Method for deep removal of anions from lithium dihydrogen phosphate solution
By adjusting the pH of the lithium dihydrogen phosphate solution and utilizing a weakly basic anion exchange resin and a special defluorination resin to selectively adsorb SO4²⁻ and Cl⁻, the problem of deep removal of anionic impurities in the preparation of lithium dihydrogen phosphate was solved, achieving high yield and high purity of lithium dihydrogen phosphate.
Patent Information
- Application Number
- CN202611458662.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-18
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies struggle to efficiently and deeply remove anionic impurities such as SO4²⁻, Cl⁻, and F⁻ during the preparation of lithium dihydrogen phosphate, while maintaining a high lithium yield. This limits the quality and domestic production of electronic-grade lithium dihydrogen phosphate.
By adjusting the pH of the lithium dihydrogen phosphate solution to 2–4, ion exchange is performed using a weakly basic anion exchange resin to selectively adsorb SO4²⁻ and Cl⁻, while retaining H₂PO₄⁻ in the solution. Combined with soluble barium salt pretreatment and a special defluorination resin, impurities are further removed, achieving deep removal.
The process achieves deep removal of SO4²⁻, Cl⁻, and F⁻ to the ppm to ppb level, with a lithium dihydrogen phosphate yield of over 95%, meeting battery-grade and electronic-grade requirements. The process is simple, cost-controllable, and applicable to various lithium dihydrogen phosphate solution sources.
Smart Images

Figure CN123105574A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of lithium battery material preparation technology, and in particular to a method for deep removal of anions from a lithium dihydrogen phosphate solution. Background Technology
[0002] Lithium dihydrogen phosphate (LiH2PO4) is an important precursor lithium salt for lithium-ion battery cathode materials. With the rapid expansion of the lithium battery industry, especially lithium iron phosphate batteries, the quality requirements for lithium dihydrogen phosphate continue to increase. Current preparation methods commonly result in lithium dihydrogen phosphate solutions or intermediate mother liquors containing SO4²⁻. - Cl - F - Anionic impurities are present. These anionic impurities are difficult to separate effectively in conventional crystallization steps and accumulate in the solid product during crystallization, directly affecting the conductivity, cycle life, and high-temperature stability of downstream cathode materials. They are one of the key bottlenecks restricting the localization and quality improvement of electronic-grade lithium dihydrogen phosphate.
[0003] However, existing anion removal technologies have consistently lacked an economically feasible solution that combines high removal rates with high lithium yields. Specifically, this requires selectively removing impurity anions while retaining the target H₂PO₄. - It is quite difficult. For example, chemical precipitation methods (such as barium salt precipitation) can remove SO4²⁻. - However, it is difficult to balance Cl - F - And introduce new cations (Ba²) + Ca² + It also generates solid waste; nanofiltration and other membrane methods for treating divalent SO4²⁻ - It has some retention effect, but for monovalent Cl... - Poor selectivity, and H2PO4 - It may also be trapped, limiting lithium recovery; ion exchange resins are theoretically the most direct, economical, and renewable method for removing anions, but the prevailing understanding is that anion exchange resins are less effective at exchanging SO4²⁻. - Cl - It will also adsorb the target H2PO4 at the same time. - This leads to a significant decrease in lithium dihydrogen phosphate recovery. This perception that "removing anions inevitably reduces lithium yield" constitutes a clear negative instruction regarding the use of ion exchange resins to remove anions from lithium dihydrogen phosphate solutions.
[0004] Therefore, there is an urgent need for a general technical solution that can deeply remove anionic impurities while maintaining a high yield of lithium dihydrogen phosphate, and that is simple, industrializable, cost-controllable, and applicable to various lithium dihydrogen phosphate solution sources (ore / salt lake / acid hydrolysis / recovery). Summary of the Invention
[0005] In view of the technical problems existing in the background art, this application provides a method for deep removal of anions from lithium dihydrogen phosphate solution, aiming to solve the technical problem of the bottleneck of anion impurity removal in the process of domestic production of electronic-grade lithium dihydrogen phosphate.
[0006] To achieve the above objectives, this application provides a method for deep removal of anions from a lithium dihydrogen phosphate solution, characterized by comprising the following steps: S1. Provide a crude lithium dihydrogen phosphate solution, adjust the pH to 2-4, and obtain the adjusted lithium dihydrogen phosphate solution; S2. The adjusted lithium dihydrogen phosphate solution is passed through a weakly basic anion exchange resin for ion exchange, selectively adsorbing anions to obtain a refined lithium dihydrogen phosphate solution.
[0007] Furthermore, in step S2, selective adsorption includes: adsorbing SO4²⁻. - Cl - H2PO4 - It remains in the solution.
[0008] Furthermore, in step S1, the crude lithium dihydrogen phosphate solution contains SO4²⁻. - Cl - At least one of them.
[0009] Furthermore, in step S1, the pH of the crude solution is adjusted to 2.5–3.5.
