A coal tar pitch-based porous carbon, its preparation method and application
By treating coal tar pitch with microwave heating equipment and composite activators in air, the problems of stability and pore size inhomogeneity of coal tar pitch-based porous carbon were solved, achieving efficient and low-cost preparation of porous carbon and improving the performance of supercapacitors.
Patent Information
- Application Number
- CN202611211049.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-11
- Publication Date
- 2026-11-17
AI Technical Summary
Existing coal tar pitch-based porous carbon suffers from poor stability, uneven pore size distribution, complex preparation methods, severe pollution, and high cost, making it difficult to meet the high-performance requirements of supercapacitors.
The process involves pyrolysis carbonization/activation of coal tar pitch, boric acid, and a composite activator in air using microwave heating equipment. This avoids the use of strong alkaline activators. The process utilizes the molten protective barrier generated by boric acid at high temperatures and the etching effect of K+ and CO2 produced by the activator at high temperatures to form a uniform porous structure.
This method achieves uniformity and stability of porous carbon pore structure, reduces production costs, simplifies the process, increases specific surface area and conductivity, and improves the specific capacitance performance of supercapacitors.
Smart Images

Figure CN123105632A_ABST
Abstract
Description
Technical Field
[0001] This application belongs to the field of functional carbon material preparation technology, specifically relating to a coal tar pitch-based porous carbon, its preparation method, and its application. Background Technology
[0002] Supercapacitors have attracted widespread attention due to their advantages such as high energy storage and power density, long cycle life, and fast charge and discharge. In 2025, the GB300 standard for GPU products introduced new industry standards for capacitors, requiring supercapacitors to have high discharge current (1300A) and fast response time (4-5ms). With the rapid development of electrochemical energy storage technologies such as supercapacitors, the demand for porous carbon with high capacitance performance is increasing. Porous carbon generally uses organic matter or natural carbon sources as raw materials, such as synthetic resins and biomass. These materials are limited by resource supply, production costs, and synthesis conditions. Coal tar pitch is a large amount of coal-based solid waste generated during coal chemical production, and it has advantages such as low cost, wide availability, and stable supply.
[0003] Traditional methods for preparing coal tar pitch-based porous carbon exist, but they suffer from poor stability, uneven pore size distribution, and low synthesis efficiency, limiting their practical applications. For example, the template method can precisely control pore size distribution and pore structure, but the template preparation and removal processes are complex, leading to environmental pollution. Physical activation is simple and easily scaled up, but the porous carbon products exhibit uneven pore size distribution, low product quality, and low yield. Currently, chemical activation is the most widely used industrial method, but this process uses strong alkalis, consumes a lot of energy during carbonization and activation, and requires inert gas protection, increasing production costs and environmental treatment difficulties. Therefore, it is necessary to develop a green and environmentally friendly activator and an efficient, low-cost synthesis method that ensures the uniformity, stability, and controllability of the pore structure of coal tar pitch-based porous carbon. Summary of the Invention
[0004] This application provides a coal tar pitch-based porous carbon, its preparation method, and its application, aiming to solve the problems of poor stability, uneven pore size distribution, complex preparation methods, pollution, and high cost of existing coal tar pitch-based porous carbon.
[0005] The first aspect of this application provides a method for preparing coal tar pitch-based porous carbon, comprising the following steps: (1) Mix coal tar pitch, boric acid and activator, and perform air microwave carbonization activation treatment to obtain activated material; (2) Clean and dry the activated material to obtain the coal tar pitch-based porous carbon.
[0006] The second aspect of this application provides a coal tar pitch-based porous carbon, which is prepared by the coal tar pitch-based porous carbon preparation method described in the first aspect of this application.
[0007] A third aspect of this application provides an electrode material for a supercapacitor, including the coal tar pitch-based porous carbon described in the second aspect of this application.
[0008] The beneficial effects of this application include: the coal tar pitch-based porous carbon described in this application uses coal tar pitch as raw material, employs a composite activator and a recyclable vacuum flame retardant, and undergoes pyrolysis carbonization / activation treatment in air using microwave heating equipment, avoiding the use of strong alkaline activators, reducing equipment corrosion and environmental treatment costs, and ensuring the uniformity of the porous carbon pore structure; the use of vacuum flame retardant enables rapid and efficient pyrolysis carbonization / activation treatment in air, simplifies the process flow, and reduces operating costs.
