storage. x(Rare earth hydride phase) Two catalytic centers are introduced, and a third catalytic center is introduced through external doping of nano Mo2C spheres; the three catalytic centers complement each other and work together to form a multi-center relay catalytic system inside the material, thereby significantly reducing the hydrogen desorption temperature and improving the hydrogen absorption and desorption kinetics. This solves the problem that existing magnesium-based hydrogen storage materials have difficulty in balancing hydrogen absorption and desorption kinetics and hydrogen desorption temperature, and have insufficient cycle stability.

[0006] To achieve the above objectives, the technical solution adopted by the present invention is: a method for preparing a magnesium-based hydrogen storage material with multi-center relay catalysis, the preparation method comprising the following steps: Step 1: Mix and stir ammonium molybdate solution and dopamine hydrochloride ethanol solution, add ammonia water and stir, collect the precipitate, calcine the precipitate under an inert atmosphere to obtain nano Mo2C spheres; Step 2: Add Mg 100-a-b Ni a RE b The matrix alloy, after being crushed, is ball-milled and mixed with the nano-Mo2C spheres obtained in step one to obtain a magnesium-based hydrogen storage material with multi-center relay catalysis; the Mg 100-a-b Ni a RE b RE in the matrix alloy is a rare earth alloying element.

[0007] This invention involves mixing and stirring an ammonium molybdate solution and a dopamine hydrochloride ethanol solution, followed by the addition of ammonia water. This causes dopamine to polymerize, coat, and self-assemble on the surface of a molybdenum source, forming a precipitate. After calcination, nano-Mo2C spheres are obtained. Subsequently, the nano-Mo2C spheres and crushed Mg... 100-a-b Ni a RE b Using a matrix alloy as raw material, a magnesium-based hydrogen storage material composite with multi-center relay catalysis is obtained after ball milling and mixing. This magnesium-based hydrogen storage material forms three catalytic centers, which complement each other and work synergistically to significantly reduce the hydrogen desorption temperature and improve the hydrogen absorption and desorption kinetics.

[0008] In the above-mentioned method for preparing a magnesium-based hydrogen storage material with multi-center relay catalysis, the mass ratio of ammonium molybdate to dopamine hydrochloride in step one is 1:(1~1.5), the concentration of the ammonium molybdate solution is 3mg / mL~4mg / mL, and the concentration of the dopamine hydrochloride ethanol solution is 1.8mg / mL~2.4mg / mL.

[0009] In the above-mentioned method for preparing a magnesium-based hydrogen storage material with multi-center relay catalysis, the volume of ammonia water in step one accounts for 0.7% to 1.0% of the total volume of ammonium molybdate solution and dopamine hydrochloride ethanol solution.

[0010] In the above-mentioned method for preparing a magnesium-based hydrogen storage material with multi-center relay catalysis, the calcination temperature in step one is 800℃~900℃, and the calcination time is 3h~5h.

[0011] In the above-mentioned method for preparing a magnesium-based hydrogen storage material with multi-center relay catalysis, the diameter of the nano-Mo2C spheres in step one is 300nm~500nm.

[0012] The above-mentioned method for preparing a magnesium-based hydrogen storage material with multi-center relay catalysis, wherein step two involves crushing the Mg... 100-a-b Ni a RE b The particle size of the matrix alloy is 100-200 mesh.

[0013] This invention controls the diameter of the nano-Mo2C spheres to be 300nm~500nm and Mg... 100-a-b Ni a RE b The matrix alloy has a particle size of 100-200 mesh to increase the surface area, thereby increasing the reaction contact surface during hydrogen storage and accelerating the reaction efficiency.

[0014] In the above-mentioned method for preparing a magnesium-based hydrogen storage material with multi-center relay catalysis, the RE in step two is one of La, Ce, Y, and Gd, and the Mg... 100-a-b Ni a RE b In the matrix alloy, both a and b are atomic ratios, where a is 1~5 and b is 1~3.