[0010] Furthermore, in step S2, the weakly basic anion exchange resin includes: tertiary amine type, primary amine type, and polyamine type macroporous weakly basic anion exchange resin; the flow rate of the adjusted lithium dihydrogen phosphate solution through the weakly basic anion exchange resin is 0.5 to 3 BV / h.
[0011] Furthermore, in step S2, a weakly basic anion exchange resin is packed into an ion exchange column; the height-to-diameter ratio of the ion exchange column is 3 to 10.
[0012] Furthermore, it also includes: regenerating the weakly basic anion exchange resin that has been saturated with adsorption after ion exchange. The regeneration process includes soaking or washing the saturated weakly basic anion exchange resin with sodium hydroxide or sodium chloride solution. The mass concentration of sodium hydroxide solution or sodium chloride solution is 2-10%.
[0013] Furthermore, it also includes: adding a soluble barium salt to the adjusted lithium dihydrogen phosphate solution before passing it through a weakly basic anion exchange resin, allowing it to react fully, then separating the solid and liquid components, and finally performing ion exchange. The soluble barium salt is at least one of barium carbonate, barium hydroxide, and barium chloride, and the amount of soluble barium salt added is equal to the amount of SO4²⁻ in the crude lithium dihydrogen phosphate solution. - 0.9 to 1.2 times the molar amount.
[0014] Further crude lithium dihydrogen phosphate solution contains F - After obtaining the refined lithium dihydrogen phosphate solution, a defluorination treatment is also included; the defluorination treatment includes: passing the refined lithium dihydrogen phosphate solution through an activated alumina adsorption column or a special defluorination resin to remove F. - ; Among them, the special defluorination resins include: zirconium-loaded or aluminum-loaded hydrated oxide defluorination resins.
[0015] Furthermore, it also includes: crystallizing, separating solids and liquids, washing, and drying the refined lithium dihydrogen phosphate solution to obtain battery-grade or electronic-grade lithium dihydrogen phosphate.
[0016] The beneficial technical effects of this application are as follows: 1. This application provides a method for deep removal of anions from a lithium dihydrogen phosphate solution, which involves adjusting the pH of the lithium dihydrogen phosphate solution to 2-4 and then passing it through a weakly basic anion exchange resin to selectively adsorb SO4²⁻. - Cl - And make H2PO4 - Retained in solution, it achieves deep removal of anions, thus reducing SO4²⁻. - Cl - F - It can remove lithium dihydrogen phosphate down to the ppm to ppb level, meeting the requirements of battery-grade and even electronic-grade lithium dihydrogen phosphate, while achieving a lithium dihydrogen phosphate yield of over 95%.
[0017] 2. This application provides a method for deep removal of anions from a lithium dihydrogen phosphate solution. This method utilizes the inherent selectivity of weak-base resins—which only exchange strong acid anions and not weak acid anions—which is independent of concentration, even when H2PO4 is present. - The concentration is much higher than that of SO4² - Cl - It can still stably "discard more and retain less," selectively removing impurity anions without losing the target anion, and overcomes the technical bias of decreased yield caused by resin adsorption of target products. For the first time, it has achieved selective removal of H2PO4. - (Weak acid radical) and SO4² - / Cl - The selective separation of (strong acid radicals) achieves both deep removal and high yield while using the simplest and most economical ion exchange unit.
[0018] 3. This application provides a method for deep removal of anions from a lithium dihydrogen phosphate solution, which targets SO4²⁻. - / Cl - With F - Different chemical forms were removed separately using anion exchange resin and fluoride adsorbent, resulting in high removal efficiency and no interference between them.
[0019] 4. The method for deep removal of anions from lithium dihydrogen phosphate solution provided in this application does not depend on a specific raw material route and can be universally applied to lithium dihydrogen phosphate solutions from various sources such as lithium extraction from ore, lithium extraction from salt lakes, lithium phosphate acid hydrolysis, and recycling of waste lithium batteries. It provides a universal anion removal solution for the localization of electronic-grade lithium dihydrogen phosphate.
[0020] 5. The method for deep removal of anions from lithium dihydrogen phosphate solution provided in this application uses ion exchange as a mature unit operation, the resin is regenerable and economical, the process is simple and low-cost, and it is easy to scale up industrially. Attached Figure Description
[0021] To more clearly illustrate the technical solutions of this application, the accompanying drawings used in this application will be briefly described below. Obviously, the drawings described below are merely some embodiments of this application. For those skilled in the art, other drawings can be obtained from these drawings without any creative effort.
[0022] Figure 1 This is a schematic diagram of the process for deep removal of anions from lithium dihydrogen phosphate solution in the examples. Detailed Implementation
[0023] The embodiments of the technical solution of this application will now be described in detail with reference to the accompanying drawings. These embodiments are only used to more clearly illustrate the technical solution of this application and are therefore merely examples, and should not be used to limit the scope of protection of this application.
[0024] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains; the terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the application; the terms “comprising” and “having”, and any variations thereof, in the specification, claims, and foregoing description of the drawings are intended to cover non-exclusive inclusion.
[0025] In this document, the term "embodiment" means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of this application. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments.
