A method for recovering phosphorus and fluorine and producing high-purity dihydrate gypsum as a byproduct via a hemihydrate-dihydrate process.
Through improvements to the hemihydrate-dihydrate process, deep recovery of phosphorus and fluorine resources and high-purity preparation of dihydrate gypsum have been achieved, solving the problems of low utilization rate of phosphorus and fluorine resources and poor gypsum quality in existing technologies, and improving the economic benefits and product stability of production.
Patent Information
- Application Number
- CN202611515875.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-28
- Publication Date
- 2026-11-17
AI Technical Summary
The existing hemihydrate-dihydrate process has insufficient phosphorus and fluorine resource recovery rate, poor quality of dihydrate gypsum, high acid consumption, and unstable product concentration.
The process involves hemihydrate acid hydrolysis, fluorine recovery, slurry treatment, and hydration recrystallization to achieve deep recovery of phosphorus and fluorine resources. The purity of dihydrate gypsum is improved through crystal growth technology, and a two-stage acid return system is used to optimize the acid hydrolysis and dissolution process and control the acid concentration to reduce sulfuric acid consumption.
It achieves efficient recovery of phosphorus and fluorine resources, and the purity of dihydrate gypsum reaches 98%, meeting the requirements of high value-added applications, reducing acid consumption, improving production stability, and diversifying product output.
Smart Images

Figure CN123105652A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of wet-process phosphoric acid production technology, specifically to a method for recovering phosphorus and fluorine and producing high-purity dihydrate gypsum as a byproduct using a hemihydrate-dihydrate process. Background Technology
[0002] Wet-process phosphoric acid is a phosphoric acid product obtained by decomposing phosphate rock powder with strong acids such as sulfuric acid, using medium- and low-grade phosphate rock as raw material. Since my country's phosphate rock is mainly of medium- and low-grade grade, domestic phosphoric acid production currently relies primarily on the wet-process method.
[0003] The main wet-process phosphoric acid production technologies include the hemihydrate process, the dihydrate process, and the hemihydrate-dihydrate process. The main chemical component of phosphate rock is Ca5F(PO4)3, which reacts with sulfuric acid to produce phosphoric acid and insoluble calcium sulfate crystals. The chemical reaction formula is as follows:
[0004] When reaction temperature, sulfuric acid dosage, and other conditions vary, calcium sulfate precipitates in three different crystalline forms: calcium sulfate dihydrate (CaSO4·2H2O), calcium sulfate hemihydrate (CaSO4·1 / 2H2O), and anhydrous calcium sulfate (CaSO4). The hemihydrate-dihydrate process involves controlling reaction conditions to first crystallize calcium sulfate hemihydrate, simultaneously producing high-concentration phosphoric acid. Then, the reaction conditions are changed to hydrate and recrystallize the calcium sulfate hemihydrate back into calcium sulfate dihydrate.
[0005] The hemihydrate-dihydrate process has become the preferred process for wet-process phosphoric acid production because it combines the advantages of high-concentration phosphoric acid production from the hemihydrate process with the advantages of easy crystallization and filtration of gypsum from the dihydrate process. However, the existing hemihydrate-dihydrate process still has the following drawbacks: (1) Insufficient recovery rate of phosphorus and fluorine resources: During the hemihydrate acid hydrolysis process, fluorine in phosphate rock escapes as silicon tetrafluoride gas. Traditional processes simply absorb it, resulting in low utilization of fluorine resources. At the same time, free phosphoric acid, eutectic phosphorus, intercrystalline fluorine and undecomposed phosphate rock entrained in hemihydrate phosphogypsum are not fully recovered, resulting in waste of phosphorus and fluorine resources.
[0006] (2) Poor quality of by-product gypsum: Due to the presence of impurities such as free phosphoric acid, eutectic phosphorus, water-soluble fluorine, and intercrystalline fluorine in hemihydrate phosphogypsum, the dihydrate gypsum produced by hydration and recrystallization of hemihydrate phosphogypsum not only has a high impurity content (excessive phosphorus, fluorine, and acid insoluble matter), but can only be used as a low-value-added building material raw material. It cannot meet the requirements of high-value-added fields such as gypsum building materials and medical gypsum. Moreover, the crystals are small and the aspect ratio is high, resulting in the dihydrate gypsum slurry being viscous, having poor fluidity, and poor filtration and washing effect.
