A two-dimensional silicon germanene nanomaterial, its preparation method and application

Two-dimensional silicon germanene nanomaterials prepared by chemical insertion/extraction method have solved the problems of high cost, narrow spectral absorption and low conversion efficiency of existing photothermal materials, and have achieved broad spectral absorption and high-efficiency photothermal conversion, with excellent stability and high-efficiency photothermal performance.

CN123105651APending Publication Date: 2026-11-17SHANDONG UNIV OF TECH
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611469154.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-21
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing photothermal materials have significant shortcomings in terms of cost, narrow spectral absorption range, and insufficient photothermal conversion efficiency. In particular, oxygen atoms in two-dimensional silicon germanium oxide materials affect photothermal conversion performance, and there are no experimental results to achieve the preparation of two-dimensional silicon germanium oxide alloys with precise controllable composition and stable structure.

Method used

Two-dimensional silicon-germanene nanomaterials were prepared by chemical intercalation-deintercalation method. The reaction of CaGe2xSi2(1-x) crystals with elemental iodine in an organic solvent, combined with ultrasonic treatment and centrifugation, produced two-dimensional silicon-germanene materials with tunable composition, maintaining the integrity of the crystal structure and achieving broad-spectrum absorption and high photothermal efficiency.

Benefits of technology

The prepared two-dimensional silicon germanene nanomaterials have a light absorption rate of no less than 70% in the range of 200-2500nm, a photothermal conversion efficiency of over 90%, and excellent stability. They can be irradiated with 980nm monochromatic light and the temperature rises by more than 80℃ within 1 minute. After being placed in air for 30 days, they still maintain a photothermal conversion efficiency of more than 85%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123105651A_ABST
    Figure CN123105651A_ABST
Patent Text Reader

Abstract

The present invention provides a two-dimensional silicon germanene nanomaterial, with the chemical formula Ge x Si 1‑x , wherein 0<x<1. Meanwhile, a preparation method of the two-dimensional silicon germanene nanomaterial is also disclosed, which specifically comprises: first, mixing CaGe under the protection of an inert atmosphere 2x Si 2(1‑x) crystal, elemental iodine and an organic solvent, reacting for 3 to 21 days at a temperature of 15 to 30°C, and performing suction filtration after the reaction is completed to obtain a filter cake; then washing the filter cake multiple times with an organic solvent, placing the filter cake in a dispersion liquid after washing, performing ultrasonic treatment for 1 to 8 hours at a temperature of 1 to 10°C, sequentially performing low-speed centrifugation and high-speed centrifugation after the ultrasonic treatment, collecting the precipitate after high-speed centrifugation, and finally drying the precipitate under vacuum conditions at 60 to 80°C for 12 to 24 hours to obtain the two-dimensional silicon germanene nanomaterial. The nanomaterial of the present invention can be applied to photothermal conversion materials, has high photothermal conversion efficiency, and the preparation method is simple, low in cost and easy for large-scale production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of nanomaterials technology, specifically relating to a two-dimensional silicon germanene nanomaterial, its preparation method, and its application. Background Technology

[0002] Photothermal technology, with its core advantage of converting light energy into heat energy, has become one of the key technologies in energy, environment, and biomedicine. Photothermal conversion materials are the core carriers for the development of this technology. Currently, the photothermal materials that are widely used in commercial applications and research have significant shortcomings: noble metal nanomaterials are expensive and have narrow spectral absorption ranges; the intrinsic zero bandgap of carbon-based graphene leads to insufficient photothermal conversion efficiency; and two-dimensional transition metal chalcogenides such as MoS2 have poor absorption capacity for near-infrared second window light (1000~1350nm), making them unsuitable for full-spectrum photothermal applications.

[0003] Group IV silicon and germanium semiconductors can achieve bandgap tuning through alloying, making them a research hotspot for next-generation two-dimensional functional materials. Bulk silicon-germanium alloys suffer from poor light absorption performance due to the inherent defect of indirect bandgap, limiting their applications. Existing technologies disclose a bandgap-tunable two-dimensional silicon-germanium oxide, a two-dimensional silicon-germanium material rich in hydroxyl and hydrogen groups. Its light absorption mechanism mainly targets photocatalytic reactions in the ultraviolet-visible region, but its photothermal conversion capability in the near-infrared region, especially the second biological window (1000–1350 nm), has not been studied. Furthermore, the material contains a large number of oxygen atoms, affecting its intrinsic carrier relaxation efficiency in photothermal conversion. Patent application number 202211457227.X discloses the preparation and lubrication application of pure silicene nanosheets; this technology system does not contain germanium components and does not include material design or performance optimization for photothermal scenarios.