[0026] The "range" disclosed in this application is defined by a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a specific parameter, it is expected that ranges of 60-110 and 80-120 are also included. Furthermore, if minimum range values of 1 and 2 are listed, and if maximum range values of 3, 4, and 5 are listed, then the following ranges are all expected: 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5. In this application, unless otherwise stated, the numerical range "ab" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0-5" have been listed in this article; "0-5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is stated as an integer ≥2, it is equivalent to disclosing that the parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0027] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions.
[0028] Unless otherwise specified, all technical features and optional technical features of this application may be combined to form new technical solutions.
[0029] Unless otherwise specified, the terms "comprising" and "including" as used in this application are open-ended. For example, "comprising" and "including" may mean that other components not listed may also be included or contained.
[0030] In the description of the embodiments in this application, the term "and / or" is merely a description of the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A existing alone, A and B existing simultaneously, and B existing alone. Additionally, the character " / " in this document generally indicates that the preceding and following related objects have an "or" relationship.
[0031] To address the technical bottleneck of anion removal during the domestic production of electronic-grade lithium dihydrogen phosphate, this application provides a method for deep removal of anions from a lithium dihydrogen phosphate solution. This application involves adjusting the pH of a crude lithium dihydrogen phosphate solution to 2-4 to obtain an adjusted lithium dihydrogen phosphate solution, which is then passed through a weakly basic anion exchange resin for ion exchange, selectively adsorbing anions to obtain a refined lithium dihydrogen phosphate solution. Through these steps, deep removal of SO4²⁻ is achieved. -Cl - F - While eliminating anionic impurities, it maintains a high yield of lithium dihydrogen phosphate.
[0032] Specifically, this application provides a method for deep removal of anions from a lithium dihydrogen phosphate solution, characterized by the following steps: S1. Provide a crude lithium dihydrogen phosphate solution, adjust the pH to 2-4, and obtain the adjusted lithium dihydrogen phosphate solution; S2. The adjusted lithium dihydrogen phosphate solution is passed through a weakly basic anion exchange resin for ion exchange, selectively adsorbing anions to obtain a refined lithium dihydrogen phosphate solution.
[0033] In the technical solution of this application embodiment, the above steps constitute a complete deep anion removal process. Its core lies in utilizing the selectivity difference between strong and weak acid anions of the weakly basic anion exchange resin to achieve the removal of impurity anions while retaining the target anion. It can be understood that the functional group of the weakly basic anion exchange resin is a weakly basic group, and its ion exchange is essentially "acid adsorption." Under acidic conditions, the weakly basic group is protonated and becomes positively charged, allowing only strong acid anions (such as Cl-) to be removed. - SO4² - Only when the protonated amine group is present can it form a stable salt and be adsorbed; while the anion of a weak acid, H2PO4, can be adsorbed. - (Its conjugate acid, H3PO4, is a weak acid with pKa1 = 2.15) and is not adsorbed. In other words, the selectivity of a weakly basic anion exchange resin for anions is determined by the strength of the acid corresponding to that anion, not by the concentration of that anion in the solution—regardless of H2PO4. - Regardless of the concentration, it is not adsorbed by the weakly basic resin. This is also corroborated by well-known anion-selective sequences in the field: the strong basic resin sequence contains H2PO4. - (Therefore it will adsorb it), the weakly basic resin sequence does not contain H2PO4. - (Therefore, it does not adsorb). Therefore, by adjusting the pH of the lithium dihydrogen phosphate solution to 2-4 and passing it through a weakly basic anion exchange resin, SO4²⁻ can be removed. - Cl - At the same time, H2PO4 - The solution is retained to obtain a refined lithium dihydrogen phosphate solution. The above method can be used independently for deep anion removal from lithium dihydrogen phosphate solutions, or it can be used as an anion removal unit in an overall impurity removal process.
[0034] Furthermore, in step S2, selective adsorption includes: adsorbing SO4²⁻. - Cl - H2PO4 - It remains in the solution.
[0035] In the technical solution of this application embodiment, the selective adsorption is determined by the intrinsic characteristics of the weakly basic anion exchange resin. It is understood that this selectivity is determined by the strength of the acid corresponding to the anion and is independent of the concentration of each anion in the solution; therefore, even with H2PO4… - The concentration is much higher than that of SO4² - Cl - It can still achieve selective removal by "discarding more and taking less".
[0036] Furthermore, in step S1, the crude lithium dihydrogen phosphate solution contains SO4²⁻. - Cl - At least one of them.
[0037] In the technical solutions of this application, the aforementioned anionic impurities are typical impurities commonly found in various lithium dihydrogen phosphate preparation routes, mainly originating from sulfates and chlorides in the raw materials. The method of this application has a deep removal effect on all of the aforementioned anionic impurities.
[0038] Furthermore, in step S1, the pH of the crude solution is adjusted to 2.5–3.5.
