A method for recovering phosphoric acid from phosphate slag using membrane separation technology
Phosphoric acid can be recovered from phosphate slag using membrane separation technology, which solves the problem of low resource utilization rate of phosphate slag and realizes efficient recovery and low-cost production of high-purity phosphoric acid, making it suitable for industrial applications.
Patent Information
- Application Number
- CN202611560067.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-09
- Publication Date
- 2026-11-17
AI Technical Summary
In existing technologies, the phosphorus slag produced after lithium extraction from lithium iron phosphate batteries has a low resource utilization rate, low phosphorus recovery rate, low product purity, complex process and high cost. Traditional phosphate rock preparation of phosphoric acid has problems of resource depletion and pollution.
Phosphoric acid is recovered from phosphate iron slag using membrane separation technology combined with acid leaching. The process includes crushing, sieving, acid leaching, microfiltration, nanofiltration, reverse osmosis, and vacuum distillation. Through gradient membrane separation and refining processes, phosphoric acid is efficiently recovered and purified.
It achieves high-purity recovery of phosphoric acid (≥85%) and high phosphorus recovery rate (≥90%), simplifies the process, reduces costs and energy consumption, is suitable for large-scale production, and is environmentally friendly.
Abstract
Description
Technical Field
[0001] This invention relates to the field of industrial solid waste resource utilization technology, and in particular to a method for recovering phosphoric acid from phosphoric acid slag using membrane separation technology. Background Technology
[0002] With the rapid development of the new energy vehicle industry, the demand for lithium iron phosphate batteries has increased significantly, leading to a growing problem of recycling and disposing of used lithium iron phosphate batteries. Currently, the lithium extraction process from used lithium iron phosphate batteries is relatively mature, but it generates a large amount of waste phosphorus-iron slag. This slag contains phosphorus, iron, and other elements; if discarded directly, it not only wastes resources but also causes environmental problems such as soil and water pollution due to phosphorus loss.
[0003] In existing technologies, the main methods for treating waste phosphate slag from lithium iron phosphate extraction are stockpiling or landfilling, resulting in extremely low resource utilization rates. Some studies have attempted to recycle phosphate slag, such as extracting iron to prepare iron-based products, but research on the efficient recovery and utilization of phosphorus is limited. Phosphoric acid, widely used in fertilizers, food, pharmaceuticals, electronics, and other fields, has a large market demand. If phosphorus can be efficiently recovered from phosphate slag and used to produce phosphoric acid, it would not only solve the environmental disposal problem of phosphate slag but also achieve phosphorus resource recycling, yielding significant economic and social benefits. Traditional phosphoric acid production methods mainly use phosphate rock as raw material, employing wet or thermal processes. However, phosphate rock is a non-renewable resource, and long-term mining will lead to resource depletion. Furthermore, traditional processes suffer from high energy consumption and significant pollution. Therefore, developing a method for preparing phosphoric acid from industrial solid waste phosphate slag as a raw material, replacing traditional phosphate rock, is of great significance for resource recycling and environmental protection.
[0004] Existing technologies for preparing phosphoric acid from solid waste often suffer from drawbacks such as low phosphorus recovery rates, low product purity, complex processes, and high costs. For example, some processes use strong acid leaching followed by direct crystallization to prepare phosphoric acid, but the presence of numerous impurity ions in the leachate leads to low product purity. Other processes employ multi-stage precipitation for impurity removal, resulting in lengthy processes, high reagent consumption, and increased production costs. Therefore, there is an urgent need to develop a simple, high-efficiency, high-purity, and low-cost method for preparing phosphoric acid from iron phosphate slag. Summary of the Invention
[0005] The purpose of this invention is to provide a method for recovering phosphoric acid from phosphate iron slag using membrane separation technology. This method has a high phosphorus recovery rate and high product purity, and can realize the efficient resource utilization of phosphate iron slag.