[0004] Currently, only theoretical predictions demonstrate that two-dimensional silicon-germanene without surface groups has the potential for tunable direct bandgap. However, the tunable bandgap range is 0–0.01 eV, which is close to zero. Furthermore, there are no experimental results demonstrating the preparation of two-dimensional silicon-germanene alloys with precise compositional control and structural stability, and there are no reports of its application in the field of photothermal conversion. Existing technologies also lack two-dimensional silicon-germanium-based photothermal materials that simultaneously possess broad-spectrum absorption, near-infrared response, and high photothermal efficiency.

[0005] Therefore, developing a two-dimensional silicon germanene photothermal material that is easy to prepare, has a near-zero bandgap, and exhibits excellent photothermal conversion performance with full-spectrum absorption can effectively fill the current technological gap and has significant research value and application prospects. Summary of the Invention

[0006] The technical problem to be solved by the present invention is to address the above-mentioned deficiencies of the prior art, and provide a two-dimensional silicon germanene nanomaterial, as well as its preparation method and application. This preparation method is simple, low-cost, and easy for large-scale production. The adopted chemical deintercalation method can effectively maintain the crystal structure and integrity of the two-dimensional material. This nanomaterial has excellent photothermal conversion performance, and under the irradiation of 1W 980nm monochromatic light, the temperature rise can reach over 80°C within 1 minute, with a photothermal conversion efficiency exceeding 90%.

[0007] To solve the above technical problem, the technical solution adopted by the present invention is: a two-dimensional silicon germanene nanomaterial, characterized in that the chemical formula of the two-dimensional silicon germanene nanomaterial is Ge x Si 1-x , where 0<x<1; the two-dimensional silicon germanene nanomaterial has a six-membered honeycomb lattice structure composed of silicon atoms and germanium atoms, with a thickness of 1 to 100 nm and a lateral dimension of 50 nm to 100 μm.

[0008] Preferably, the two-dimensional silicon germanene nanomaterial has a light absorptivity of not less than 70% in the wavelength range of 200 to 2500 nm.

[0009] The present invention also provides a preparation method of the above-mentioned two-dimensional silicon germanene nanomaterial, and the preparation method is: first, under the protection of an inert atmosphere, mix CaGe 2x Si 2(1-x) crystal, elemental iodine and an organic solvent, react for 3 to 21 days at a temperature of 15 to 30°C, and perform suction filtration after the reaction is completed to obtain a filter cake; then wash the filter cake multiple times with an organic solvent, place the filter cake in a dispersion liquid after washing, perform ultrasonic treatment for 1 to 8 hours at a temperature of 1 to 10°C, sequentially perform low-speed centrifugation and high-speed centrifugation after the ultrasonic treatment is completed, collect the precipitate after high-speed centrifugation, and finally dry the precipitate for 12 to 24 hours under vacuum at 60 to 80°C to obtain the two-dimensional silicon germanene nanomaterial.

[0010] Preferably, the ratio of the CaGe 2x Si 2(1-x) crystal, elemental iodine and the organic solvent when mixed is 1 g : (2 to 4) g : (100 to 200) mL.

[0011] Preferably, the organic solvent is acetonitrile or ethanol, and the dispersion liquid is N-methylpyrrolidone, acetonitrile or ethanol.

[0012] Preferably, the power during the ultrasonic treatment is 500 to 1600 W, and the mass-to-volume ratio of the filter cake to the dispersion liquid is 1 g : (200 to 500) mL.

[0013] Preferably, the low-speed centrifugation is performed at a speed of 1000–5000 rpm for 10–30 min; the high-speed centrifugation is performed at a speed of 11000–12000 rpm for 20–40 min.

[0014] The present invention also provides an application of the above-mentioned two-dimensional silicon germanene nanomaterial, characterized in that the two-dimensional silicon germanene nanomaterial is applied to two-dimensional photothermal conversion materials.

[0015] Compared with the prior art, the present invention has the following advantages: The present invention provides a method for preparing two-dimensional silicon-germanium nanomaterials, which successfully prepares compositionally tunable two-dimensional silicon-germanium nanomaterials via a chemical intercalation-deintercalation method. This method is simple, low-cost, and easily scalable, achieving uniform alloying of silicon and germanium at the atomic scale. The two-dimensional silicon-germanium nanomaterial possesses a unique band structure and exhibits strong absorption in a broad spectral range of 200–2500 nm, with an absorption rate of no less than 70%, covering the ultraviolet, visible, near-infrared, and infrared regions. Its light absorption performance is superior to that of the widely studied MXene.