[0015] The above-mentioned method for preparing a magnesium-based hydrogen storage material with multi-center relay catalysis, wherein the magnesium-based hydrogen storage material with multi-center relay catalysis in step two is composed of the following components by mass percentage: 3%~10% nano-Mo2C spheres, with the balance being Mg. 100-a- b Ni a RE b Matrix alloy.

[0016] This invention uses Mo2C as the catalytic center, which can significantly reduce the hydrogen desorption temperature and improve the hydrogen absorption and desorption kinetics. However, Mo2C itself hardly stores hydrogen. When the proportion of Mo2C added is too high, it will reduce the overall reversible hydrogen storage capacity of the material. Therefore, limiting it to 3%~10% can achieve the optimal balance between catalytic activity and hydrogen storage capacity.

[0017] This invention also discloses a magnesium-based hydrogen storage material with multi-center relay catalysis, which is obtained by the above-mentioned preparation method of a magnesium-based hydrogen storage material with multi-center relay catalysis.

[0018] The above-mentioned multi-center relay catalytic magnesium-based hydrogen storage material, wherein the multi-center relay catalytic magnesium-based hydrogen storage material is heated at a rate of 3°C·min -1 Under argon conditions, the initial hydrogen release temperature is 150℃~170℃; and the reversible hydrogen absorption capacity of the magnesium-based hydrogen storage material with multi-center relay catalysis is not less than 5.5wt. under the conditions of hydrogen absorption pressure of 4MPa, hydrogen absorption temperature of 250℃ and hydrogen absorption time of 60min.

[0019] Compared with the prior art, the present invention has the following advantages: 1. This invention utilizes nano-Mo2C spheres and crushed Mg 100-a-b Ni a RE b Using a matrix alloy as raw material, a multi-center relay catalytic magnesium-based hydrogen storage material composite was obtained after ball milling. This resulted in the in-situ construction of a Mg2Ni phase within the magnesium-based hydrogen storage material composite, and the formation of REH during the hydrogen storage process. x The three complementary catalytic centers, consisting of the phase and the external composite nano-Mo2C spheres, achieve relay catalysis of "H2 dissociation-hydrogen atom overflow / diffusion-MgH2 reversible phase transition", breaking through the performance bottleneck of a single catalytic center.

[0020] 2. The preparation method of the present invention adopts the conventional process route of smelting + ball milling, which has the characteristics of low cost, simple process, readily available raw materials, low equipment requirements, easy scale-up and suitability for large-scale preparation.

[0021] 3. The magnesium-based hydrogen storage material prepared by this invention with multi-center relay catalysis has the characteristics of significantly reduced hydrogen desorption temperature and high hydrogen storage capacity: at a heating rate of 3℃·min -1 Under argon conditions, the initial hydrogen release temperature is 150℃~170℃, which is much lower than that of pure MgH2 (about 400℃) and conventional magnesium-based hydrogen storage materials, which is beneficial for the coupling utilization of medium and low temperature waste heat. At the same time, under the conditions of hydrogen absorption pressure of 4MPa, hydrogen absorption temperature of 250℃ and hydrogen absorption time of 60min, the reversible hydrogen absorption capacity is not less than 5.5wt.%, maintaining the intrinsic advantage of high capacity of magnesium-based hydrogen storage materials.

[0022] The technical solution of the present invention will be further described in detail below with reference to the accompanying drawings and embodiments. Attached Figure Description

[0023] Figure 1 This is a morphology diagram of the nano-Mo2C spheres prepared in Example 1 of the present invention.

[0024] Figure 2 This is a 2000x magnification image of the magnesium-based hydrogen storage material with multi-center relay catalysis prepared in Example 1 of the present invention.