[0009] The coal tar pitch-based porous carbon described in this application has an ultra-high specific surface area and microporosity, good electrical conductivity, thermal stability and graphitization degree, and exhibits high specific capacitance performance as an electrode material for supercapacitors. Attached Figure Description
[0010] Figure 1 The N2 adsorption-desorption curves of the coal tar pitch-based porous carbon described in Example 1 and Comparative Examples 1-3 of this application are shown. Figure 2 This is a pore size distribution curve of the coal tar pitch-based porous carbon described in Example 1 and Comparative Examples 1-3 of this application; Figure 3 The X-ray diffraction pattern of the coal tar pitch-based porous carbon described in Example 1 of this application is shown below. Figure 4 The Raman spectrum of the coal tar pitch-based porous carbon described in Example 2 of this application; Figure 5 This is a thermogravimetric analysis curve of the coal tar pitch-based porous carbon described in Example 1 of this application; Figure 6 This is a scanning electron microscope image of the coal tar pitch-based porous carbon described in Example 1 of this application; Figure 7 This is the EDS elemental mapping diagram of the coal tar pitch-based porous carbon described in Example 1 of this application; Figure 8 This is a high-magnification transmission electron microscope image of the coal tar pitch-based porous carbon described in Example 1 of this application. Detailed Implementation
[0011] The embodiments of the present invention are described in detail below. These embodiments are exemplary and intended to explain the present invention, and should not be construed as limiting the present invention.
[0012] In this invention, the terms "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., refer to a specific feature, structure, material, or characteristic described in connection with that embodiment or example, which is included in at least one embodiment or example of the invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples. Moreover, without contradiction, those skilled in the art can combine and integrate the different embodiments or examples described in this specification, as well as the features of different embodiments or examples.
[0013] This application provides a method for preparing coal tar pitch-based porous carbon, comprising the following steps: (1) Mix coal tar pitch, boric acid and activator, and perform air microwave carbonization activation treatment to obtain activated material; (2) Clean and dry the activated material to obtain the coal tar pitch-based porous carbon.
[0014] The coal tar pitch-based porous carbon described in this application uses a composite activator and a recyclable vacuum flame retardant. It undergoes pyrolysis carbonization / activation treatment in air using microwave heating equipment, avoiding the use of strong alkaline activators, reducing equipment corrosion and environmental treatment costs, and ensuring the uniformity of the porous carbon pore structure. The use of vacuum flame retardant enables rapid and efficient pyrolysis carbonization / activation treatment in air, simplifying the process and reducing operating costs.
[0015] Boric acid, as a reaction medium, generates a molten protective barrier at temperatures above 170°C, spontaneously creating an oxygen-free environment without the need for high pressure or complex procedures. Furthermore, this boron-containing molten protective barrier can serve as both a template and an auxiliary chemical activator, promoting pore formation and catalyzing the generation of porous carbon.
[0016] In some embodiments of this application, the coal tar pitch includes one or more of coal liquefaction pitch, coal liquefaction pitch, coal tar pitch, and tar residue pitch.
[0017] In some embodiments of this application, the coal tar pitch has an ash content of <100 ppm, a quinoline-insoluble content of <100 ppm, and a magnetic content of <50 ppm. High-purity coal tar pitch can be prepared by solvent extraction-centrifugal filtration to meet the requirements of ash content <100 ppm, quinoline-insoluble content <100 ppm, and magnetic content <50 ppm. Then, the high-purity coal tar pitch is crushed using a high-speed pulverizer to obtain raw material powder with a particle size >300 mesh.
[0018] In some embodiments of this application, the mass ratio of the coal tar pitch to the boric acid is 1:(5-10); for example, 1:5, 1:6, 1:8, 1:10, etc. Boric acid creates a vacuum region at high temperatures, effectively isolating the air. If the mass of boric acid is below the aforementioned range, the air-isolation effect is reduced, and the coal tar pitch will react with the air at high temperatures. If the mass of boric acid is above the aforementioned range, the boric acid will, to some extent, affect the activation effect of the porous carbon and damage its pore structure.
