A method for preparing nano-transition metal nitride powder by molten salt-assisted gas-phase combustion synthesis
By using a molten salt-assisted gas-phase combustion synthesis method, transition metal chlorides, ionic nitrides, and alkali metal halides as raw materials, a highly active gas-phase reaction system is constructed. This solves the problems of incomplete reaction and difficulty in controlling particle size in traditional methods, and realizes the efficient preparation and large-scale production of high-purity nano-transition metal nitride powders.
Patent Information
- Application Number
- CN202611237148.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-14
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies make it difficult to achieve efficient preparation of high-purity nano-transition metal nitride powders. Traditional methods suffer from problems such as incomplete reaction, difficulty in controlling particle size, and easy agglomeration.
A molten salt-assisted gas-phase combustion synthesis method was adopted, using transition metal chlorides, ionic nitrides and alkali metal halides as raw materials to prepare nano-transition metal nitride powders through combustion synthesis. A highly active gas-phase reaction system was constructed, and molten salt was used as a dispersant and heat regulation medium to achieve rapid and uniform reaction.
This method enables efficient and controllable preparation of nano-transition metal nitride powders with high product purity and adjustable particle size, avoiding the high energy consumption and environmental pollution problems of traditional methods, and has the potential for green and large-scale production.
Smart Images

Figure CN123105564A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of inorganic nanomaterial preparation technology, specifically relating to a method for preparing nano-transition metal nitride powder by molten salt-assisted gas-phase combustion synthesis. Background Technology
[0002] Transition metal nitrides (such as TiN, ZrN, CrN, WN, VN, and HfN) possess high melting points, high hardness, high wear resistance, and excellent oxidation and corrosion resistance, while also exhibiting good electrical conductivity and thermal stability. They represent a class of advanced ceramic materials with immense development potential. They have irreplaceable application value in aerospace thermal protection coatings, high-speed cutting tools, microelectronic devices, optoelectronic functional materials, and components used in extreme environments. In particular, nanoscale transition metal nitride powders, due to their high specific surface area, high defect concentration, and high sintering activity, can significantly enhance the densification process and interface control capabilities, making them crucial strategic foundation materials for the preparation of high-performance hard materials, nanocomposite ceramics, and advanced functional devices.
[0003] Currently, the main methods for preparing nano-transition metal nitride powders include physical vapor deposition (PVD), chemical vapor deposition (CVD), mechanical alloying, sol-gel method, thermal reduction nitriding, and combustion synthesis. Among these, PVD and CVD can prepare high-purity, nanoscale nitride powders or films, but they require sophisticated equipment, involve complex processes, and have low production efficiency, making large-scale powder preparation difficult. Mechanical alloying offers advantages such as simple processes and wide applicability, but suffers from high energy consumption, easy introduction of impurities into the powder, uneven particle size distribution, and severe agglomeration. The sol-gel method offers advantages such as uniform molecular-scale mixing and lower reaction temperatures, but typically requires complex precursor preparation processes, resulting in high organic reagent costs, low yields, and complex post-processing. Traditional thermal reduction nitriding, while using widely available raw materials and simple equipment, usually requires high reaction temperatures and long holding times, leading to high energy consumption and a tendency for grain coarsening and powder sintering agglomeration.