[0025] Figure 3This is a 20,000x magnification image of the magnesium-based hydrogen storage material with multi-center relay catalysis prepared in Example 1 of this invention. Detailed Implementation

[0026] Example 1 The preparation method of this embodiment includes the following steps: Step 1: Weigh 240 mg of ammonium molybdate and 240 mg of dopamine hydrochloride, and dissolve them separately in 64 mL of deionized water and 128 mL of anhydrous ethanol, stirring thoroughly until completely dissolved. Mix the two solutions and continue stirring. Add 1.4 mL of ammonia water (containing 30% NH3·H2O by mass), and continue stirring for 4 hours to allow dopamine to polymerize, coat, and self-assemble on the surface of the molybdenum source. After the reaction, centrifuge to collect the precipitate, wash it alternately with deionized water and anhydrous ethanol, and calcine it at 800℃ for 3 hours under an argon atmosphere to obtain the following... Figure 1 The image shows Mo2C nanospheres with diameters ranging from 300 nm to 500 nm. Step 2, according to Mg 95 To obtain Ni3La2, stoichiometric amounts of Mg, Mg-Ni master alloy, and Mg-La master alloy with a purity higher than 99.9% were weighed and placed in a crucible resistance furnace. Under argon protection, the furnace temperature was raised to 750°C until the raw materials were fully melted. After holding at this temperature for 30 minutes, the mixture was cast into a stainless steel mold and cooled to obtain Mg. 95 Ni3La2 matrix alloy; Mg 95 The Ni3La2 matrix alloy was mechanically crushed to 100 mesh and mixed with the nano-Mo2C spheres obtained in step one in an argon-atmosphere ball mill jar. The mixture was then subjected to a reaction between the Mg2Ni phase and REH... x Based on this, a third catalytic center, nano-Mo2C spheres, is introduced to obtain a magnesium-based hydrogen storage material with multi-center relay catalysis, characterized by a significantly reduced hydrogen desorption temperature and high hydrogen storage capacity. The mass of the nano-Mo2C spheres accounts for 5% of the total mass of the magnesium-based hydrogen storage material with multi-center relay catalysis. The ball milling parameters are: ball-to-material ratio 20:1, rotation speed 150 r·min. -1 The ball milling time is 2 hours.

[0027] The magnesium-based hydrogen storage material prepared in this embodiment, featuring multi-center relay catalysis, is as follows: Figure 2 and Figure 3 As shown, the nano Mo2C balls retain their original shape after ball milling and are evenly distributed on the alloy surface.

[0028] Example 2 The difference between this embodiment and Embodiment 1 is that: Mg 100-a-b Ni a RE b The matrix alloy has the composition of Mg. 97The mass of Ni1La2 nano-Mo2C spheres accounts for 3% of the total mass of the magnesium-based hydrogen storage material in the multi-center relay catalysis.

[0029] Example 3 The difference between this embodiment and Embodiment 1 is that: Mg 100-a-b Ni a RE b The matrix alloy has the composition of Mg. 96 The mass of Ni1Y3 nano-Mo2C spheres accounts for 10% of the total mass of the magnesium-based hydrogen storage material in the multi-center relay catalysis.

[0030] Example 4 The difference between this embodiment and Embodiment 1 is that: Mg 100-a-b Ni a RE b The matrix alloy has the composition of Mg. 94 Ni5Ce1.

[0031] Example 5 The difference between this embodiment and Embodiment 1 is that: Mg 100-a-b Ni a RE b The matrix alloy has the composition of Mg. 96 Ni2Gd2.

[0032] Example 6 The difference between this embodiment and Embodiment 1 is as follows: In step one, the concentration of ammonium molybdate solution is 3 mg / mL, the concentration of dopamine hydrochloride ethanol solution is 2.25 mg / mL, the mass ratio of ammonium molybdate to dopamine hydrochloride is 1:1.5, ammonia water is added, and the volume of the ammonia water accounts for 0.7% of the total volume of the ammonium molybdate solution and the dopamine hydrochloride ethanol solution (the ammonia water contains 30% NH3·H2O by mass), the calcination temperature is 900℃, and the calcination time is 5 hours; in step two, Mg... 95 Ni3La2 matrix alloy is mechanically crushed to 200 mesh.