[0039] In the technical solution of this application embodiment, the pH is further preferably 2.5 to 3.5, which can improve the exchange capacity of the weakly basic resin for strong acid anions and its exchange capacity for H2PO4. - A better balance is achieved between the retention rates of these components. It is understandable that if the pH is too low, the H+ in the solution will increase. + The concentration is too high, and the protonation degree of some weakly basic resins is too high, which may affect H2PO4. - A certain degree of adsorption occurs, leading to H2PO4... - The retention rate decreases slightly; if the pH is too high, the protonation degree of the weakly basic resin decreases, affecting its ability to retain SO4²⁻. - Cl - The exchange capacity is reduced, the removal rate is decreased, and H2PO4 is also reduced. - It may partially dissociate into HPO4² - (pKa2=7.20), divalent anion HPO4² - The charge density is higher than that of H2PO4 - It is more easily adsorbed by weakly basic resins, increasing H2PO4. - The risk of loss.
[0040] Furthermore, in step S2, the weakly basic anion exchange resin includes: tertiary amine type, primary amine type, and polyamine type macroporous weakly basic anion exchange resin; the flow rate of the adjusted lithium dihydrogen phosphate solution through the weakly basic anion exchange resin is 0.5 to 3 BV / h.
[0041] In the technical solution of this application embodiment, the particle size of the weakly basic anion exchange resin is 0.3–1.25 mm, and the total exchange capacity is ≥4.2 mmol / g. Regarding weakly basic resins, tertiary amine, primary amine, and polyamine macroporous weakly basic resins have the weakest basicity and the best selectivity for weak acid radicals. Commercially available D301 type resins (e.g., D301G, D301R, D301T, etc.) can be used for this purpose. Their functional groups are tertiary amine groups, and their backbone is a styrene-divinylbenzene copolymer. Primary amine and polyamine weakly basic resins can also be used in this invention, but their selectivity for H2PO4 is limited. - The retention rate is slightly lower than that of tertiary amines. Maintaining a reasonable flow rate within a suitable range ensures sufficient exchange while maintaining reasonable processing efficiency. If the flow rate is too high, the contact time between the solution and the resin is insufficient, resulting in incomplete ion exchange; if the flow rate is too low, the processing efficiency decreases.
[0042] In the embodiments of this application, it is necessary to explain the specific meanings of "macropores" and "weak alkalinity": "Macropores" refers to the resin having a permanent macroporous structure with an average pore size of 20-40 nm, a specific surface area of 400-600 m² / g, and a milky white and opaque appearance in a wet state; "weak alkalinity" refers to the resin having a tertiary amine functional group, a pKa of approximately 7-9, and an applicable pH range of 0-7.
[0043] Furthermore, in step S2, a weakly basic anion exchange resin is packed into an ion exchange column; the height-to-diameter ratio of the ion exchange column is 3 to 10.
[0044] In the technical solution of this application embodiment, the weakly basic anion exchange resin is packed in an ion exchange column to form a resin bed. The adjusted lithium dihydrogen phosphate solution enters from one end of the ion exchange column and flows out from the other end, undergoing ion exchange with the protonated amine groups on the resin surface during the flow through the resin bed. It is understood that the ion exchange column provides a fixed bed structure for the resin, ensuring sufficient contact between the solution and the resin while facilitating flow rate control and regeneration operations. It is also understood that the height-to-diameter ratio of the ion exchange column can affect the mass transfer efficiency and pressure drop of the resin bed to a certain extent. If the height-to-diameter ratio is too small, the resin bed is too short, resulting in insufficient residence time of the solution in the bed and incomplete exchange; if the height-to-diameter ratio is too large, the bed pressure drop increases, increasing the requirements for the pumping equipment. Controlling the height-to-diameter ratio within the range of 3 to 10 can ensure sufficient exchange while maintaining a reasonable bed pressure drop.
[0045] Furthermore, it also includes: regenerating the weakly basic anion exchange resin that has been saturated with adsorption after ion exchange. The regeneration process includes soaking or washing the saturated weakly basic anion exchange resin with sodium hydroxide or sodium chloride solution. The mass concentration of sodium hydroxide solution or sodium chloride solution is 2-10%.
[0046] In the technical solution of this application embodiment, the purpose of the regeneration treatment is to remove the SO4² adsorbed on the resin. - Cl - The OH groups are washed away, restoring the resin's exchange capacity. It's understandable that when using sodium hydroxide solution, the OH groups in NaOH... - SO4² on the resin can be removed - Cl - Displacement causes the resin to convert to the OH form; when using sodium chloride solution, the Cl in NaCl... - SO4² on the resin can be removed - The process involves displacement, converting the resin to the Cl-type. If the concentration of the sodium hydroxide or sodium chloride solution is too low, regeneration will be insufficient, and the resin's exchange capacity will not be fully restored; if the concentration is too high, regeneration costs will increase and may damage the resin structure. Controlling the concentration within a reasonable range ensures both regeneration effectiveness and economic efficiency. During regeneration, the flow rate of the sodium hydroxide or sodium chloride solution should be 1–3 BV / h, the temperature 20–40 °C, and the time 2–4 h.