[0007] (3) High acid consumption and unstable product concentration: The design of the acid return system is unreasonable, resulting in high sulfuric acid consumption and large fluctuations in the concentration of phosphoric acid in the product, which affects the production stability of subsequent phosphate products. Summary of the Invention
[0008] In view of this, the purpose of this invention is to provide a method for recovering phosphorus and fluorine and producing high-purity gypsum dihydrate as a byproduct using a hemihydrate-dihydrate process, which aims to solve the problems of low phosphorus and fluorine recovery efficiency, poor quality of gypsum dihydrate, high acid consumption, and unstable product concentration in existing hemihydrate-dihydrate processes.
[0009] To achieve the above objectives, the present invention provides a method for recovering phosphorus and fluorine and producing high-purity dihydrate gypsum as a byproduct via a hemihydrate-dihydrate process, the method comprising the following steps: (1) Hemihydrate acid hydrolysis reaction process: Phosphate rock powder and first acid solution are mixed at a mass ratio of 1:(2.5~3.5), and acid hydrolysis reaction is carried out at a temperature of 95~105℃ to obtain first slurry and silicon tetrafluoride gas; the first acid solution includes concentrated sulfuric acid solution, phosphoric acid back acid and phosphoric acid mixed acid, and the SO3 concentration of the first acid solution is controlled at 0.5~2wt%; (2) Fluorine recovery process: The silicon tetrafluoride gas is introduced into the absorption tank and reacted with the absorbent to obtain a fluorosilicic acid solution; the absorbent includes water and dilute fluorosilicic acid solution; (3) First slurry treatment process: The first slurry is filtered and washed by a belt vacuum filter to obtain the first filtrate and the first filter cake. The first filtrate is divided into two parts: phosphoric acid back acid and product phosphoric acid. The phosphoric acid back acid is used as the first acid solution in the hemihydrate acid hydrolysis reaction process. (4) Hydration and recrystallization process: The first filter cake and the second acid solution are mixed at a mass ratio of 1:(2.5-4), and the first filter cake is dissolved in the second acid solution at a temperature of 60-75°C to obtain the second slurry; the second acid solution includes aluminum sulfate solution, concentrated sulfuric acid solution, fluoride solution and dissolution back acid, and the SO3 concentration, aluminum sulfate concentration and fluoride ion concentration of the second acid solution are controlled to be 0.5-5wt%; (5) Gypsum dihydrate crystal growth process: Add concentrated sulfuric acid solution to the second slurry, control the SO3 concentration in the liquid phase to 0.5-5wt%, and carry out crystal growth at a temperature of 60-75℃ until the crystal particle size d50≥80μm to obtain the third slurry; (6) Third slurry treatment process: The third slurry is filtered and washed by a belt vacuum filter to obtain the second filtrate and gypsum dihydrate filter cake. The second filtrate is divided into two parts: phosphorus and fluorine mixed acid and dissolution and return acid. The phosphorus and fluorine mixed acid is used as the first acid solution in the hemihydrate acid hydrolysis reaction process, and the dissolution and return acid is used as the second acid solution in the hydration and recrystallization process.
[0010] In the above method, the present invention first realizes the recycling of fluorine resources through a fluorine recovery process; then, the first filter cake, which is mainly composed of hemihydrate phosphogypsum, is dissolved in the second acid solution to fully dissolve the hemihydrate phosphogypsum and undecomposed phosphate rock, releasing the free phosphoric acid, eutectic phosphorus, intercrystalline fluorine, and water-soluble fluorine entrained therein, thus completing the secondary recovery of phosphorus and fluorine resources. This invention returns the slurry filtrate to be used as acid in the hemihydrate acid hydrolysis and hydration recrystallization processes, reducing the amount of raw acid used and lowering acid consumption. The second filtrate is a fluorinated filtrate acid, which is divided into two parts and introduced into the hemihydrate acid hydrolysis and hydration recrystallization processes respectively. On one hand, introducing the second filtrate into the hemihydrate acid hydrolysis process significantly improves the strength properties of hemihydrate phosphogypsum. On the other hand, it avoids a significant increase in fluoride ion concentration in the acid during the hydration recrystallization process, which would inhibit the hydration of hemihydrate phosphogypsum and prevent the purification of dihydrate gypsum. Furthermore, the fluorosilicic acid ions in the fluorinated filtrate acid introduced into the hemihydrate acid hydrolysis process react with sulfuric acid to form silicon tetrafluoride gas, which, after absorption, forms fluorosilicic acid products. This ensures the stability of the liquid phase parameters in the hemihydrate acid hydrolysis process, allowing the hemihydrate phosphogypsum to maintain good gel strength.