[0004] In comparison, combustion synthesis utilizes the large amount of chemical energy released within the reaction system to achieve a self-propagating high-temperature reaction, offering significant advantages such as fast reaction rate, low energy consumption, simple process flow, high product purity, and ease of large-scale production. Due to the extremely high instantaneous temperature gradient and rapid cooling conditions during combustion synthesis, grain growth can be effectively suppressed, providing favorable thermodynamic conditions for the formation of nanoscale transition metal nitride powders. Simultaneously, this method can precisely control the product composition, particle size, and microstructure by adjusting the reactant composition, nitrogen source type, and reaction atmosphere, making it a highly promising technical approach for preparing high-performance nanoscale transition metal nitride powders. However, the combustion synthesis process of nanoscale transition metal nitrides still faces certain challenges. Since the formation of transition metal nitrides involves complex processes such as metal element diffusion, nitridation reactions, and rapid crystal nucleation, high requirements are placed on the purity, particle size, activity of the metal powder, and the reactivity of the nitrogen source. Traditional reaction systems using metal powder and nitrogen as raw materials suffer from insufficient reactivity, incomplete nitridation, and difficulty in controlling product particle size, making it difficult to meet the requirements for preparing high-purity nanoscale transition metal nitride powders. Therefore, developing novel combustion synthesis systems with high activity, high dispersibility, and controllable reaction characteristics is key to achieving efficient preparation of high-purity nano-transition metal nitride powders.
[0005] Therefore, it is urgent to develop a novel synthesis method for preparing nanoscale transition metal nitride powders by leveraging the deep synergy between highly reactive gaseous raw materials (high reactivity and easy diffusion) and combustion synthesis processes (rapid reaction, low energy consumption, and high efficiency) to overcome the bottlenecks in traditional solid-solid reaction processes, such as limited element diffusion, high reaction temperature, low nitridation degree, and easy product agglomeration. This method aims to solve the key powder material preparation problems in high-end equipment, advanced manufacturing, and extreme environment applications. Summary of the Invention
[0006] To overcome the shortcomings of existing technologies, this invention provides a method for preparing nano-sized transition metal nitride powders through molten salt-assisted gas-phase combustion synthesis. This method uses transition metal chlorides as the metal source, ionic nitride powders as the nitrogen source, and alkali metal halides as the dispersant. Nano-sized transition metal nitride powders are prepared through combustion synthesis, solving problems such as incomplete metal nitridation, uneven reaction, and difficulty in controlling coarse particle size in traditional methods.
[0007] To achieve the above objectives, the present invention adopts the following technical solution:
[0008] A method for preparing nano-transition metal nitride powder by molten salt-assisted gas-phase combustion synthesis includes the following steps:
[0009] S1. Raw material pretreatment: Alkali metal halide powder, transition metal chloride powder and ionic nitride powder are vacuum dried to remove surface-adsorbed water and impurities.
[0010] Optionally, the transition metal chloride powder is selected from at least one of zirconium tetrachloride, chromium trichloride, hafnium tetrachloride, and tungsten hexachloride. Transition metal chlorides are volatile upon heating and rapidly sublimate under high combustion temperatures, forming gaseous active species. Due to their high chemical activity, low melting point, and high volatility, transition metal chlorides can form liquid or gaseous active intermediates during combustion, accelerating metal migration and promoting metal-nitrogen bond formation. Simultaneously, chloride ions combine with cations in ionic nitrides to form molten salts, providing a liquid-phase mass transfer environment for the reaction, enhancing particle wetting and interfacial diffusion, thereby lowering the activation energy and increasing the combustion reaction rate. Therefore, transition metal chlorides play a dual role as both metal precursors and reaction regulating media in the combustion synthesis system.
[0011] Optionally, the alkali metal halide powder is selected from at least one of sodium chloride, potassium chloride, calcium chloride, sodium fluoride, calcium fluoride, and sodium bromide. The main function of the alkali metal halide is to act as a cooling and liquid-phase dispersant by utilizing its high melting point and endothermic melting at high temperatures; the cations in the halide do not participate in the reaction. Sodium chloride is a preferred alkali metal halide because it is not easily hygroscopic, its melting point is close to the product formation temperature, and the molten salt has a low viscosity after melting.
[0012] Optionally, the ionic nitride powder is selected from at least one of barium nitride, strontium nitride, calcium nitride, magnesium nitride, and europium nitride. Ionic nitrides are highly reactive, easily hydrolyzed, and can decompose into a gaseous nitrogen source at high temperatures. The cations of the ionic nitride enter the product to form chloride inorganic salts, which are soluble in water and can be removed by washing. Strontium nitride is a preferred ionic nitride because it has a high exothermic reaction and is less hygroscopic than barium nitride.