[0047] Furthermore, it also includes: adding a soluble barium salt to the adjusted lithium dihydrogen phosphate solution before passing it through a weakly basic anion exchange resin, allowing it to react fully, then separating the solid and liquid components, and finally performing ion exchange. The soluble barium salt is at least one of barium carbonate, barium hydroxide, and barium chloride, and the amount of soluble barium salt added is equal to the amount of SO4²⁻ in the crude lithium dihydrogen phosphate solution. - 0.9 to 1.2 times the molar amount.
[0048] In the technical solution of this application embodiment, the purpose of adding soluble barium salt is to pre-precipitate and remove part of SO4². - This is to reduce the load on the subsequent anion exchange resin. It is understandable that Ba²⁺... + With SO4² - The reaction produces a sparingly soluble BaSO4 precipitate, most of which can be separated by solid-liquid separation. - Removing SO4² from the solution prolongs the resin regeneration cycle and reduces the regeneration frequency. If the amount added is too low, SO4²⁻ - Incomplete precipitation, residual SO4² - The resin still needs to bear the burden; if the amount added is too high, excessive Ba² will cause damage. + It may remain in the solution and needs to be further removed in subsequent steps. Controlling the amount added within a reasonable range can ensure the preservation of SO4²⁻. - While achieving precipitation effect, avoid Ba² + Excessive residue.
[0049] Further crude lithium dihydrogen phosphate solution contains F - After obtaining the refined lithium dihydrogen phosphate solution, a defluorination treatment is also included; the defluorination treatment includes: passing the refined lithium dihydrogen phosphate solution through an activated alumina adsorption column or a special defluorination resin to remove F. - ; Among them, the special defluorination resins include: zirconium-loaded or aluminum-loaded hydrated oxide defluorination resins.
[0050] In the technical solution of this application embodiment, since hydrofluoric acid is a weak acid (pKa≈3.17), fluoride exists mainly in the form of neutral HF molecules under pH 2-4 conditions. Ion exchange resins have weak exchange capacity for it, therefore a separate fluoride removal method is required. Activated alumina has a porous structure and a large specific surface area (particle size 1-3 mm, specific surface area ≥200 m² / g), which is effective against fluoride. - The removal of fluoride is mainly achieved through adsorption and surface complexation. Zirconium-loaded or aluminum-loaded hydrated oxide defluorinating resins remove fluoride through hydrated zirconium oxide or hydrated aluminum oxide. - Highly selective adsorption enables deep defluorination. The defluorination step is combined with SO4²⁻. - Cl - The resin removal is separated, which can avoid F - With SO4² - Cl - Competing adsorption sites on the same resin achieves classification and impurity removal without interference.
[0051] Furthermore, it also includes: crystallizing, separating solids and liquids, washing, and drying the refined lithium dihydrogen phosphate solution to obtain battery-grade or electronic-grade lithium dihydrogen phosphate.
[0052] In the technical solution of this application embodiment, crystallization can be performed by alcohol recrystallization, wherein the alcohol is one of ethanol, methanol, and isopropanol; drying can be performed by vacuum step drying at a temperature of 40–120°C. The above steps are all conventional operations in the art, and those skilled in the art can select them according to actual needs.
[0053] The embodiments of this application will be described in further detail below with reference to the accompanying drawings and examples. The detailed description of the following embodiments and the accompanying drawings are used to illustrate the principles of this application by way of example, but should not be used to limit the scope of this application, that is, this application is not limited to the described embodiments.
[0054] I. Preparation Method Example 1 This embodiment provides a method for deep removal of anions from a lithium dihydrogen phosphate solution, specifically including the following steps: S1 has a main content of 30% and an anion concentration of SO4². - =500 ppm, Cl- =300 ppm, F - =100 ppm lithium dihydrogen phosphate solution, adjust pH to 3.
[0055] S2. The pH-adjusted lithium dihydrogen phosphate solution is passed at a flow rate of 1 BV / h through an exchange column (height-to-diameter ratio of 5) packed with tertiary amine-type macroporous weakly basic anion exchange resin (D301G type, particle size 0.3–1.25 mm, total exchange capacity ≥4.2 mmol / g) to remove SO4²⁻. - Cl - .
[0056] S3. Pass the effluent through an activated alumina adsorption column (γ-Al2O3 type, particle size 1-3 mm, specific surface area 320 m² / g) to remove F. - The resulting lithium dihydrogen phosphate purified solution with deep anion removal was obtained.
[0057] It should be noted that the ion exchange resins used in this embodiment and the following embodiments and comparative examples were all purchased from Zhejiang Zhengguang Industrial Co., Ltd. However, this application is not limited to this. It is understood that other manufacturers that can supply resins of the same specifications (such as Xi'an Lanxiao Technology New Materials Co., Ltd.) can meet the requirements, and all types of resins of the same model are applicable to this application.
[0058] Example 2 This embodiment provides a method for deep removal of anions from a lithium dihydrogen phosphate solution. The difference from Embodiment 1 is that in step S2, a polyamine-type macroporous weakly basic anion exchange resin (commercially available D311 type) is used. The remaining steps and parameters are the same as in Embodiment 1 and will not be repeated here.