[0011] Furthermore, the first filtrate contains 10-40 wt% phosphoric acid reversion, with the remainder being the product phosphoric acid.
[0012] Furthermore, the second filtrate contains 20-40 wt% phosphorus-fluorine mixed acid, with the remainder being dissolved acid.
[0013] Furthermore, the phosphate rock powder has a P2O5 content of ≥27wt% and a fineness of ≥90% of 100 mesh.
[0014] Furthermore, the concentrated sulfuric acid solution contains ≥98% sulfuric acid by mass.
[0015] Furthermore, the content of fluorosilicic acid in the dilute fluorosilicic acid solution is ≤10wt%.
[0016] Furthermore, the fluorinated acid solution includes at least one of fluorosilicic acid, hydrofluoric acid, fluoroboric acid, fluoroantimonic acid, fluoroplatinic acid, fluorosulfonic acid, and fluorochloric acid.
[0017] Furthermore, the acidolysis reaction time in the hemihydrate acidolysis reaction process is 2-3 hours, the dissolution time in the hydration recrystallization process is 2-3 hours, and the crystal growth time in the dihydrate gypsum crystal growth process is 1-2 hours.
[0018] Furthermore, the temperature at which the absorbent absorbs the silicon tetrafluoride gas is controlled between 30 and 50°C.
[0019] Furthermore, the washing program of the belt vacuum filter is 3-4 stages of countercurrent washing, the washing water is desalinated water, and the water content of the filter cake is <20wt%.
[0020] Compared with the prior art, the present invention has the following beneficial effects: (1) High-efficiency recovery of phosphorus and fluorine resources: Through the two-stage process of "phosphate rock acid hydrolysis + hemihydrate phosphogypsum dissolution", the deep recovery of phosphorus and fluorine resources is achieved, with a total phosphorus recovery rate of ≥99%; at the same time, a separate fluorine absorption unit is set up to convert silicon tetrafluoride gas into fluorosilicic acid products, with a fluorine recovery rate of ≥95%, which greatly improves the resource utilization rate.
[0021] (2) The quality of by-product dihydrate gypsum is greatly improved: First, the free phosphoric acid, eutectic phosphorus, intercrystalline fluorine and water-soluble fluorine entrained in the first filter cake are released by dissolving the first filter cake. Then, combined with the crystal growth process, not only are impurities such as phosphorus and fluorine in dihydrate gypsum effectively removed, but the high-purity dihydrate gypsum produced has a purity of ≥98%, which meets the requirements of high value-added applications, realizes the resource utilization of phosphogypsum, and solves the environmental protection problem of stockpiling. Moreover, the prepared dihydrate calcium sulfate crystals are large and the slurry has good fluidity, which is conducive to filtration and washing.
[0022] (3) Strong process stability and low acid consumption: Through the closed-loop design of the two-stage acid return system, the acid concentration control of the acid hydrolysis and dissolution process is optimized, the sulfuric acid consumption is reduced, and the phosphoric acid concentration of the product is stabilized, thereby improving the operational stability of the production system.
[0023] (4) Product diversification: Simultaneously produce three products: high-concentration phosphoric acid, fluorosilicic acid, and high-purity dihydrate gypsum, thereby improving the economic benefits of wet-process phosphoric acid production and expanding product application scenarios. Attached Figure Description
[0024] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on the provided drawings without creative effort.