[0006] To achieve the above-mentioned objectives, the present invention provides the following technical solution: This invention provides a method for recovering phosphoric acid from ferrophosphate slag using membrane separation technology, comprising the following steps: The waste phosphorus iron slag from lithium iron phosphate extraction is crushed and sieved sequentially to obtain phosphorus iron slag powder. The phosphorus iron slag powder is mixed with an acidic solution and subjected to acid leaching treatment. After solid-liquid separation, acid leaching solution and acid leaching residue are obtained. The acid leaching solution was sequentially filtered through a microfiltration membrane, separated by a nanofiltration membrane, and concentrated by a reverse osmosis membrane to obtain a concentrated phosphoric acid solution. The concentrated phosphoric acid solution was subjected to vacuum distillation, and the fraction was collected to obtain phosphoric acid.
[0007] Preferably, the particle size of the phosphorus iron slag powder is 100-200 mesh.
[0008] Preferably, the acidic solution includes a sulfuric acid solution or a hydrochloric acid solution.
[0009] Preferably, the sulfuric acid solution has a mass fraction of 20-40%; the hydrochloric acid solution has a mass fraction of 15-30%.
[0010] Preferably, the mass ratio of the phosphorus iron slag powder to the volume of the acidic solution is 1 g:(3-8) mL.
[0011] Preferably, the acid leaching treatment is carried out under stirring conditions, with a stirring rate of 200-500 r / min; the temperature of the acid leaching treatment is 60-90℃, and the time is 2-6 h.
[0012] Preferably, the solid-liquid separation method includes pressure filtration or centrifugation; the pressure of the pressure filtration is 0.3-0.6 MPa, the speed of the centrifugation is 3000-5000 r / min, and the solid-liquid separation time is 15-60 min.
[0013] Preferably, the microfiltration membrane has a pore size of 0.1-1 μm and an operating pressure of 0.1-0.3 MPa, and the material of the microfiltration membrane includes polytetrafluoroethylene, polyvinylidene fluoride, or polypropylene. The nanofiltration membrane has a molecular weight cutoff of 200-800 Da and an operating pressure of 0.5-1.5 MPa. The material of the nanofiltration membrane includes polyamide, polyethersulfone, or composite polyamide. The reverse osmosis membrane operates at a pressure of 1.0-2.5 MPa and is made of aromatic polyamide composite membrane.
[0014] Preferably, the concentrated phosphoric acid solution has a phosphoric acid mass concentration of 45-65%, a total metal impurity content of ≤0.05%, and a solid impurity content of ≤0.01%.
[0015] Preferably, the vacuum degree of the reduced pressure distillation is 0.06-0.09 MPa, the temperature is 80-140℃, and the time is 2-4 hours.
[0016] The beneficial effects of this invention are: This invention employs an integrated acid leaching and gradient membrane separation process, combined with a refining step. First, the refined lithium iron phosphate (LiFePO4) waste iron phosphate slag powder is acid-leached to convert the phosphorus-containing components into phosphoric acid. Then, a specific membrane separation process sequentially removes suspended impurities and metal ions from the solution. Finally, high-purity phosphoric acid is obtained through vacuum distillation. This invention abandons traditional chemical precipitation, extraction, and high-temperature roasting processes for impurity removal. By optimizing acid leaching conditions and membrane separation parameters, it achieves simple and efficient separation of iron and phosphorus elements, with a phosphorus recovery rate exceeding 90%. The resulting phosphoric acid product has a purity ≥85%, meeting the requirements for industrial-grade phosphoric acid and realizing the resource utilization of solid waste. This method eliminates the need for large amounts of chemical impurity removal agents, has a simple process flow, and produces no secondary pollution, significantly reducing the cost and energy consumption of industrial production, making it suitable for large-scale production. This process is low-cost, simple, and environmentally friendly, possessing excellent prospects for industrial production. Detailed Implementation
[0017] This invention provides a method for recovering phosphoric acid from ferrophosphate slag using membrane separation technology, comprising the following steps: The waste phosphorus iron slag from lithium iron phosphate extraction is crushed and sieved sequentially to obtain phosphorus iron slag powder. The phosphorus iron slag powder is mixed with an acidic solution and subjected to acid leaching treatment. After solid-liquid separation, acid leaching solution and acid leaching residue are obtained. The acid leaching solution was sequentially filtered through a microfiltration membrane, separated by a nanofiltration membrane, and concentrated by a reverse osmosis membrane to obtain a concentrated phosphoric acid solution. The concentrated phosphoric acid solution was subjected to vacuum distillation, and the fraction was collected to obtain phosphoric acid.