[0013] Optionally, the drying conditions are: drying in a vacuum oven at 40-150℃ for 1-12 hours, with a vacuum degree ≤-0.1Mpa.
[0014] Optionally, before vacuum drying, the alkali metal halide powder is crushed using a ball mill. The ball milling method can be one of a planetary ball mill, a vibratory ball mill, or a rolling ball mill. The ball mill speed is 200-1000 r / min, the time is 5-60 min, and the grinding balls used are one of zirconium oxide, tungsten carbide, or silicon nitride grinding balls, with a ball-to-material mass ratio of 1:1-10:1.
[0015] S2. Preparation of mixed powder: Under vacuum or inert gas protection, the pretreated raw materials obtained in S1 are ball-milled and mixed to obtain uniformly mixed powder raw materials.
[0016] Optionally, the molar ratio of the ionic nitride to the transition metal chloride is 1:0.5-1:5; the molar ratio of the ionic nitride to the alkali metal halide is 1:2-1:10. The required stoichiometric ratio of the ionic nitride to the transition metal chloride varies depending on the reactants. For example, according to the chemical reaction equation, the most suitable ratio of Sr3N2 to ZrCl4 is 1:1.5, and the most suitable ratio of Sr3N2 to CrCl3 is 1:2. The ratio of the ionic nitride to the alkali metal halide is based on experimental experience; when the molar ratio of the ionic nitride to the alkali metal halide exceeds 1:10, the combustion synthesis reaction is difficult to complete.
[0017] Optionally, the ball milling method is selected from one of planetary ball mills, vibratory ball mills, and rolling ball mills. The ball mill speed is 100-500 r / min, the time is 4-24 h, and the grinding balls are selected from one of zirconium oxide, tungsten carbide, and silicon nitride grinding balls, with a ball-to-material mass ratio of 2:1-10:1. Preferably, the pretreated raw material obtained in S1 is placed in a ball mill jar protected by vacuum or inert gas under the inert atmosphere of a glove box, and then placed in the ball mill for ball milling and mixing. The glove box environment is an argon atmosphere with a water content of <0.1 ppm and an oxygen content of <0.1 ppm.
[0018] S3. Combustion Synthesis: The mixed powder raw materials obtained in S2 are placed into a combustion synthesis reaction device, vacuumed and filled with inert gas, and the igniter is ignited by electricity to initiate a rapid combustion synthesis reaction; after the reaction is completed, a block product is obtained, which is then ground and washed with water to obtain the nano-transition metal nitride powder.
[0019] Optionally, the raw material for the combustion synthesis reaction is the mixed powder obtained in step S2, and the inert gas is high-purity nitrogen or argon or a mixture of both, with an inert gas filling pressure of 0.2-6 MPa; the grinding is carried out in an agate mortar.
[0020] Optionally, the igniter is a titanium-carbon mixed powder, with a mass ratio of elemental titanium to elemental carbon of 4:1, and the amount of igniter is 0.5-1 wt% of the reaction raw materials.
[0021] Optionally, in the water washing step, a magnetic stirrer is used to thoroughly mix water and powder, with a water-to-powder mass ratio of 20:1-50:1, a rotation speed of 200-500 r / min, and a time of 4-10 h.
[0022] The present invention also provides nano-transition metal nitride powder synthesized by the method, wherein the transition metal nitride powder has good dispersibility and the particle size can be continuously controlled in the range of 40-300 nm.