[0019] In some embodiments of this application, the mass ratio of the coal tar pitch to the activator is 1:(1-5); for example, 1:1, 1:2, 1:3, 1:5. The activator generates "K" at high temperatures. + "The activator is etched with CO2 to form a porous structure. If the quality of the activator is lower than the above range, the activation effect will be poor, the porous carbon pore structure will not be rich, and the specific surface area will be low. If the quality of the activator is lower than the above range, it will be over-activated, which will destroy the porous carbon pore structure."
[0020] In some embodiments of this application, the activator includes potassium tetraborate and potassium citrate. This application uses potassium tetraborate and potassium citrate as a composite activator. During high-power microwave pyrolysis, the high-temperature activation effect is achieved by utilizing the rapid generation of K₂C and CO₂ at high temperatures through the thermal decomposition properties of the environmentally friendly activator. The generated K₂C... + It produces a "foaming etching" effect with CO2 gas, creating more open pore structures, forming a more stable and less prone-to-collapse carbon skeleton, and improving the porous carbon yield and specific surface area.
[0021] In some embodiments of this application, the mass ratio of potassium tetraborate to potassium citrate in the activator is 1:(5-10); for example, 1:5, 1:6, 1:8, 1:10, etc. Potassium citrate produces "K" at high temperatures. + "and CO2 etching to create pores, potassium tetraborate produces "B" at high temperature + "When boron is incorporated into porous carbon, if the mass of potassium tetraborate is below the above range, the boron doping effect is not obvious and cannot effectively improve the conductivity of porous carbon; if the mass of potassium tetraborate is above the above range, excessive H2O will be generated at high temperature, which will overactivate and destroy the pore structure of porous carbon."
[0022] In some embodiments of this application, the power of the microwave carbonization treatment is 4000-6000W, such as 4000W, 4500W, 5000W, 5500W, 6000W, etc., and the time is 10-30 minutes, such as 10 minutes, 16 minutes, 18 minutes, 25 minutes, 30 minutes, etc. Microwave carbonization treatment is more effective than traditional high-temperature carbonization. Rapid high-temperature heating causes porous carbon to generate more cracks and pore structures, which is also beneficial for subsequent air activation treatment.
[0023] Microwave heating equipment can be microwave tube furnaces, microwave carbonization furnaces, microwave ashing furnaces, or microwave pyrolysis furnaces, etc.
[0024] In some embodiments of this application, the microwave power of the activation treatment is 6000-8000W, such as 6000W, 6500W, 7000W, 7500W, 8000W, etc., and the time is 10-30 minutes.
[0025] In some embodiments of this application, the atmosphere for the microwave carbonization activation treatment is an air atmosphere.
[0026] In some embodiments of this application, step (2) includes cleaning with acid, deionized water and ethanol in sequence.
[0027] In some embodiments of this application, the acid solution includes one or more of hydrochloric acid, sulfuric acid, and nitric acid; when cleaning with acid solution, dilute acid is used, such as a 1 mol / L acid solution.
[0028] In some embodiments of this application, the drying temperature is 60-80°C and the time is 12-24 hours.
[0029] In some embodiments of this application, the method further includes the step of evaporating and concentrating deionized water and ethanol washing liquid to obtain boric acid; the boric acid can be reused, saving costs.
[0030] In some embodiments of this application, the evaporation and concentration temperature is 80°C.
[0031] This application also provides a coal tar pitch-based porous carbon, prepared by the method described in the first aspect of this application. The coal tar pitch-based porous carbon described in this application possesses ultra-high specific surface area and microporosity, good electrical conductivity, thermal stability, and a high degree of graphitization.
[0032] This application also provides an electrode material for a supercapacitor, comprising the coal tar pitch-based porous carbon described in the second aspect of this application. The electrode material for the supercapacitor described in this application exhibits high pseudocapacitance and specific capacitance performance.
[0033] The technical solution of this application will be further described below with reference to specific embodiments.