[0018] The principle of this invention for recovering phosphoric acid is as follows: Phosphoric iron slag is mainly composed of a mixture of iron phosphate, carbon powder, etc. Under the action of acid solution, phosphorus element is converted into phosphate ions and enters the solution, that is, the following reaction occurs (taking sulfuric acid as an example): 2FePO4 + 3H2SO4 = Fe2(SO4)3 + 2H3PO4; then, suspended impurities and metal ions in the solution are removed sequentially by membrane separation technology, and then after concentration and purification, high-purity phosphoric acid product is obtained.
[0019] In this invention, unless otherwise specified, all raw materials required for preparation are commercially available products well known to those skilled in the art.
[0020] The present invention preferably uses an air jet mill to crush the waste phosphorus iron slag from lithium iron phosphate extraction, and then sieves it with a standard inspection sieve to ensure that the phosphorus iron slag powder has a uniform particle size, thus obtaining phosphorus iron slag powder.
[0021] In this invention, the phosphorus iron slag is preferably waste material obtained after lithium extraction from waste lithium iron phosphate battery materials.
[0022] In this invention, the particle size of the phosphorus iron slag powder is preferably 100-200 mesh, and more preferably 150-200 mesh; this particle size is beneficial to improving the efficiency of the subsequent acid leaching reaction.
[0023] The present invention preferably involves adding the above-mentioned phosphorus iron slag powder to a reaction vessel, then adding an acidic solution, and performing acid leaching under stirring conditions. After the reaction is completed, solid-liquid separation is performed to obtain acid leaching solution and acid leaching residue.
[0024] In this invention, the acidic solution preferably includes a sulfuric acid solution or a hydrochloric acid solution; the mass fraction of the sulfuric acid solution is preferably 20-40%, more preferably 30-40%; the mass fraction of the hydrochloric acid solution is preferably 15-30%, more preferably 20-30%; using an acid solution within this concentration range can ensure that the phosphorus element in the phosphorus-iron slag is fully leached out, while avoiding excessive acid leading to increased subsequent processing costs.
[0025] In this invention, the mass ratio of the phosphorus iron slag powder to the volume of the acidic solution is preferably 1 g:(3-8) mL, and more preferably 1 g:(5-8) mL.
[0026] In this invention, the stirring rate is preferably 200-500 r / min, more preferably 300-500 r / min; the acid leaching temperature is preferably 60-90℃, more preferably 70-90℃, and the time is preferably 2-6 h, more preferably 4-6 h.
[0027] In this invention, the solid-liquid separation method preferably includes pressure filtration or centrifugation to ensure thorough separation of the acid leaching solution and the acid leaching residue, and to reduce the impurity content in the acid leaching solution. The pressure filtration is preferably carried out using a plate and frame filter press, and the pressure of the pressure filtration is preferably 0.3-0.6 MPa, more preferably 0.5-0.6 MPa. The centrifugation is preferably carried out using a centrifuge, and the centrifugation speed is preferably 3000-5000 r / min, more preferably 4000-5000 r / min. The solid-liquid separation time is preferably 15-60 min, more preferably 20-45 min. Through solid-liquid separation, the solid phase and liquid phase in the acid leaching system can be completely separated, avoiding the impact of solid residue on subsequent membrane separation processes.
[0028] The present invention preferably filters the above-mentioned acid leaching solution through a microfiltration membrane, separates the microfiltration filtrate through a nanofiltration membrane, and then concentrates the nanofiltration filtrate through a reverse osmosis membrane to obtain concentrated phosphoric acid solution. Through the gradient coupling effect of microfiltration to remove suspended colloids, nanofiltration to remove metal ions, and reverse osmosis to precisely concentrate, various impurities in the acid leaching solution can be deeply removed, solving the pain points of incomplete impurity removal and low product purity in traditional processes, and significantly improving the purity of phosphoric acid products.