[0023] Compared with the prior art, the present invention has the following significant advantages:
[0024] 1. Constructing a highly reactive gas-phase precursor combustion synthesis system for the efficient preparation of transition metal nitrides: Traditional transition metal nitride combustion synthesis typically involves the direct reaction of transition metal powder with nitrogen, a typical solid-gas reaction mode. This mode suffers from problems such as low nitrogen diffusion rate, difficulty in activating the N-N triple bond, limited reaction interface, and the surface nitride layer hindering further reaction, leading to incomplete reaction, coarse product particle size, and residual impurities. To address these shortcomings, this invention proposes a molten salt-assisted gas-phase combustion synthesis method. Using ionic nitrides and transition metal chlorides with high-temperature volatility as precursors, a highly reactive gas-phase reaction system is constructed in an alkali metal halide molten salt environment. The combustion reaction time is only a few seconds to tens of seconds. During combustion, the precursors rapidly vaporize and form uniformly distributed reactive species, achieving sufficient contact of reactant elements on a spatial scale. This fundamentally overcomes the problem of limited mass transfer in traditional solid-gas reactions, improving reaction efficiency and element utilization.
[0025] Taking zirconium tetrachloride as the transition metal chloride powder, sodium chloride as the alkali metal halide powder, and strontium nitride as the ionic nitride powder as an example, the combustion reaction formula is:
[0026] 4Sr3N2+6ZrCl4=12SrCl2+6ZrN+N2(g)
[0027] In the molten salt-assisted gas-phase combustion synthesis process, Sr3N2 and ZrCl4 are used as reaction precursors, and NaCl is used as an inert molten salt diluent. When the system is ignited by an external heat source, a rapid exothermic reaction occurs between Sr3N2 and ZrCl4, releasing a large amount of heat and causing the temperature of the reaction zone to rise rapidly. Therefore, no further heating is required after the reaction begins, and the reaction can be sustained by its own exothermic reaction. Due to the high volatility of ZrCl4, it rapidly sublimates under the high-temperature combustion environment to form gaseous ZrCl4. x Active nitrogen species are generated during the reaction. Simultaneously, Sr3N2 decomposes and vaporizes at high temperatures, releasing active nitrogen species. Gaseous Zr species collide and react rapidly with these active nitrogen species at the reaction front, generating ZrN crystal nuclei, while simultaneously forming SrCl2 as a byproduct and a small amount of N2 gas. Alkali metal halides are not consumed and do not participate in the reaction. During the reaction, the NaCl molten salt first acts as a heat regulation medium, absorbing some of the heat released during combustion, lowering the local combustion temperature, and slowing down the rapid particle growth caused by intense exothermic reactions. Simultaneously, as the temperature rises, NaCl melts, forming a continuous liquid phase environment that coats and isolates the reactants and the generated ZrN crystal nuclei, separating the newly formed ZrN particles from each other and reducing the probability of direct particle contact and sintering. The molten salt liquid phase also provides certain ion migration channels, improving the uniformity of reactant dispersion, allowing ZrN crystal nuclei to form and grow in a more uniform environment.
[0028] 2. Based on a rapid gas-phase reaction mechanism, this method achieves full nitridation of metal precursors and homogeneous nucleation of transition metal nitrides: The combustion synthesis process features instantaneous high temperature and self-sustaining propagation, which promotes the rapid conversion of ionic nitrides and transition metal chlorides at the reaction front into metal-chlorine reactive species and nitrogen-containing gaseous components. This transforms the nitride formation process from a traditional solid-phase interfacial reaction to a homogeneous gas-phase reaction. This reaction mode significantly improves the reaction kinetic rate, promotes rapid nucleation of transition metal nitrides, and reduces unreacted metal residues. Simultaneously, the gas-phase reaction avoids the formation of a dense nitride layer during traditional nitridation, which is beneficial for obtaining uniformly composed, high-purity transition metal nitride powders.