[0059] Example 3 This embodiment provides a method for deep removal of anions from a lithium dihydrogen phosphate solution. The difference from Embodiment 1 is that in step S2, a primary amine-type macroporous weakly basic anion exchange resin (commercially available D315 type) is used. The remaining steps and parameters are the same as in Embodiment 1 and will not be repeated here.
[0060] Example 4 This embodiment provides a method for deep removal of anions from a lithium dihydrogen phosphate solution. The difference from Embodiment 1 is that in step S1, the pH of the lithium dihydrogen phosphate solution is adjusted to 2. The remaining steps and parameters are the same as in Embodiment 1 and will not be repeated here.
[0061] Example 5 This embodiment provides a method for deep removal of anions from a lithium dihydrogen phosphate solution. The difference from Embodiment 1 is that in step S1, the pH of the lithium dihydrogen phosphate solution is adjusted to 4. The remaining steps and parameters are the same as in Embodiment 1 and will not be repeated here.
[0062] Example 6 This embodiment provides a method for deep removal of anions from a lithium dihydrogen phosphate solution. The difference from Embodiment 1 is that in step S2, the pH-adjusted lithium dihydrogen phosphate solution is passed through a tertiary amine-type macroporous weakly basic anion exchange resin at a flow rate of 0.5 BV / h. The remaining steps and parameters are the same as in Embodiment 1 and will not be repeated here.
[0063] Example 7 This embodiment provides a method for deep removal of anions from a lithium dihydrogen phosphate solution. The difference from Embodiment 1 is that in step S2, the pH-adjusted lithium dihydrogen phosphate solution is passed through a tertiary amine-type macroporous weakly basic anion exchange resin at a flow rate of 3 BV / h. The remaining steps and parameters are the same as in Embodiment 1 and will not be repeated here.
[0064] Example 8 This embodiment provides a method for deep removal of anions from lithium dihydrogen phosphate solution. The difference from Embodiment 1 is that in step S3, a zirconium-supported hydrated oxide defluorination resin (particle size 0.3–1.2 mm, specific surface area ≥150 m² / g) is used instead of the activated alumina adsorption column. The remaining steps and parameters are the same as in Embodiment 1 and will not be repeated here.
[0065] Comparative Example 1 This comparative example provides a method for deep removal of anions from a lithium dihydrogen phosphate solution. The difference from Example 1 is that in step S2, a strongly basic (quaternary ammonium type) anion exchange resin (commercially available D201 type) is used instead. The remaining steps and parameters are the same as in Example 1 and will not be repeated here.
[0066] Comparative Example 2 This comparative example provides a method for deep removal of anions from a lithium dihydrogen phosphate solution. The difference from Example 1 is that in step S1, the pH of the lithium dihydrogen phosphate solution is adjusted to 1. The remaining steps and parameters are the same as in Example 1 and will not be repeated here.
[0067] Comparative Example 3 This comparative example provides a method for deep removal of anions from a lithium dihydrogen phosphate solution. The difference from Example 1 is that in step S1, the pH of the lithium dihydrogen phosphate solution is adjusted to 6. The remaining steps and parameters are the same as in Example 1 and will not be repeated here.
[0068] Comparative Example 4 This comparative example provides a method for deep removal of anions from a lithium dihydrogen phosphate solution. The difference from Example 1 is that in step S2, the pH-adjusted lithium dihydrogen phosphate solution is passed through a tertiary amine-type macroporous weakly basic anion exchange resin at a flow rate of 5 BV / h. The remaining steps and parameters are consistent with Example 1 and will not be repeated here.
[0069] Comparative Example 5 This comparative example provides a method for deep removal of anions from a lithium dihydrogen phosphate solution. The difference from Example 1 is that step S3, F, is omitted. - Impurity removal. The remaining steps and parameters are the same as in Example 1, and will not be repeated here.
[0070] II. Analysis of Test Results for Each Embodiment and Comparative Example The contents of relevant components in the lithium dihydrogen phosphate purified solutions after deep anion removal prepared in Examples 1-8 were determined, and the results are shown in Table 1.
[0071] Table 1. Anion purification and process performance analysis of Examples 1-8 The contents of relevant components in the lithium dihydrogen phosphate purified solutions after deep anion removal prepared in Comparative Examples 1-5 were determined, and the results are shown in Table 2.