[0029] In this invention, the pore size of the microfiltration membrane is preferably 0.1-1 μm, more preferably 0.5-1 μm, and the working pressure is preferably 0.1-0.3 MPa, more preferably 0.2-0.3 MPa; the material of the microfiltration membrane preferably includes polytetrafluoroethylene, polyvinylidene fluoride, or polypropylene, more preferably polytetrafluoroethylene; microfiltration membrane filtration can completely remove fine suspended solid impurities in the acid leaching solution.
[0030] In this invention, the nanofiltration membrane preferably has a molecular weight cutoff of 200-800 Da, more preferably 500-800 Da, and a working pressure preferably of 0.5-1.5 MPa, more preferably 1.0-1.5 MPa; the nanofiltration membrane is preferably made of polyamide, polyethersulfone, or composite polyamide, more preferably composite polyamide; filtration through the nanofiltration membrane can effectively retain metal ion impurities and improve the purity of the phosphoric acid solution.
[0031] In this invention, the working pressure of the reverse osmosis membrane is preferably 1.0-2.5 MPa, more preferably 2.0-2.5 MPa; the material of the reverse osmosis membrane is preferably an aromatic polyamide composite membrane.
[0032] In this invention, the concentrated phosphoric acid solution preferably has a phosphoric acid mass concentration of 45-65%, more preferably 45-55%, a total metal impurity content preferably ≤0.05%, more preferably ≤0.03%, and a solid impurity content preferably ≤0.01%, more preferably ≤0.005%. After being treated by a three-stage membrane process of microfiltration, nanofiltration, and reverse osmosis, the obtained concentrated phosphoric acid solution meets the phosphoric acid refining pretreatment standard.
[0033] The present invention preferably places the above-mentioned concentrated phosphoric acid solution in a vacuum distillation apparatus for vacuum distillation, collects the fractions, and obtains phosphoric acid. Vacuum distillation can lower the boiling point of phosphoric acid, avoid the decomposition of phosphoric acid at high temperature, and further remove trace impurities and water in the solution, thereby improving the purity of the phosphoric acid product.
[0034] In this invention, the vacuum degree of the vacuum distillation is preferably 0.06-0.09 MPa, more preferably 0.08-0.09 MPa, the temperature is preferably 80-140℃, more preferably 120-140℃, and the time is preferably 2-4 h, more preferably 3-4 h.
[0035] The technical solutions provided by the present invention will be described in detail below with reference to the embodiments, but they should not be construed as limiting the scope of protection of the present invention.
[0036] The microfiltration membranes used in Examples 1-3 and Comparative Examples 1-2 were made of polytetrafluoroethylene, the nanofiltration membranes were made of composite polyamide, and the reverse osmosis membranes were made of aromatic polyamide composite membranes.
[0037] Example 1
[0038] The waste phosphorus slag from lithium iron phosphate extraction is crushed by air jet mill and then passed through 100 mesh and 200 mesh standard inspection sieves in sequence. The material under the 100 mesh sieve and over the 200 mesh sieve is collected to obtain phosphorus slag powder in the range of 100-200 mesh. The phosphorus iron slag powder was mixed with a 30% sulfuric acid solution at a solid-liquid ratio of 1 g: 5 mL and placed in a reaction vessel. The mixture was then subjected to acid leaching at 70℃ and 300 r / min for 4 h. After the reaction, a plate and frame filter press was used to separate the solid and liquid at 0.5 MPa for 45 min to obtain the acid leaching solution and acid leaching residue. The acid leaching solution was first filtered through a microfiltration membrane with a pore size of 0.5 μm at 0.2 MPa; then, the microfiltration filtrate was separated by passing it through a nanofiltration membrane with a molecular weight cutoff of 500 Da at 1.0 MPa; finally, the nanofiltration filtrate was concentrated by passing it through a low-pressure reverse osmosis membrane at 2.0 MPa to obtain a concentrated phosphoric acid solution with a phosphoric acid mass concentration of 45%, a total metal impurity content of 0.03%, and a solid impurity content of 0.005%. The concentrated phosphoric acid solution was placed in a vacuum distillation apparatus and distilled under reduced pressure at 140°C and 0.08 MPa for 3 h. The fraction was collected to obtain phosphoric acid.