[0034] Example 1 A method for preparing coal tar pitch-based porous carbon includes the following steps: (1) Xylene was used to extract coal liquefaction pitch and centrifugation was performed to obtain high-purity coal liquefaction pitch with 98 ppm ash, 95 ppm quinoline insoluble matter and 40 ppm magnetic matter. The high-purity coal liquefaction pitch was then crushed by a high-speed pulverizer to obtain raw material powder with a particle size >300 mesh. (2) Weigh 10g of coal liquefaction pitch raw material powder, add 70g of boric acid (raw material: boric acid mass ratio 1:7) and 30g of potassium tetraborate and potassium citrate mixture (raw material powder: activator mass ratio 1:3; wherein, the mass ratio of potassium tetraborate and potassium citrate is 1:6), and ball mill the mixture at 5℃ and 800rpm for 4h using a cryogenic ball mill to obtain pretreated material; (3) Place the pretreated material in a microwave pyrolysis furnace, in an air atmosphere, and perform microwave pyrolysis carbonization treatment at 5000W power for 30 minutes; then perform microwave pyrolysis activation treatment at 8000W power for 20 minutes to obtain activated material; (4) The activated material was placed in a low-temperature ultrasonic cleaner, and an excess of 1 mol / L dilute hydrochloric acid was added. The material was ultrasonically acid-washed at 5°C for 4 hours, and then vacuum filtered and washed with deionized water and ethanol in sequence. The material was then vacuum dried at 60°C for 24 hours to obtain coal tar pitch-based porous carbon. The water-ethanol washing solution was evaporated and concentrated at 80°C to obtain boric acid.
[0035] Example 2 The only difference between the preparation method of coal tar pitch-based porous carbon in Example 2 and that in Example 1 is that coal tar pitch is used instead of coal liquefaction pitch in the preparation process of coal tar pitch-based porous carbon in Example 2.
[0036] Example 3 The only difference between the preparation method of coal tar pitch-based porous carbon in Example 3 and that in Example 1 is that the mass ratio of coal liquefaction pitch raw material powder to boric acid in the preparation process of coal tar pitch-based porous carbon in Example 3 is 1:1.
[0037] Example 4 The only difference between the preparation method of coal tar pitch-based porous carbon in Example 4 and that in Example 1 is that the mass ratio of coal liquefaction pitch raw material powder to boric acid in the preparation process of coal tar pitch-based porous carbon in Example 4 is 1:6.
[0038] Example 5 The only difference between the preparation method of coal tar pitch-based porous carbon in Example 5 and that in Example 1 is that the mass ratio of coal liquefaction pitch raw material powder to boric acid in the preparation process of coal tar pitch-based porous carbon in Example 5 is 1:15.
[0039] Example 6 The only difference between the preparation method of coal tar pitch-based porous carbon in Example 6 and that in Example 1 is that the mass ratio of coal liquefaction pitch raw material powder to activator in the preparation process of coal tar pitch-based porous carbon in Example 6 is 1:0.5.
[0040] Example 7 The only difference between the preparation method of coal tar pitch-based porous carbon in Example 7 and that in Example 1 is that the mass ratio of coal liquefaction pitch raw material powder to activator in the preparation process of coal tar pitch-based porous carbon in Example 7 is 1:2.
[0041] Example 8 The only difference between the preparation method of coal tar pitch-based porous carbon in Example 8 and that in Example 1 is that the mass ratio of coal liquefaction pitch raw material powder to activator in the preparation process of coal tar pitch-based porous carbon in Example 8 is 1:10.
[0042] Example 9 The only difference between the preparation method of coal tar pitch-based porous carbon in Example 9 and that in Example 1 is that the mass ratio of potassium tetraborate and potassium citrate in the activator during the preparation of coal tar pitch-based porous carbon in Example 9 is 1:1.
[0043] Example 10 The only difference between the preparation method of coal tar pitch-based porous carbon in Example 10 and that in Example 1 is that the mass ratio of potassium tetraborate and potassium citrate in the activator during the preparation of coal tar pitch-based porous carbon in Example 10 is 1:8.