[0033] Example 7 The difference between this embodiment and Embodiment 1 is as follows: In step one, the concentration of ammonium molybdate solution is 4 mg / mL, the concentration of dopamine hydrochloride ethanol solution is 2.4 mg / mL, the mass ratio of ammonium molybdate to dopamine hydrochloride is 1:1.2, ammonia water is added, and the volume of the ammonia water accounts for 1.0% of the total volume of the ammonium molybdate solution and the dopamine hydrochloride ethanol solution (the ammonia water contains 30% NH3·H2O by mass). The calcination temperature is 850℃ and the calcination time is 4 hours; in step two, Mg... 95 Ni3La2 matrix alloy is mechanically crushed to 150 mesh.

[0034] Example 8 The difference between this embodiment and Embodiment 1 is as follows: In step one, the concentration of ammonium molybdate solution is 3.4 mg / mL, the concentration of dopamine hydrochloride ethanol solution is 1.8 mg / mL, the mass ratio of ammonium molybdate to dopamine hydrochloride is 1:1.05, ammonia water is added, and the volume of the ammonia water accounts for 0.85% of the total volume of the ammonium molybdate solution and the dopamine hydrochloride ethanol solution (the ammonia water contains 30% NH3·H2O by mass). The calcination temperature is 800℃ and the calcination time is 3 hours; in step two, Mg... 95 Ni3La2 matrix alloys are mechanically crushed to 100 mesh.

[0035] Comparative Example 1 The preparation method of this comparative example is as follows: Mg powder with a mass purity greater than 99.9% is subjected to the same ball milling process as in Example 1.

[0036] Comparative Example 2 The preparation method of this comparative example is as follows: according to Mg 97 The stoichiometric proportions of Mg and Mg-Ni master alloy were weighed and placed in a crucible resistance furnace. Under argon protection, the furnace temperature was raised to 750°C until the raw materials were fully melted. After holding at this temperature for 30 minutes, the mixture was cast into a stainless steel mold and cooled to obtain Mg. 97 Ni3 alloy; for Mg 97 The Ni3 alloy was subjected to the same ball milling process as in Example 1.

[0037] Comparative Example 3 The difference between this comparative example and Example 1 is that no nano Mo2C spheres are added during the preparation of the magnesium-based hydrogen storage material, while the rest of the process is the same as in Example 1.

[0038] The performance of the magnesium-based hydrogen storage materials prepared in Examples 1-8 and Comparative Examples 1-3 was tested: The reversible hydrogen absorption was tested using the Sieverts volumetric method under conditions of hydrogen pressure 4 MPa, absorption temperature 250 °C, and absorption time 60 min; and a simultaneous thermal analyzer (TG-DSC) was used at a heating rate of 3 °C / min. -1 The initial hydrogen release temperature of each sample was tested under argon gas with a volume purity greater than 99.9%, and the performance is shown in Table 1. Table 1. Results of Composition and Performance Tests

[0039] As shown in Table 1, the high hydrogen desorption temperature and extremely poor kinetics of Mg in Comparative Example 1 resulted in a reversible hydrogen storage capacity far lower than the theoretical hydrogen storage capacity (7.6 wt.%). Although Comparative Examples 2 and 3 improved the hydrogen desorption temperature and capacity by designing internal catalytic centers of Mg2Ni, Mg2Ni, and LaH2, respectively, the initial hydrogen desorption temperature was still relatively high. In contrast, Examples 1-8, by combining nano-Mo2C spheres with alloyed internal dual catalytic centers, reduced the initial hydrogen desorption temperature of the magnesium-based hydrogen storage material to 150℃~170℃, and the reversible hydrogen absorption capacity reached over 6.1 wt.%, fully verifying the "Mg2Ni phase + REH2" principle. x The synergistic effect of the multi-center relay catalytic system of "phase + nano Mo2C spheres" on improving kinetics and hydrogen desorption temperature.