[0029] 3. Synergistic Regulation of Molten Salt Confinement and In-situ Isolation of Byproducts for Controllable Nanoparticle Preparation: This invention introduces alkali metal halide molten salt as a dilution and confinement medium, forming a liquid-phase environment at high temperatures. This regulates the heat release process of the combustion reaction, reduces local overheating, and weakens the driving force for grain growth. Simultaneously, the molten salt liquid phase can coat and spatially isolate the generated nitride particles, limiting particle migration, collision, and sintering. Furthermore, the strontium chloride byproduct generated in the reaction is uniformly distributed among the product particles, further enhancing the in-situ isolation effect and jointly inhibiting particle aggregation and abnormal growth. Therefore, this method can effectively regulate the size and dispersion state of transition metal nitride particles.
[0030] 4. High product purity and simple post-processing, with potential for green and large-scale preparation: The combustion products of this system mainly consist of halides and transition metal nitrides. The generated halides have good water solubility, and by-products can be removed by simple water washing, avoiding the environmental pollution and equipment corrosion problems caused by traditional acid washing processes. The obtained transition metal nitride particles have good dispersibility and uniform particle size, without obvious agglomeration. Meanwhile, the combustion synthesis process relies on its own exothermic reaction to sustain the reaction, eliminating the need for prolonged external heating, and offering advantages such as short reaction cycle, low energy consumption, and simple equipment. The alkali metal halide molten salts used are widely available, inexpensive, and recyclable. Therefore, this technology provides a new technical route for the green, efficient, and large-scale preparation of high-purity nano-transition metal nitride powders. Attached Figure Description
[0031] To more clearly illustrate the technical solutions in the embodiments of the present invention, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0032] Figure 1 This is a schematic diagram of the process for preparing nano-transition metal nitride powders by molten salt-assisted gas-phase combustion synthesis provided by the present invention.
[0033] Figure 2 The images show SEM morphology of zirconium nitride powder synthesized by combustion using strontium nitride, zirconium tetrachloride, and sodium chloride in different molar ratios in Example 1 of this invention. The molar ratios of strontium nitride, zirconium tetrachloride, and sodium chloride are (A) 1:1.5:3, (B) 1:1.5:5, (C) 1:1.5:7, and (D) 1:1.5:9.
[0034] Figure 3 The image shows the XRD pattern of zirconium nitride powder obtained in Example 1 of this invention with a molar ratio of strontium nitride, zirconium tetrachloride, and sodium chloride of 1:1.5:5.
[0035] Figure 4 The image shows the morphology of the chromium nitride powder obtained in Example 2 of the present invention, where (A) is a SEM image and (B) is a TEM image.
[0036] Figure 5 The image shows the XRD pattern of the chromium nitride powder obtained in Example 2 of this invention. Detailed Implementation
[0037] To make the technical problems, technical solutions and advantages of the present invention clearer, a detailed description will be given below in conjunction with the accompanying drawings and specific embodiments.
[0038] Figure 1 This invention provides a schematic flowchart for the preparation of nano-transition metal nitride powders via molten salt-assisted gas-phase combustion synthesis. The method includes the following steps: First, alkali metal halide powder (i.e., molten salt), transition metal chloride powder (i.e., transition metal precursor), and ionic nitride powder (i.e., highly active nitrogen source) are vacuum dried separately, then ball-milled to obtain a uniformly mixed powder raw material. The obtained mixed powder raw material is placed in a combustion synthesis reaction apparatus, evacuated, and filled with inert gas. An igniter is then applied to initiate the combustion synthesis reaction. During the reaction, the transition metal chloride powder decomposes to obtain highly active transition metal atoms, the alkali metal halide powder melts and acts as a reaction medium, and the ionic nitride powder decomposes to form highly active nitrogen atoms, which combine with the aforementioned transition metal atoms to obtain transition metal nitrides.
[0039] Example 1
[0040] 1. Place zirconium oxide grinding balls and sodium chloride powder (mass ratio 2:1) into a vibrating ball mill jar. Use a vibrating ball mill to refine the sodium chloride powder at a speed of 1000 r / min for 20 min. Place the crushed sodium chloride powder, zirconium tetrachloride powder, and strontium nitride powder into a vacuum oven for vacuum drying. The drying conditions are: temperature 120℃, drying time 10 h, and vacuum degree -0.1 MPa.