[0016] The two-dimensional silicon-germanene nanomaterial of the present invention has excellent photothermal conversion performance, and Ge 0.5 Si 0.5 Nanosheets and sodium acetate trihydrate were used to prepare a photothermal phase change thermal storage material. Under irradiation with 1W of 980nm monochromatic light, the temperature rise could reach over 80°C within 1 minute, with a photothermal conversion efficiency exceeding 90%. Furthermore, after being placed in air for 30 days, it still maintained a photothermal conversion efficiency of over 85%, demonstrating the excellent stability of the two-dimensional silicon-germanene nanomaterials prepared in this invention.

[0017] The technical solution of the present invention will be further described in detail below with reference to the accompanying drawings and embodiments. Attached Figure Description

[0018] Figure 1 The Ge prepared in Example 1 of this invention 0.5 Si 0.5 Atomic force microscopy (AFM) images of nanosheets; (a) a two-dimensional surface topography image from an AFM image; (b) a height profile image from an AFM image. Figure 2 The Ge prepared in Example 1 of this invention 0.5 Si 0.5 Transmission electron microscope image of nanosheets; Figure 3 The Ge prepared in Example 1 of this invention 0.5 Si 0.5Scanning electron microscope-energy scattering spectrometer images of nanosheets: (a) Scanning electron microscope (SEM) microstructure, (b) EDS surface distribution map of germanium (Ge), and (c) EDS surface distribution map of silicon (Si). Figure 4 The Ge prepared in Example 1 of this invention 0.5 Si 0.5 Nanosheets and Ge prepared in Example 2 0.01 Si 0.99 Nanosheets and purchased commercial Ti3C2T x -Measured UV-Vis-NIR absorption spectrum of MXene; Figure 5 The Ge prepared in Example 1 of this invention 0.5 Si 0.5 Heating curves of nanosheets under irradiation with 980nm monochromatic light of different powers; Figure 6 The Ge prepared in Example 1 of this invention 0.5 Si 0.5 Temperature rise curve of nanosheets under 1W power 980nm monochromatic light irradiation. Detailed Implementation

[0019] Example 1

[0020] The Ge disclosed in this embodiment 0.5 Si 0.5 A method for preparing nanosheets (two-dimensional silicogermanene nanomaterials) is as follows: S1. In an argon-filled glove box, 1.0 g of CaGeSi crystal powder (corresponding to x=0.5) and 3.0 g of iodine were transferred to a 250 mL round-bottom flask, and 200 mL of acetonitrile was added as a solvent. The flask was then sealed and transferred out of the glove box. The mixture was magnetically stirred at room temperature (25 °C) for 7 days. After the reaction was completed, the mixture was filtered using a sintered glass funnel to obtain 1.8 g of filter cake. The filter cake was washed three times with acetonitrile, using 50 mL of acetonitrile each time. S2. After washing the filter cake three times, transfer it to a 500mL beaker, add 300mL of N-methylpyrrolidone (NMP), place it in an ice-water bath to keep the temperature below 5℃, and simultaneously use a cell disruptor to sonicate it for 4 hours at a power of 800W to obtain a dispersion; the sonication mode of the cell disruptor is 2s of sonication followed by 1s of intermittent sonication. S3. Centrifuge the dispersion from S2 at 3000 rpm for 20 min and collect the supernatant. Then centrifuge the supernatant at 11500 rpm for 30 min, discard the supernatant, collect the precipitate, and finally place the precipitate in a vacuum drying oven and dry it under vacuum at 70℃ for 24 h to obtain dark gray Ge.0.5 Si 0.5 Nanoparticle powder.

[0021] The Ge prepared in this embodiment 0.5 Si 0.5 Nanosheets were tested: Figure 1 Ge prepared in this embodiment 0.5 Si 0.5 Atomic force microscopy (AFM) images of nanosheets, such as Figure 1 As shown, the measured values ​​of a single silicogermanene (Ge) were obtained. 0.5 Si 0.5 The thickness of the nanosheets is 1–1.3 nm, and the lateral dimension is 300–350 nm. Figure 2 This is the Ge prepared in this embodiment. 0.5 Si 0.5 Transmission electron microscopy (TEM) images of nanosheets; from Figure 2 It can be seen from Ge 0.5 Si 0.5 Nanosheets possess a complete two-dimensional planar structure and high crystallinity. Figure 3 This is the Ge prepared in this embodiment. 0.5 Si 0.5 Scanning electron microscope-energy scattering spectroscopy (SEM-EDS) images of nanosheets. Figure 3 Display Ge 0.5 Si 0.5 Silicon and germanium are evenly distributed in the nanosheets, with an element ratio of approximately 1:1, forming a two-dimensional alloy structure material.