[0040] The above description is merely a preferred embodiment of the present invention and does not constitute any limitation on the present invention. Any simple modifications, alterations, or equivalent structural transformations made to the above embodiments based on the technical essence of the present invention shall still fall within the protection scope of the present invention.

Claims

1. A method for preparing a magnesium-based hydrogen storage material with multi-center relay catalysis, characterized in that, The preparation method includes the following steps: Step 1: Mix and stir ammonium molybdate solution and dopamine hydrochloride ethanol solution, add ammonia water and stir, collect the precipitate, calcine the precipitate under an inert atmosphere to obtain nano Mo2C spheres; Step two, ball-mixing Mg 100-a-b Ni a RE b The matrix alloy is broken and ball-mixed with the nano-Mo2C balls obtained in step one to obtain a multi-center relay catalyzed magnesium-based hydrogen storage material; the Mg 100-a-b Ni a RE b The RE in the matrix alloy is a rare earth alloying element.

2. The method for preparing a magnesium-based hydrogen storage material with multi-center relay catalysis according to claim 1, characterized in that, In step one, the mass ratio of ammonium molybdate to dopamine hydrochloride is 1:(1~1.5), the concentration of the ammonium molybdate solution is 3mg / mL~4mg / mL, and the concentration of the dopamine hydrochloride ethanol solution is 1.8mg / mL~2.4mg / mL.

3. The method for preparing a magnesium-based hydrogen storage material with multi-center relay catalysis according to claim 1, characterized in that, In step one, the volume of ammonia water accounts for 0.7% to 1.0% of the total volume of ammonium molybdate solution and dopamine hydrochloride ethanol solution.

4. The method for preparing a magnesium-based hydrogen storage material with multi-center relay catalysis according to claim 1, characterized in that, The calcination temperature in step one is 800℃~900℃, and the calcination time is 3h~5h.

5. The method for preparing a magnesium-based hydrogen storage material with multi-center relay catalysis according to claim 1, characterized in that, The diameter of the nano Mo2C spheres mentioned in step one is 300nm~500nm.

6. The method for preparing a magnesium-based hydrogen storage material with multi-center relay catalysis according to claim 1, characterized in that, The crushed Mg described in step two 100-a-b Ni a RE b The particle size of the matrix alloy is 100-200 mesh.

7. The method for preparing a magnesium-based hydrogen storage material with multi-center relay catalysis according to claim 1, characterized in that, In step two, RE is one of La, Ce, Y, and Gd, and Mg... 100-a-b Ni a RE b In the matrix alloy, both a and b are atomic ratios, where a is 1~5 and b is 1~3.

8. The method for preparing a magnesium-based hydrogen storage material with multi-center relay catalysis according to claim 1, characterized in that, The magnesium-based hydrogen storage material with multi-center relay catalysis described in step two consists of the following components by mass percentage: 3%~10% nano-Mo2C spheres, with the balance being Mg. 100-a-b Ni a RE b Matrix alloy.

9. A magnesium-based hydrogen storage material with multi-center relay catalysis, characterized in that, It is obtained by the preparation method of a magnesium-based hydrogen storage material with multi-center relay catalysis as described in any one of claims 1 to 8.

10. A magnesium-based hydrogen storage material with multi-center relay catalysis according to claim 9, characterized in that, The magnesium-based hydrogen storage material with multi-center relay catalysis was heated at a rate of 3 °C·min. -1 Under argon conditions, the initial hydrogen release temperature is 150℃~170℃; and the reversible hydrogen absorption capacity of the magnesium-based hydrogen storage material with multi-center relay catalysis is not less than 5.5wt. under the conditions of hydrogen absorption pressure of 4MPa, hydrogen absorption temperature of 250℃ and hydrogen absorption time of 60min.