[0041] 2. Under the protection of an inert atmosphere (argon atmosphere, water content <0.1ppm, oxygen content <0.1ppm) in a glove box, the pretreated raw materials are weighed according to the molar ratios of strontium nitride, zirconium tetrachloride, and sodium chloride as follows: (A) 1:1.5:3, (B) 1:1.5:5, (C) 1:1.5:7, (D) 1:1.5:9. Among them, (A) 29.1g of strontium nitride, 34.9g of zirconium tetrachloride, and 17.5g of sodium chloride; (B) 29.1g of strontium nitride, 34.9g of zirconium tetrachloride, and 29.2g of sodium chloride; (C) 29.1g of strontium nitride, 34.9g of zirconium tetrachloride, and 40.9g of sodium chloride; (D) 29.1g of strontium nitride, 34.9g of zirconium tetrachloride, and 52.6g of sodium chloride. The weighed raw materials and zirconia grinding balls were placed into a vacuum ball mill jar at a ball-to-material mass ratio of 5:1. The powder was then mixed using a vertical planetary ball mill at a speed of 300 r / min for 8 hours.
[0042] 3. The uniformly mixed powders were placed into a combustion synthesis reaction apparatus. After evacuation, 2 MPa of high-purity argon gas was introduced, and 1 g of igniter was ignited to initiate the combustion synthesis reaction. The igniter was a titanium-carbon mixed powder with a mass ratio of elemental titanium to elemental carbon of 4:1. After the reaction, a blocky product was obtained. The blocky product was ground and crushed in an agate mortar. The ground powder and water were weighed at a mass ratio of 20:1 and placed in a magnetic stirrer container for washing. The rotor speed was 300 r / min for 5 h to obtain the nano-zirconium nitride powder.
[0043] Figure 2 The SEM images show the morphology of zirconium nitride powder synthesized by combustion using strontium nitride, zirconium tetrachloride, and sodium chloride in different molar ratios. The molar ratios of strontium nitride, zirconium tetrachloride, and sodium chloride are (A) 1:1.5:3, (B) 1:1.5:5, (C) 1:1.5:7, and (D) 1:1.5:9. The images show that when the molar ratio of sodium chloride to strontium nitride is 3:1, the resulting particle size is approximately 150–300 nm; when the molar ratio increases to 5:1, the particle size further decreases to 100–200 nm; further increasing to 7:1, the particle size decreases to 60–100 nm; and when the molar ratio reaches 9:1, ultrafine ZrN nanoparticles with a size of only 40–60 nm can be obtained, exhibiting good dispersion and no obvious agglomeration. Therefore, this invention limits the molar ratio of ionic nitride to alkali metal halide to 1:2–1:10. Within the aforementioned range, the greater the amount of alkali metal halide as molten salt, the greater the heat required for melting, leading to a decrease in the system reaction temperature, which is conducive to the formation of fine particles; on the other hand, the large amount of liquid medium after melting acts as a dispersant, making the reaction products less prone to agglomeration.
[0044] Figure 3 The image shows the XRD pattern of zirconium nitride powder synthesized by combustion when the molar ratio of strontium nitride, zirconium tetrachloride, and sodium chloride is 1:1.5:5. This indicates that the product phase has high purity, and the characteristic peaks are consistent with the standard peak shape of ZrN.
[0045] Example 2
[0046] 1. Place zirconium oxide grinding balls and sodium chloride powder (mass ratio 2:1) into a vibrating ball mill jar. Use a vibrating ball mill to refine the sodium chloride powder at a speed of 1000 r / min for 20 min. Place the crushed sodium chloride powder, chromium trichloride powder, and strontium nitride powder into a vacuum oven for vacuum drying. The drying conditions are: temperature 120℃, drying time 10 h, and vacuum degree -0.1 MPa.