[0022] UV-Vis-NIR absorption spectroscopy Figure 4 Display Ge 0.5 Si 0.5 Silicogerm nanosheets and Ge 0.01 Si 0.99 All silicon-germanene nanosheets exhibit broad-spectrum strong absorption in the wavelength range of 200–2500 nm, and are superior to Ti3C2T. x -MXene (commercially available) has a wider light absorption range and stronger intensity. 0.5 Si 0.5 The nanosheet material exhibits an absorption rate exceeding 80% in the 300-2500 nm range. The nanosheet material was irradiated with 980 nm monochromatic light at stepped irradiation powers of 0.47 W and 0.82 W, respectively, and the temperature change curves of the nanosheets over irradiation time were recorded using a temperature data logger to conduct photothermal performance tests. Figure 5 The results show that under irradiation with 980nm monochromatic light of different powers, Ge 0.5 Si 0.5The nanosheet materials can all heat up rapidly and reach their equilibrium temperature within 60 seconds. Under 1W power cyclic switching irradiation (… Figure 6 The material exhibits an extremely fast photothermal response, with its temperature rising from 30°C to 80°C within one minute, and demonstrates excellent cycling stability after five light-on-off cycles. Furthermore, this Ge... 0.5 Si 0.5 After the nanosheet material was placed in the air for 30 days, its photothermal performance was tested, and the calculated photothermal conversion efficiency under 980nm monochromatic light irradiation remained above 85%.

[0023] Example 2

[0024] The Ge disclosed in this embodiment 0.01 Si 0.99 A method for preparing nanosheets (two-dimensional silicogermanene nanomaterials) is as follows: S1. In a glove box filled with argon gas, place 1.0g of CaGe... 0.02 Si 1.98 The crystalline powder (corresponding to x=0.01) and 3.0g of iodine were transferred to a 250mL round-bottom flask, 150mL of ethanol was added as a solvent, and the flask was sealed and transferred out of the glove box. The reaction was carried out at room temperature (25℃) with magnetic stirring for 7 days. After the reaction was completed, the mixture was filtered using a sintered glass funnel to obtain an accurate amount of 1.8g of filter cake. The filter cake was washed three times with ethanol, each time using 50mL of ethanol. S2. After washing the filter cake three times, transfer it to a 500mL beaker, add 300mL of N-methylpyrrolidone (NMP), place it in an ice-water bath to keep the temperature below 5℃, and simultaneously use a cell disruptor to sonicate it for 4 hours at a power of 800W to obtain a dispersion; the sonication mode of the cell disruptor is 2s of sonication followed by 1s of intermittent sonication. S3. Centrifuge the dispersion from S2 at 3000 rpm for 20 min and collect the supernatant. Then centrifuge the supernatant at 11500 rpm for 30 min, discard the supernatant, collect the precipitate, and finally place the precipitate in a vacuum drying oven and dry it under vacuum at 70℃ for 24 h to obtain dark gray Ge. 0.01 Si 0.99 Nanoparticle powder.

[0025] The Ge prepared in this embodiment 0.01 Si 0.99 The nanosheet powder was subjected to atomic force microscopy, external-visible-near-infrared absorption spectroscopy, and photothermal performance tests. Atomic force microscopy (AFM) revealed Ge... 0.01 Si 0.99 The nanosheets are approximately 5–10 nm thick and have a lateral dimension of 0.8–4 μm. UV-Vis-NIR absorption spectroscopy shows that this Ge...0.01 Si 0.99 The nanosheets exhibit broad-spectrum strong absorption in the 200–2500 nm wavelength range, particularly with an absorption rate exceeding 79% in the 300–2500 nm range. Photothermal performance tests show that Ge… 0.01 Si 0.99 When irradiated with an 808nm laser, the nanosheets exhibited excellent photothermal response speed, with the material temperature rising from 25°C to 72°C within one minute. However, its final equilibrium temperature was slightly lower than that of Ge. 0.5 Si 0.5 Nanosheets.