[0044] Example 11 The only difference between the preparation method of coal tar pitch-based porous carbon in Example 11 and that in Example 1 is that the mass ratio of potassium tetraborate and potassium citrate in the activator in the preparation process of coal tar pitch-based porous carbon in Example 11 is 1:15.
[0045] Comparative Example 1 The only difference between the preparation method of coal tar pitch-based porous carbon in Comparative Example 1 and Example 1 is that boric acid was not added during the preparation process of coal tar pitch-based porous carbon in Comparative Example 1.
[0046] Comparative Example 2 The only difference between the preparation method of coal tar pitch-based porous carbon in Comparative Example 2 and Example 1 is that only potassium tetraborate is used as an activator in the preparation process of coal tar pitch-based porous carbon in Comparative Example 2, and the amount of potassium tetraborate added is 30g.
[0047] Comparative Example 3 The only difference between the preparation method of coal tar pitch-based porous carbon in Comparative Example 3 and Example 1 is that only potassium citrate is used as an activator in the preparation process of coal tar pitch-based porous carbon in Comparative Example 3, and the amount of potassium citrate added is 30g.
[0048] Comparative Example 4 The only difference between the preparation method of coal tar pitch-based porous carbon in Comparative Example 4 and Example 1 is that a high-temperature tube furnace is used instead of microwave air for carbonization and activation treatment in the preparation process of coal tar pitch-based porous carbon in Comparative Example 4.
[0049] The specific operating steps include: (4) Place the pretreated material in a tube furnace under a nitrogen atmosphere with a nitrogen flow rate of 40 mL / min; heat up at a rate of 10 °C / min and heat up to 500 °C for carbonization treatment for 2 hours; then heat up at a rate of 10 °C / min and heat up to 850 °C for activation treatment for 2 hours to obtain activated material. The remaining operation steps are the same as in Example 1.
[0050] Comparative Example 5 The only difference between the preparation method of coal tar pitch-based porous carbon in Comparative Example 5 and Example 1 is that sodium borate is used instead of boric acid in the preparation process of coal tar pitch-based porous carbon in Comparative Example 5.
[0051] Comparative Example 6 The only difference between the preparation method of coal tar pitch-based porous carbon in Comparative Example 6 and Example 1 is that sodium borohydride is used instead of boric acid in the preparation process of coal tar pitch-based porous carbon in Comparative Example 6.
[0052] Comparative Example 7 The only difference between the preparation method of coal tar pitch-based porous carbon in Comparative Example 7 and Example 1 is that potassium hydroxide is used instead of potassium citrate in the preparation process of coal tar pitch-based porous carbon in Comparative Example 7.
[0053] 1. Performance studies of coal tar pitch-based porous carbon described in Examples 1-11 and Comparative Examples 1-7 of this application are shown in Table 1.
[0054] Table 1
[0055] As shown in Table 1, the specific surface area of the coal tar pitch-based porous carbon in Example 1, prepared by microwave air pyrolysis, is 1921.3 m². 2 With an average pore size of 1.96 nm, a microporosity of 86%, and a sample yield of 47%, this product exhibits excellent specific surface area and pore structure. The high microporosity contributes to higher pseudocapacitance in supercapacitor applications. A comparison of Examples 1 and 3-5 reveals that using boric acid as a protective agent for carbonization activation in air is significantly effective, but the optimal addition ratio is 1:7. A comparison of Examples 1 and 6-8 shows that the optimal addition ratio of the composite activator is 1:3. A comparison of Examples 1 and 9-11 shows that the optimal ratio of potassium tetraborate to potassium citrate is 1:6.
[0056] Comparative Example 1 did not use boric acid as a vacuum flame retardant, and reacted with air during microwave pyrolysis carbonization / activation, resulting in a sample yield of only 19%. Comparative Examples 2 and 3 used only potassium tetraborate and potassium citrate as activators, which were less effective than composite activators during activation, leading to a decrease in specific surface area and a deterioration in pore structure. Comparative Example 4 used a traditional high-temperature tube furnace for carbonization / activation, but the overall time and process were relatively long. Comparative Examples 5 and 6 used other borides as protective agents, but their air isolation protection effect was less than that of boric acid, resulting in a reaction with air during carbonization / activation and a significant decrease in the pore structure parameters of the porous carbon. Comparative Example 7 used traditional KOH and potassium tetraborate to form a composite activator, but it did not generate CO2 at high temperatures to achieve the "foaming etching" effect, and did not produce more open pore structures or a higher specific surface area.