[0047] 2. Under an inert atmosphere (argon atmosphere, water content <0.1ppm, oxygen content <0.1ppm) in a glove box, weigh the pretreated raw materials according to the molar ratio of strontium nitride, chromium trichloride, and sodium chloride of 1:2:5, wherein 29.1g of strontium nitride, 31.7g of chromium trichloride, and 29.2g of sodium chloride are added. Place the weighed raw materials and zirconia grinding balls into a vacuum ball mill jar at a ball-to-material mass ratio of 5:1. Mix the powder using a vertical planetary ball mill at a speed of 300 rpm for 8 hours.
[0048] 3. The uniformly mixed powders were placed into a combustion synthesis reaction apparatus. After evacuation, 2 MPa of high-purity argon gas was introduced, and 1 g of igniter was ignited to initiate the combustion synthesis reaction. The igniter was a titanium-carbon mixed powder with a mass ratio of elemental titanium to elemental carbon of 4:1. After the reaction, a blocky product was obtained. The blocky product was ground and crushed in an agate mortar. The ground powder and water were weighed at a mass ratio of 20:1 and placed into a magnetic stirrer container for washing. The rotor speed was 300 r / min for 5 h to obtain the nano-chromium nitride powder.
[0049] Figure 4The images show the morphology of chromium nitride powder synthesized by combustion of strontium nitride, chromium trichloride, and sodium chloride in a molar ratio of 1:2:5. (A) is a SEM image, and (B) is a TEM image. Observation reveals that the obtained chromium nitride mainly exhibits a plate-like morphology with a particle size of approximately 100-200 nm. This indicates that the chromium nitride crystal growth during gas-phase combustion synthesis exhibits significant anisotropic characteristics. Due to the high reactivity and large atomic migration rate of the gas-phase reaction, after rapid nucleation, differences in surface energy and growth rate exist between different crystal planes, causing the crystal to preferentially grow along specific crystal orientations, ultimately forming a two-dimensional plate-like structure. Furthermore, the liquid phase environment provided by the NaCl molten salt can reduce interfacial energy and promote mass migration, creating conditions for the directional growth of crystals along low-energy crystal planes, thereby further enhancing the anisotropic growth behavior of chromium nitride crystals.
[0050] Figure 5 The XRD pattern of the chromium nitride powder obtained by combustion synthesis is shown. XRD results indicate that the obtained chromium nitride product has relatively low crystallinity, with significant broadening of diffraction peaks. This suggests that the grain size / lamella thickness is small during combustion synthesis. Furthermore, due to the extremely short reaction time, the system is in a rapid non-equilibrium solidification state, preventing sufficient crystal growth and resulting in a chromium nitride product with relatively poor crystallinity. This non-equilibrium environment created by the rapid combustion reaction is a key characteristic that distinguishes combustion synthesis from traditional long-time sintering methods, and is also an important basis for obtaining metastable structures and unique morphologies.
[0051] This invention utilizes highly reactive raw materials that can decompose into gaseous intermediates to initiate a gas-phase reaction mechanism at high temperatures, achieving the preparation of well-dispersible and size-controllable nano-transition metal nitride powders. The raw materials used in this invention are widely available, the preparation process is simple and environmentally friendly, making it suitable for the large-scale preparation of nano-transition metal nitride powders.
[0052] The above description is merely a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention should be included within the scope of protection of the present invention. Therefore, the scope of protection of the present invention should be determined by the scope of the claims.
Claims
1. A method for preparing nano-transition metal nitride powder by molten salt-assisted gas-phase combustion synthesis, characterized in that, Includes the following steps: S1. The alkali metal halide powder, transition metal chloride powder, and ionic nitride powder are vacuum dried separately. S2. Under vacuum or inert gas protection, the pretreated raw material obtained in S1 is ball-milled and mixed to obtain a uniformly mixed powder raw material. S3. The mixed powder raw material obtained in S2 is placed into a combustion synthesis reaction device, vacuumed and filled with inert gas, and the igniter is ignited by electricity to initiate the combustion synthesis reaction; after the reaction is completed, a block product is obtained, which is then ground and washed with water to obtain the nano-transition metal nitride powder.