[0072] Table 2. Anion purification and process performance analysis of Comparative Examples 1-5 To analyze the impact of anion exchange resin type on impurity removal selectivity and product purity, the detection results of lithium dihydrogen phosphate prepared in Examples 1-3 and Comparative Example 1 were compared. Tables 1-2 show that Example 1 used a tertiary amine type macroporous weakly basic anion exchange resin, especially the D301 type resin. This resin has the weakest basicity and the best selectivity for weak acid anions, effectively removing anionic impurities at a suitable pH while reducing the adsorption of dihydrogen phosphate, thus ensuring product purity and yield. Example 2 used a polyamine type macroporous weakly basic anion exchange resin, and Example 3 used a primary amine type macroporous weakly basic anion exchange resin. Both belong to the category of weakly basic anion exchange resins and can achieve a certain degree of deep anion impurity removal. However, their functional groups differ from those of the tertiary amine type, and their basicity and weak acid anion selectivity may differ. Therefore, their deep impurity removal effect may be slightly inferior to that of Example 1, but they should still be able to effectively remove anionic impurities and obtain electronic-grade lithium dihydrogen phosphate. This setting indicates that the anion exchange resin is not limited to tertiary amine type; weakly basic anion exchange resins do not adsorb H2PO4. - This is a common characteristic (independent of concentration), and among them, the tertiary amine type macroporous weak base resin has the best selectivity, making it the preferred solution of this invention. Comparative Example 1 used a strongly basic quaternary ammonium type anion exchange resin, which could remove SO4²⁻.- Cl - and F - However, strong alkali resins simultaneously adsorb large amounts of H2PO4. - This resulted in a significant decrease in the lithium dihydrogen phosphate yield (from 98.5% in Example 1 to 64%), and also led to frequent resin regeneration and increased production costs. This comparative example confirms that the phenomenon of "resin adsorption of lithium dihydrogen phosphate" in the comparative document is indeed caused by strong base resin, while weak base resin can overcome this. In summary, a weak base anion exchange resin should be used, preferably a tertiary amine type macroporous weak base anion exchange resin.
[0073] To analyze the effect of the pH of the lithium dihydrogen phosphate solution on the depth of anion removal and product purity, the detection results of lithium dihydrogen phosphate prepared in Examples 1, 4-5, and Comparative Examples 2-3 were compared. As shown in Tables 1-2, the pH of the lithium dihydrogen phosphate solution in Example 1 is within the preferred range of this invention. The weakly basic anion exchange resin can maintain appropriate protonation, thus improving the removal of Cl-. - SO4² - Anionic impurities exhibit good exchange capacity, while the lithium dihydrogen phosphate system remains stable and does not readily precipitate. In Example 4, the pH was adjusted to 2, and in Example 5, the pH was adjusted to 4. Both are within suitable ranges, allowing the resin to maintain a moderately protonated state and exhibit good selectivity for weak acid radicals. Meanwhile, H... + The competition was not excessive, the lithium dihydrogen phosphate system was stable, and a similar impurity removal effect as in Example 1 was achieved. In Comparative Example 2, the pH was adjusted to 1. At this point, the acidity was too strong, and H... + The competitive effect is significant; the exchange capacity of weakly basic anion exchange resin decreases, SO4² - Cl - F is difficult to remove effectively, resulting in increased residue; at the same time, in a strong acid environment, activated alumina partially dissolves and its defluorination ability decreases, leading to increased fluoride levels. - The residue also increased, and the resulting product had higher levels of anionic impurities and fluorine, resulting in lower purity than in Example 1. In Comparative Example 3, the pH was adjusted to 6, but the weakly basic anion exchange resin showed insufficient protonation, leading to a decrease in exchange capacity and SO4²⁻ content. - Cl - Residual levels increased; however, pH 6 was close to the optimal defluorination range for activated alumina, F - It can still be deeply removed, its F - The content is similar to that in Example 1. In summary, the pH of the lithium dihydrogen phosphate solution should be controlled between 2 and 4. A pH that is too low or too high is not conducive to the deep purification of weakly basic anion exchange resin.
[0074] To analyze the effect of the flow rate of the lithium dihydrogen phosphate solution after pH adjustment on the exchange efficiency through the resin, the detection results of lithium dihydrogen phosphate prepared in Examples 1, 6-7, and Comparative Example 4 were compared. As shown in Tables 1-2, Example 6 used a low flow rate of 0.5 BV / h, ensuring sufficient contact between the solution and the resin, and reducing SO4²⁻. - Cl - More thorough removal (reduced to 3 ppm and 1 ppm respectively); Example 7 used a higher flow rate of 3 BV / h, SO4² - Cl - The removal efficiency decreased slightly (to 9 ppm and 5 ppm respectively), but still met the electronic grade requirements; while Comparative Example 4 used an excessively high flow rate of 5 BV / h, resulting in severely insufficient contact time and SO4²⁻ removal. - Cl - The residual concentrations increased significantly (to 200 ppm and 120 ppm, respectively), failing to meet the requirements for electronic grade. In summary, it can be concluded that the flow rate of the lithium dihydrogen phosphate solution through the resin after pH adjustment has a significant impact on the exchange efficiency.
[0075] To analyze the impact of defluorination materials on the fluoride removal efficiency, the detection results of lithium dihydrogen phosphate prepared in Example 8 and Example 1 were compared. As shown in Table 1, Example 1 used activated alumina for fluoride removal, and the F... - Content 2 ppm; Example 8 uses zirconium-loaded hydrated oxide defluorinating resin, F - Both can achieve deep defluorination at a concentration of 1 ppm, with the zirconium-loaded hydrated oxide defluorinating resin exhibiting superior defluorination performance.