[0057] 2. Performance Study of Coal Tar Pitch-Based Porous Carbon as Described in Examples 1-11 and Comparative Examples 1-7 of this Application Cut 14mm diameter nickel foam using a punching die, and clean it with deionized water and anhydrous ethanol using ultrasonic cleaning. Weigh each piece of nickel foam and record it as m1. Weigh porous carbon (coal tar pitch-based porous carbon as described in Examples 1-11 and Comparative Examples 1-7 of this application), conductive agent, and polytetrafluoroethylene dispersion at a mass ratio of 8:1:1. Add an appropriate amount of anhydrous ethanol and grind for 30 minutes until it becomes a viscous mud. Coat 50mg of the sample evenly on the nickel foam and compact it. Vacuum dry at 80℃ for 12 hours and press it at 5MPa for 5 minutes. Weigh the prepared electrode and record it as m2. The amount of porous carbon coating is m2-m1, which is approximately 50mg.
[0058] The electrodes prepared above were used as working electrodes, Pt electrodes as counter electrodes, Hg / HgO electrodes as reference electrodes, and 6 mol / L KOH as electrolyte. The specific capacitance performance of the half-cell was tested under a current density of 0.5 A / g, and the results are shown in Table 2.
[0059] Table 2
[0060] As shown in Table 2, the specific surface area and microporosity are crucial for porous carbon as an electrode material in supercapacitors, directly affecting the current density and pseudocapacitance, thus determining the specific capacitance performance. Since Example 1 has the optimal conditions for adding boric acid, activator, and their proportions, it possesses the highest specific surface area and microporosity, resulting in higher specific capacitance performance than Examples 3-11. The higher specific capacitance of Example 1 compared to Comparative Examples 1-7 indicates that boric acid, composite activator, and air microwave carbonization / activation processes can effectively improve the properties and specific capacitance performance of porous carbon.
[0061] 3. The N2 adsorption-desorption curves and pore size distribution curves calculated based on DFT for the coal tar pitch-based porous carbon described in Example 1 and Comparative Examples 1-3 of this application are shown in the figures below. Figure 1 and Figure 2 As shown.
[0062] from Figure 1 and Figure 2 As can be seen from the data, the N2 adsorption-desorption curve of the coal tar pitch-based porous carbon described in Example 1 of this application is a typical Type I curve, indicating that the coal tar pitch-based porous carbon described in Example 1 of this application mainly has a microporous structure, with a maximum specific surface area of 1921.3 m². 2 / g, average pore size 1.96nm, microporosity 86%. This is because the porous carbon preparation process described in Example 1 uses boric acid flame retardant and potassium tetraborate / potassium citrate composite activator. Boric acid generates a molten vacuum protective barrier above 170℃, and also plays the role of template and auxiliary activation, promoting pore formation; potassium tetraborate and potassium citrate rapidly generate K2C and CO2 at high temperature, producing K + The interaction between CO2 and carbon creates a "foaming etching" effect, resulting in more open pore structures, thereby increasing the porous carbon yield and specific surface area. Therefore, the pore size and specific surface area of the samples in Comparative Examples 1-3 are significantly lower than those in Example 1.
[0063] 4. The X-ray diffraction pattern of the coal tar pitch-based porous carbon described in Example 1 of this application, as shown below. Figure 3 As shown.
[0064] from Figure 3 As can be seen from the data, the coal tar pitch-based porous carbon described in Example 1 of this application exhibits obvious porous carbon (002) and (100) characteristic diffraction peaks near 22° and 43°.
[0065] 5. The Raman spectrum of the coal tar pitch-based porous carbon described in Example 2 of this application, as follows: Figure 4 As shown.