[0026] Example 3

[0027] The Ge disclosed in this embodiment 0.2 Si 0.8 A method for preparing nanosheets (two-dimensional silicogermanene nanomaterials) is as follows: S1. In a glove box filled with argon gas, place 1.0g of CaGe... 0.4 Si 1.6 (Corresponding to x=0.2) crystalline powder and 2.0g of iodine were transferred to a 250mL round-bottom flask, 100mL of acetonitrile was added as solvent, and the flask was sealed and transferred out of the glove box. The reaction was carried out at 15℃ with magnetic stirring for 21 days. After the reaction was completed, the mixture was filtered using a sintered funnel to obtain 1.5g of filter cake. The filter cake was washed three times with acetonitrile, each time using 50mL of acetonitrile. S2. After washing the filter cake three times, transfer it to a 500mL beaker, add 200mL of acetonitrile, place it in an ice-water bath to keep the temperature below 10℃, and simultaneously use a cell disruptor to sonicate it for 8 hours at a power of 500W to obtain a dispersion; the sonication mode of the cell disruptor is 2s of sonication followed by 1s of intermittent sonication. S3. Centrifuge the dispersion from S2 at 1000 rpm for 30 min and collect the supernatant. Then centrifuge the supernatant at 11000 rpm for 40 min, discard the supernatant, collect the precipitate, and finally place the precipitate in a vacuum drying oven and dry it under vacuum at 60℃ for 24 h to obtain Ge. 0.2 Si 0.8 Nanoparticle powder.

[0028] Ge prepared in this embodiment 0.2 Si 0.8 The nanosheets exhibit broad-spectrum strong absorption in the 200–2500 nm wavelength range, particularly with an absorption rate exceeding 82% in the 300–2500 nm range. Photothermal performance tests show that Ge… 0.2 Si 0.8 When the nanosheets are irradiated with an 808nm laser, the temperature of the material rises from 25°C to 75°C within 1 minute.

[0029] Example 4

[0030] The Ge disclosed in this embodiment 0.2 Si 0.8 A method for preparing nanosheets (two-dimensional silicogermanene nanomaterials) is as follows: S1. In a glove box filled with argon gas, place 1.0g of CaGe... 0.4 Si 1.6 (Corresponding to x=0.2) The crystal powder and 4.0g of iodine were transferred to a 250mL round-bottom flask, 200mL of ethanol was added as solvent, and the flask was sealed and transferred out of the glove box. The reaction was carried out at 30℃ with magnetic stirring for 3 days. After the reaction was completed, the mixture was filtered using a sintered funnel to obtain 2g of filter cake. The filter cake was washed with ethanol 3 times, each time using 50mL of ethanol. S2. After washing the filter cake three times, transfer it to a 500mL beaker, add 500mL of ethanol, place it in an ice-water bath to keep the temperature below 5℃, and simultaneously use a cell disruptor to sonicate it for 1h at a power of 1600W to obtain a dispersion; the sonication mode of the cell disruptor is 2s of sonication followed by 1s of intermittent sonication. S3. Centrifuge the dispersion from S2 at 5000 rpm for 10 min and collect the supernatant. Then centrifuge the supernatant at 12000 rpm for 20 min, discard the supernatant, collect the precipitate, and finally place the precipitate in a vacuum drying oven and dry it under vacuum at 80℃ for 12 h to obtain Ge. 0.2 Si 0.8 Nanoparticle powder.

[0031] Ge prepared in this embodiment 0.2 Si 0.8 The nanosheets exhibit broad-spectrum strong absorption in the 200–2500 nm wavelength range, particularly with an absorption rate exceeding 77% in the 300–2500 nm range. Photothermal performance tests show that Ge… 0.2 Si 0.8 When the nanosheets are irradiated with an 808nm laser, the temperature of the material rises from 25°C to 70°C within 1 minute.