[0076] To analyze the necessity of the fluoride ion removal step, the detection results of lithium dihydrogen phosphate prepared in Example 1 and Comparative Example 5 were compared. As shown in Tables 1-2, Comparative Example 5, by omitting the fluoride removal step S3, resulted in a lower concentration of fluoride ions in its product. - The residual amount is as high as 100 ppm, which cannot meet the requirements for electronic-grade F - The requirement is ≤5 ppm, while SO4² - Cl - It can still be effectively removed by weakly basic anion exchange resins (reduced to 5 ppm and 3 ppm, respectively). In contrast, the F in the lithium dihydrogen phosphate prepared in Example 1... - The content was 2 ppm, significantly lower than that of Comparative Example 5, indicating that the defluorination step and the removal of SO4² by the weakly basic anion exchange resin were effective. - Cl - All of these steps are indispensable for achieving electronic-grade lithium dihydrogen phosphate, and the two work together to achieve deep removal of anions.
[0077] All embodiments that have the same structure and achieve the same effect as the technical concept within the scope of this application are included in the scope of this application. Various modifications that can be conceived by those skilled in the art to the embodiments, and other ways of constructing embodiments by combining some of the constituent elements, without departing from the spirit of this application, are also included in the scope of this application.
[0078] Furthermore, although this application has been described with reference to preferred embodiments, various modifications can be made thereto and components can be replaced with equivalents without departing from the scope of this application. In particular, the technical features mentioned in the various embodiments can be combined in any manner, provided there is no structural conflict. This application is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.
Claims
1. A method for deep removal of anions from a lithium dihydrogen phosphate solution, characterized in that, Includes the following steps: S1. Provide a crude lithium dihydrogen phosphate solution, adjust the pH to 2-4, and obtain the adjusted lithium dihydrogen phosphate solution; S2. The adjusted lithium dihydrogen phosphate solution is passed through a weakly basic anion exchange resin for ion exchange, selectively adsorbing anions to obtain a refined lithium dihydrogen phosphate solution.
2. The method for deep removal of anions from lithium dihydrogen phosphate solution according to claim 1, characterized in that, In step S2, the selective adsorption includes: adsorbing SO4²⁻ - Cl - H2PO4 - It remains in the solution.
3. The method for deep removal of anions from lithium dihydrogen phosphate solution according to claim 1, characterized in that, In step S1, the crude lithium dihydrogen phosphate solution contains SO4²⁻. - Cl - At least one of them.
4. The method for deep removal of anions from lithium dihydrogen phosphate solution according to claim 1, characterized in that, In step S1, the pH of the crude solution is adjusted to 2.5-3.
5.
5. The method for deep removal of anions from lithium dihydrogen phosphate solution according to claim 1, characterized in that, In step S2, the weakly basic anion exchange resin includes: tertiary amine type, primary amine type, and polyamine type macroporous weakly basic anion exchange resin; the flow rate of the adjusted lithium dihydrogen phosphate solution through the weakly basic anion exchange resin is 0.5 to 3 BV / h.
6. The method for deep removal of anions from lithium dihydrogen phosphate solution according to claim 5, characterized in that, In step S2, the weakly basic anion exchange resin is packed into an ion exchange column; the height-to-diameter ratio of the ion exchange column is 3 to 10.
7. The method for deep removal of anions from lithium dihydrogen phosphate solution according to claim 1, characterized in that, Also includes: The weakly basic anion exchange resin that has been saturated with adsorption after ion exchange is regenerated. The regeneration process includes soaking or washing the saturated weakly basic anion exchange resin with sodium hydroxide solution or sodium chloride solution. The mass concentration of the sodium hydroxide solution or sodium chloride solution is 2-10%.
8. The method for deep removal of anions from lithium dihydrogen phosphate solution according to claim 1, characterized in that, Also includes: Before passing the solution through a weakly basic anion exchange resin, a soluble barium salt is added to the adjusted lithium dihydrogen phosphate solution. After the solution reacts fully, solid-liquid separation is performed, followed by ion exchange. The soluble barium salt is at least one of barium carbonate, barium hydroxide, and barium chloride, and the amount of the soluble barium salt added is equal to the amount of SO4²⁻ in the crude lithium dihydrogen phosphate solution. - 0.9 to 1.2 times the molar amount.
9. The method for deep removal of anions from lithium dihydrogen phosphate solution according to claim 1, characterized in that, The crude lithium dihydrogen phosphate solution contains F. - After obtaining the refined lithium dihydrogen phosphate solution, the process further includes a defluorination treatment; the defluorination treatment includes: passing the refined lithium dihydrogen phosphate solution through an activated alumina adsorption column or a special defluorination resin to remove fluoride. - ; The special defluorination resin includes: zirconium-loaded or aluminum-loaded hydrated oxide defluorination resin.
10. The method for deep removal of anions from lithium dihydrogen phosphate solution according to any one of claims 1 to 9, characterized in that, Also includes: The refined lithium dihydrogen phosphate solution is subjected to crystallization, solid-liquid separation, washing, and drying to obtain battery-grade or electronic-grade lithium dihydrogen phosphate.