[0066] from Figure 4 As can be seen from the image, the coal tar pitch-based porous carbon described in Example 2 of this application has a density of 1350 cm⁻¹. -1 and 1590cm -1 There are two typical D peaks and G peaks nearby, representing the defect structure and ordered structure of carbon materials, respectively.
[0067] 6. The thermogravimetric analysis curve of the coal tar pitch-based porous carbon described in Example 1 of this application, as shown... Figure 5 As shown.
[0068] from Figure 5 As can be seen from the above, the thermal decomposition temperature of the coal tar pitch-based porous carbon described in Example 1 of this application is >800℃, and it has very strong thermal stability.
[0069] 7. Scanning electron microscope image of the coal tar pitch-based porous carbon described in Example 1 of this application, as shown below. Figure 6 As shown.
[0070] from Figure 6 As can be seen from the above, the coal tar pitch-based porous carbon described in Example 1 of this application has formed an ordered porous structure.
[0071] 8. The EDS elemental mapping diagram of the coal tar pitch-based porous carbon described in Example 1 of this application, as shown below. Figure 7 As shown.
[0072] from Figure 7 As can be seen from the above, the coal tar pitch-based porous carbon described in Example 1 of this application contains C, O, and B elements.
[0073] 9. A high-magnification transmission electron microscope image of the coal tar pitch-based porous carbon described in Example 1 of this application, as shown below. Figure 8 As shown.
[0074] from Figure 8 As can be seen from the above, the coal tar pitch-based porous carbon described in Example 1 of this application has a distinct porous structure and morphology.
[0075] Although the above embodiments have been shown and described, it is understood that the above embodiments are exemplary and should not be construed as limiting the present invention. Any changes, modifications, substitutions and variations made to the above embodiments by those skilled in the art are within the protection scope of the present invention.
Claims
1. A method for preparing coal tar pitch-based porous carbon, characterized in that, Includes the following steps: (1) Mix coal tar pitch, boric acid and activator, and perform air microwave carbonization activation treatment to obtain activated material; (2) Clean and dry the activated material to obtain the coal tar pitch-based porous carbon.
2. The method for preparing coal tar pitch-based porous carbon according to claim 1, characterized in that, The coal tar pitch includes one or more of coal liquefaction pitch, coal condensate liquefaction pitch, coal tar pitch, and tar residue pitch. And / or, the coal tar pitch has an ash content of <100 ppm, a quinoline insoluble content of <100 ppm, and a magnetic content of <50 ppm.
3. The method for preparing coal tar pitch-based porous carbon according to claim 1, characterized in that, The mass ratio of the coal tar pitch to the boric acid is 1:(5-10). And / or, the mass ratio of the coal tar pitch to the activator is 1:(1-5).
4. The method for preparing coal tar pitch-based porous carbon according to claim 1, characterized in that, The activator includes potassium tetraborate and potassium citrate.
5. The method for preparing coal tar pitch-based porous carbon according to claim 4, characterized in that, The mass ratio of potassium tetraborate to potassium citrate in the activator is 1:(5-10).
6. The method for preparing coal tar pitch-based porous carbon according to claim 1, characterized in that, The microwave carbonization process has a power of 4000-6000W and a duration of 10-30 minutes. And / or, the microwave power for activation treatment is 6000-8000W, and the time is 10-30min; And / or, the atmosphere for the microwave carbonization activation treatment is an air atmosphere.
7. The method for preparing coal tar pitch-based porous carbon according to claim 1, characterized in that, In step (2), the cleaning includes sequentially cleaning with acid, deionized water and ethanol; the acid includes one or more of hydrochloric acid, sulfuric acid and nitric acid; And / or, the drying temperature is 60-80℃ and the time is 12-24h.
8. The method for preparing coal tar pitch-based porous carbon according to claim 7, characterized in that, It also includes the step of evaporating and concentrating deionized water and ethanol washing solution to obtain boric acid.
9. A coal tar pitch-based porous carbon, characterized in that, It is prepared by the method for preparing coal tar pitch-based porous carbon according to any one of claims 1-8.
10. An electrode material for a supercapacitor, characterized in that, Includes the coal tar pitch-based porous carbon as described in claim 9.