[0025] Figure 1 A schematic flow diagram of the process method provided by the present invention; Figure 2 SEM images of hemihydrate phosphogypsum prepared in Examples 1 to 6 of this invention (in the images, EHT=1.00Kv, WD=5.0mm, Mag=1.00KX, Signa A=SE2, scale bar is 10μm). Figure 3The images show SEM images of the gypsum dihydrate prepared in Examples 1 to 6 of this invention (in the images, EHT=3.00Kv, WD=6.6mm, Mag=1.00KX, Signa A=SE2, scale bar is 10μm for Examples 1, 3, and 4; EHT=3.00Kv, WD=6.4mm, Mag=3.00KX, Signa A=SE2, scale bar is 3μm for Example 2; EHT=1.00Kv, WD=5.0mm, Mag=3.00KX, Signa A=SE2, scale bar is 3μm for Examples 5 and 6). Specific implementation methods
[0026] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0027] See Figure 1 This invention provides a method for recovering phosphorus and fluorine and producing high-purity gypsum dihydrate as a byproduct using a hemihydrate-dihydrate process, the method comprising the following steps: (1) Hemihydrate acid hydrolysis reaction process: Phosphate rock powder and the first acid solution are added to the hemihydrate acid hydrolysis tank at a mass ratio of 1:(2.5~3.5) and mixed. The acid hydrolysis reaction is carried out at a temperature of 95~105℃ to obtain the first slurry (main components: hemihydrate phosphogypsum and phosphoric acid) and silicon tetrafluoride gas; the first acid solution includes concentrated sulfuric acid solution, phosphoric acid back acid and phosphoric acid mixed acid, and the SO3 concentration of the first acid solution is controlled at 0.5~2wt%; (2) Fluorine recovery process: Silicon tetrafluoride gas escaping from the hemihydrate acid hydrolysis tank is introduced into the absorption tank and reacted with the absorbent (water and / or dilute fluorosilicic acid solution) to obtain fluorosilicic acid solution. The fluorosilicic acid solution is concentrated to obtain fluorosilicic acid product of the required concentration, thereby realizing the recovery and utilization of fluorine resources. (3) First slurry treatment process: The first slurry produced by the hemihydrate acid hydrolysis tank is sent to the first-stage filtration and washing unit (belt vacuum filter) for filtration and washing to obtain the first filtrate and the first filter cake (main component: hemihydrate phosphogypsum). The first filtrate is divided into two parts: phosphoric acid back acid and product phosphoric acid. The phosphoric acid back acid is used as the first acid solution in the hemihydrate acid hydrolysis reaction process; the first filter cake is used as the raw material for converting high-purity dihydrate gypsum. (4) Hydration and recrystallization process: The first filter cake is sent into the dihydrate dissolution tank, and the second acid solution is added to the dihydrate dissolution tank. The second acid solution includes aluminum sulfate solution, concentrated sulfuric acid solution, fluoride solution and dissolution back acid. The SO3 concentration, aluminum sulfate concentration and fluoride ion concentration of the second acid solution are controlled at 0.5-5 wt% and 0.5-5 wt%, respectively. Under the conditions of controlled temperature of 60-75℃ and solid-liquid ratio of 1: (2.5-4), the first filter cake is dissolved in the second acid solution to obtain the second slurry. In this process, the hemihydrate phosphogypsum and undecomposed phosphate rock of the first filter cake are fully dissolved, releasing the entrained free phosphoric acid, eutectic phosphorus, intercrystalline fluorine and water-soluble fluorine, thus completing the secondary recovery of phosphorus and fluorine resources. (5) Gypsum dihydrate crystal growth process: The second slurry from the dihydrate dissolving tank is fed into the dihydrate crystal growth tank. Concentrated sulfuric acid solution is added to the dihydrate crystal growth tank to control the concentration of SO3 in the liquid phase to 0.5-5wt%, which further promotes the dissolution of a small amount of undecomposed ore and hemihydrate phosphogypsum. Crystal growth is carried out under the condition of controlling the temperature to 60-75℃, so that the dissolved calcium sulfate is converted into coarse and uniform calcium sulfate dihydrate crystals, reducing the amount of crystal impurities. Crystal growth is carried out until the crystal particle size d50≥80μm, and the third slurry is obtained. (6) Third slurry treatment process: The third slurry produced from the dihydrate crystal growth tank is sent to the second-stage filtration and washing unit (belt vacuum filter) for filtration and washing to obtain the second filtrate and dihydrate gypsum filter cake. The second filtrate is divided into two parts: phosphorus-fluorine mixed acid and dissolution back acid. The phosphorus-fluorine mixed acid is returned to the hemihydrate acid hydrolysis tank as the first acid solution, and the dissolution back acid is returned to the dihydrate dissolution tank as the second acid solution. The dihydrate gypsum filter cake, which has been thoroughly washed by the belt vacuum filter, has a purity ≥98%, a phosphorus content ≤0.1%, and a fluorine content ≤0.1%, meeting the application requirements of high-value-added fields such as gypsum building materials and medical gypsum.
[0028] Preferably, the proportion of phosphoric acid reversion in the first filtrate is 10-40 wt%, with the remainder being the product phosphoric acid.
[0029] Preferably, the proportion of phosphoric acid-fluorine mixture in the second filtrate is 10-40 wt%, with the remainder being dissolved acid.
[0030] Preferably, the phosphate rock powder has a P2O5 content of ≥27wt% and a fineness of ≥90% of 100 mesh.
[0031] Preferably, the concentrated sulfuric acid solution contains ≥98% sulfuric acid by mass.