[0039] The phosphoric acid product was found to have a purity of 98.6% and a phosphorus recovery rate of 92.3%.
[0040] Example 2
[0041] The waste phosphorus slag from lithium iron phosphate extraction is pulverized using an air jet mill, and then passed through 100-mesh and 200-mesh standard inspection sieves in sequence. The material below the 100-mesh sieve and above the 200-mesh sieve is collected to obtain phosphorus slag powder in the range of 100-200 mesh. The phosphorus iron slag powder was mixed with a 20% hydrochloric acid solution at a solid-liquid ratio of 1 g: 3 mL and placed in a reaction vessel. The mixture was then subjected to acid leaching at 60℃ and 200 r / min for 6 h. After the reaction, the solid and liquid were separated by centrifugation at 3000 r / min for 20 min to obtain the acid leaching solution and acid leaching residue. The acid leaching solution was first filtered through a microfiltration membrane with a pore size of 0.1 μm at 0.1 MPa; then, the microfiltration filtrate was separated by passing it through a nanofiltration membrane with a molecular weight cutoff of 200 Da at 0.5 MPa; finally, the nanofiltration filtrate was concentrated by passing it through a low-pressure reverse osmosis membrane at 1.0 MPa to obtain a concentrated phosphoric acid solution with a phosphoric acid mass concentration of 45%, a total metal impurity content of 0.05%, and a solid impurity content of 0.01%. The concentrated phosphoric acid solution was placed in a vacuum distillation apparatus and distilled under reduced pressure at 120°C and 0.06 MPa for 4 h. The fraction was collected to obtain phosphoric acid.
[0042] The phosphoric acid product was tested and found to have a purity of 97.5% and a phosphorus recovery rate of 93.5%.
[0043] Example 3
[0044] The waste phosphorus slag from lithium iron phosphate extraction is pulverized using an air jet mill, and then passed through 100-mesh and 200-mesh standard inspection sieves in sequence. The material below the 100-mesh sieve and above the 200-mesh sieve is collected to obtain phosphorus slag powder in the range of 100-200 mesh. The phosphorus iron slag powder was mixed with a 40% sulfuric acid solution at a solid-liquid ratio of 1 g: 8 mL and placed in a reaction vessel. The mixture was then subjected to acid leaching at 70℃ and 500 r / min for 2 h. After the reaction, a plate and frame filter press was used to separate the solid and liquid at 0.6 MPa for 30 min to obtain the acid leaching solution and acid leaching residue. The acid leaching solution was first filtered through a microfiltration membrane with a pore size of 1 μm at 0.3 MPa; then, the microfiltration filtrate was separated by passing it through a nanofiltration membrane with a molecular weight cutoff of 800 Da at 1.5 MPa; finally, the nanofiltration filtrate was concentrated by passing it through a low-pressure reverse osmosis membrane at 2.5 MPa to obtain a concentrated phosphoric acid solution with a phosphoric acid mass concentration of 55%, a total metal impurity content of 0.03%, and a solid impurity content of 0.005%. The concentrated phosphoric acid solution was placed in a vacuum distillation apparatus and distilled under reduced pressure at 120°C and 0.09 MPa for 2 h. The fraction was collected to obtain phosphoric acid.
[0045] The phosphoric acid product was found to have a purity of 99.3% and a phosphorus recovery rate of 91.1%.
[0046] Comparative Example 1
[0047] The only difference from Example 1 is: The nanofiltration membrane has a molecular weight cutoff of 1500 Da; The concentrated phosphoric acid solution has a phosphoric acid concentration of 40%, a total metal impurity content of 0.07%, and a solid impurity content of 0.015%. With all other parameters unchanged, phosphoric acid is obtained.