[0032] Example 5

[0033] Ge prepared in Example 1 0.5 Si 0.5 Nanosheets are composited with polyurethane (PU) foam. Specifically, Ge... 0.5 Si 0.5Nanosheets were ultrasonically dispersed in NMP solvent at a concentration of 2 mg / mL (ultrasonic power 200 W, time 30 min) to form a uniform and stable suspension; PU foam (size 2cm × 2cm × 1cm, mass approximately 0.5g) was completely immersed in the above nanosheet suspension (Ge 0.5 Si 0.5 The mass ratio of nanosheets to PU foam was approximately 1:5. The impregnation system was placed in a vacuum dryer, evacuated to -0.1 MPa and maintained for 30 minutes to fully remove residual air from the foam. This allowed the nanosheet suspension to uniformly penetrate the three-dimensional pore structure of the foam and be loaded onto the pore wall surface under pressure differential. The vacuum was then released to atmospheric pressure, allowing the suspension to further wet the deeper pores. The loaded foam was removed and transferred to a vacuum oven, where it was vacuum dried at 60°C and -0.1 MPa for 12 hours. This allowed the nanosheets to firmly adhere to the foam skeleton surface through hydrogen bonding and physical adsorption, ultimately producing a photothermal evaporator. (The last sentence appears to be incomplete and possibly refers to a solar evaporator.) 2 Under irradiation, the water evaporation rate reached 2.1 kg / m³. 2 •h, with an evaporation efficiency of 92%.

[0034] Example 6

[0035] Ge prepared in Example 1 0.5 Si 0.5 Nanosheets were composited with a phase change material at a mass percentage of 15% via melt blending. The specific method is as follows: the phase change material, sodium acetate trihydrate (SAT), was heated to melt in a water bath at 80°C; then Ge... 0.5 Si 0.5 Nanosheets were added to completely molten SAT liquid to obtain a mixture; the mixture was then continuously stirred at a constant temperature of 80°C for 8 hours, and then cooled to room temperature to obtain a photothermal phase change thermal storage composite material. This photothermal phase change thermal storage composite material exhibits performance under 1 solar intensity (1000 W / m²) 2 Under irradiation, it can rapidly heat up to the melting point of the phase change material within 1 minute, with a photothermal conversion efficiency of 91%.

[0036] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention in any way. Any simple modifications, alterations, and equivalent changes made to the above embodiments based on the inventive essence shall still fall within the protection scope of the present invention.

Claims

1. A two-dimensional silicon-germanene nanomaterial, characterized in that, The chemical formula of the two-dimensional silicon germanene nanomaterial is Ge x Si 1-x , where 0<x<1; the two-dimensional silicon germanene nanomaterial has a six-membered honeycomb lattice structure composed of silicon atoms and germanium atoms, with a thickness of 1 to 100 nm and a lateral dimension of 50 nm to 100 μm.

2. The two-dimensional silicon-germanene nanomaterial according to claim 1, characterized in that, The two-dimensional silicon germanene nanomaterial has a light absorption rate of not less than 70% in the wavelength range of 200 to 2500 nm.

3. A method for preparing two-dimensional silicon-germanene nanomaterials as described in claim 1 or 2, characterized in that, The preparation method includes the following steps: First, under an inert atmosphere, CaGe... 2x Si 2(1-x) Crystals, elemental iodine, and an organic solvent are mixed and reacted at 15–30°C for 3–21 days. After the reaction is complete, the mixture is filtered to obtain a filter cake. The filter cake is then washed multiple times with the organic solvent. After washing, the filter cake is placed in a dispersion and ultrasonically treated at 1–10°C for 1–8 hours. After ultrasonic treatment, the mixture is then centrifuged at low speed and high speed. The precipitate after high-speed centrifugation is collected. Finally, the precipitate is dried under vacuum at 60–80°C for 12–24 hours to obtain two-dimensional silicon germanene nanomaterials.

4. The preparation method according to claim 3, characterized in that, The CaGe 2x Si 2(1-x) The ratio of crystal, iodine and organic solvent is 1g : (2-4)g : (100-200)mL.

5. The preparation method according to claim 3 or 4, characterized in that, The organic solvent is acetonitrile or ethanol, and the dispersion is N-methylpyrrolidone, acetonitrile, or ethanol.

6. The preparation method according to claim 3, characterized in that, The ultrasonic treatment power is 500-1600W, and the mass-to-volume ratio of the filter cake to the dispersion is 1g:(200-500)mL.

7. The preparation method according to claim 3, characterized in that, The low-speed centrifugation is performed at a speed of 1000–5000 rpm for 10–30 min; the high-speed centrifugation is performed at a speed of 11000–12000 rpm for 20–40 min.

8. An application of the two-dimensional silicogermanene nanomaterial as described in claim 1 or 2, characterized in that, The two-dimensional silicon germanene nanomaterial is applied to two-dimensional photothermal conversion materials.

Citation Information

Patent Citations

  • Silylene nanosheet for lubricant as well as preparation method and application of silylene nanosheet

    CN115744910A