2. The method for preparing nano-transition metal nitride powder by molten salt-assisted gas-phase combustion synthesis according to claim 1, characterized in that, In step S1, the transition metal chloride powder is selected from at least one of zirconium tetrachloride, chromium trichloride, hafnium tetrachloride, and tungsten hexachloride; And / or, the alkali metal halide powder is selected from at least one of sodium chloride, potassium chloride, calcium chloride, sodium fluoride, calcium fluoride, and sodium bromide; And / or, the ionic nitride powder is selected from at least one of barium nitride, strontium nitride, calcium nitride, magnesium nitride, and europium nitride.
3. The method for preparing nano-transition metal nitride powder by molten salt-assisted gas-phase combustion synthesis according to claim 1, characterized in that, In step S1, the drying conditions are: drying in a vacuum oven at 40-150℃ for 1-12 hours, with a vacuum degree ≤-0.1Mpa.
4. The method for preparing nano-transition metal nitride powder by molten salt-assisted gas-phase combustion synthesis according to claim 3, characterized in that, In step S1, before vacuum drying, the alkali metal halide powder is crushed using a ball mill.
5. The method for preparing nano-transition metal nitride powder by molten salt-assisted gas-phase combustion synthesis according to claim 4, characterized in that, In step S1, the ball milling method is selected from one of planetary ball mill, vibratory ball mill, and rolling ball mill. The ball mill speed is 200-1000 r / min, the time is 5-60 min, and the grinding balls are one of zirconium oxide, tungsten carbide, and silicon nitride grinding balls. The ball-to-material mass ratio is 1:1-10:
1.
6. The method for preparing nano-transition metal nitride powder by molten salt-assisted gas-phase combustion synthesis according to claim 1, characterized in that, In step S2, the molar ratio of the ionic nitride to the transition metal chloride is 1:0.5-1:5; the molar ratio of the ionic nitride to the alkali metal halide is 1:2-1:
10.
7. The method for preparing nano-transition metal nitride powder by molten salt-assisted gas-phase combustion synthesis according to claim 1, characterized in that, In step S2, the ball milling method is selected from one of planetary ball mill, vibratory ball mill, and rolling ball mill. The ball mill speed is 100-500 r / min, the time is 4-24 h, and the grinding balls are one of zirconium oxide, tungsten carbide, and silicon nitride grinding balls. The ball-to-material mass ratio is 2:1-10:
1. And / or, the pretreated raw material obtained in S1 is placed in a ball mill jar protected by vacuum or inert gas under the inert atmosphere of a glove box, and then placed in a ball mill for ball milling and mixing. The glove box environment is an argon atmosphere with a water content of <0.1ppm and an oxygen content of <0.1ppm.
8. The method for preparing nano-transition metal nitride powder by molten salt-assisted gas-phase combustion synthesis according to claim 1, characterized in that, In step S3, the inert gas is high-purity nitrogen or argon or a mixture of both, and the inert gas filling pressure is 0.2-6 MPa; the grinding is carried out in an agate mortar. And / or, the igniter is a titanium-carbon mixed powder, with a mass ratio of elemental titanium to elemental carbon of 4:1, and the amount of igniter used is 0.5-1 wt% of the reactants; And / or, in the water washing step, a magnetic stirrer is used to thoroughly mix water and powder, with a water to powder mass ratio of 20:1-50:1, a rotation speed of 200-500 r / min, and a time of 4-10 h.
9. Nanoscale transition metal nitride powder synthesized by the method according to any one of claims 1 to 8.
10. The nano-transition metal nitride powder according to claim 9, characterized in that, The powder has good dispersibility, and the particle size can be continuously adjusted within the range of 40-300nm.