[0048] The phosphoric acid product was found to have a purity of 96.1% and a phosphorus recovery rate of 88%.
[0049] Comparative Example 2
[0050] The only difference from Example 1 is: The pore size of the microfiltration membrane is 3 μm; The concentrated phosphoric acid solution has a phosphoric acid concentration of 40%, a total metal impurity content of 0.1%, and a solid impurity content of 0.02%. With all other parameters unchanged, phosphoric acid is obtained.
[0051] The phosphoric acid product was found to have a purity of 95.0% and a phosphorus recovery rate of 88.3%.
[0052] As can be seen from the above embodiments and comparative examples, the present invention provides a method for recovering phosphoric acid from phosphorus iron slag using membrane separation technology. It adopts an integrated process of acid leaching and gradient membrane separation, combined with a refining step, to effectively separate phosphorus and iron elements in the phosphorus iron slag waste from lithium iron phosphate extraction. By optimizing the acid leaching conditions and membrane separation parameters, the purity of the phosphoric acid product is as high as 99.3%, and the phosphorus recovery rate is as high as 93.5%, which can meet the requirements for industrial-grade phosphoric acid and realize the resource utilization of solid waste.
[0053] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A method for recovering phosphoric acid from ferrophosphate slag using membrane separation technology, characterized in that, Includes the following steps: The waste phosphorus iron slag from lithium iron phosphate extraction is crushed and sieved sequentially to obtain phosphorus iron slag powder. The phosphorus iron slag powder is mixed with an acidic solution and subjected to acid leaching treatment. After solid-liquid separation, acid leaching solution and acid leaching residue are obtained. The acid leaching solution was sequentially filtered through a microfiltration membrane, separated by a nanofiltration membrane, and concentrated by a reverse osmosis membrane to obtain a concentrated phosphoric acid solution. The concentrated phosphoric acid solution was subjected to vacuum distillation, and the fraction was collected to obtain phosphoric acid.
2. The method according to claim 1, characterized in that, The particle size of the phosphorus-iron slag powder is 100-200 mesh.
3. The method according to claim 1, characterized in that, The acidic solution includes sulfuric acid solution or hydrochloric acid solution.
4. The method according to claim 3, characterized in that, The sulfuric acid solution has a mass fraction of 20-40%; the hydrochloric acid solution has a mass fraction of 15-30%.
5. The method according to claim 3 or 4, characterized in that, The mass ratio of the phosphorus iron slag powder to the volume of the acidic solution is 1 g:(3-8) mL.
6. The method according to claim 5, characterized in that, The acid leaching treatment is carried out under stirring conditions, with a stirring rate of 200-500 r / min; the acid leaching treatment temperature is 60-90℃, and the time is 2-6 h.
7. The method according to claim 1, characterized in that, The solid-liquid separation method includes pressure filtration or centrifugation; the pressure of the pressure filtration is 0.3-0.6 MPa, the speed of the centrifugation is 3000-5000 r / min, and the time of the solid-liquid separation is 15-60 min.
8. The method according to claim 1, characterized in that, The microfiltration membrane has a pore size of 0.1-1 μm and an operating pressure of 0.1-0.3 MPa. The material of the microfiltration membrane includes polytetrafluoroethylene, polyvinylidene fluoride, or polypropylene. The nanofiltration membrane has a molecular weight cutoff of 200-800 Da and an operating pressure of 0.5-1.5 MPa. The material of the nanofiltration membrane includes polyamide, polyethersulfone, or composite polyamide. The reverse osmosis membrane operates at a pressure of 1.0-2.5 MPa and is made of aromatic polyamide composite membrane.
9. The method according to claim 1 or 8, characterized in that, The concentrated phosphoric acid solution has a phosphoric acid mass concentration of 45-65%, a total metal impurity content of ≤0.05%, and a solid impurity content of ≤0.01%.
10. The method according to claim 1, characterized in that, The vacuum distillation is performed at a vacuum level of 0.06-0.09 MPa, a temperature of 80-140℃, and a time of 2-4 h.