[0032] Preferably, the content of fluorosilicic acid in the dilute fluorosilicic acid solution is ≤10wt%.
[0033] Preferably, the fluorinated acid solution includes at least one of fluorosilicic acid, hydrofluoric acid, fluoroboric acid, fluoroantimonic acid, fluoroplatinic acid, fluorosulfonic acid, and fluorochloric acid.
[0034] Preferably, the acid hydrolysis reaction time in the hemihydrate acid hydrolysis reaction process is 2-3 hours, the dissolution time in the hydration recrystallization process is 2-3 hours, and the crystal growth time in the dihydrate gypsum crystal growth process is 1-2 hours.
[0035] Preferably, the temperature at which the absorbent absorbs the silicon tetrafluoride gas is controlled at 30–50°C.
[0036] Preferably, the washing program of the belt vacuum filter is 3-4 stages of countercurrent washing, the washing water is desalinated water, and the water content of the filter cake is <20wt%.
[0037] Example 1: Production of wet-process phosphoric acid according to the method described above: (1) Phosphate rock acid hydrolysis: Phosphate rock powder (P2O5 content of 32wt%, fineness: 100 mesh accounting for 95%) and the first acid solution are added to the hemihydrate acid hydrolysis tank at a solid-liquid ratio of 1:3. The reaction temperature is controlled at 100℃ and the reaction time is 2h. The first slurry is produced and silicon tetrafluoride gas is released at the same time. The first acid solution includes 98% industrial sulfuric acid, phosphoric acid back acid and phosphoric acid mixed acid. The SO3 concentration of the first acid solution is controlled at 1wt%. (2) Fluorine absorption: Silicon tetrafluoride gas is introduced into the absorption tank and absorbed by process water. The absorption temperature is controlled at 40°C to obtain a fluorosilicic acid solution with a mass fraction of 22%. The solution is concentrated to 35% to obtain the fluorosilicic acid product with a fluorine recovery rate of 96%.
[0038] (3) First slurry filtration: The first slurry is fed into a belt vacuum filter for solid-liquid separation: 60% of the filtrate is output as phosphoric acid, and the remaining filtrate is returned to the hemihydrate acid hydrolysis tank as phosphoric acid back acid; the filter cake is hemihydrate phosphogypsum, which is washed countercurrently by the belt vacuum filter and used as raw material for the production of high-purity dihydrate gypsum.
[0039] (4) Hydration and recrystallization: The hemihydrate phosphogypsum is fed into the dihydrate dissolving tank, and the second acid solution is added at a solid-liquid ratio of 1:3. The temperature is controlled at 65°C and the residence time is 2 hours to completely dissolve the hemihydrate phosphogypsum and recover the entrained phosphorus and fluorine resources to obtain the second slurry. The second acid solution includes 10% aluminum sulfate solution, 98% industrial sulfuric acid, 35% fluorosilicic acid solution and dissolution back acid. The SO3 concentration, aluminum sulfate concentration, and fluoride ion concentration of the second acid solution are controlled at 3wt%, 2wt%, and 2wt%, respectively. (5) Gypsum dihydrate crystal growth: The second slurry is fed into the dihydrate crystal growth tank, 98% industrial sulfuric acid is added, the concentration of SO3 in the liquid phase is controlled at 3%, the temperature is controlled at 65℃, and the residence time is 1h to generate coarse gypsum dihydrate crystals (crystal particle size D50 is 90μm) to obtain the third slurry; (6) Third slurry filtration: The third slurry is fed into a belt vacuum filter for solid-liquid separation: 60% of the filtrate is returned to the dihydrate dissolution tank as a dissolving acid, and 40% of the filtrate is circulated to the hemihydrate acid hydrolysis tank as the first acid solution; the filter cake is washed by the four-stage countercurrent deionized water of the belt vacuum filter and dried to obtain a high-purity dihydrate gypsum product. After testing, the purity is 98.5%, the total phosphorus content is 0.1%, the fluorine content is 0.08%, and the attached water content is 15%, which meets the requirements of GB / T 23456-2025 "Phosphogypsum" Grade I and GB / T 9776-2022 "Gypsum Building Materials" Superior Grade, and can be used in the fields of paper-faced gypsum board and building gypsum.
[0040] Example 2: Same as Example 1, except that: 50% of the filtrate from the third slurry filtration is returned to the dihydrate dissolution tank as a dissolving acid, and 50% is circulated to the hemihydrate acid hydrolysis tank as a phosphorus and fluorine mixed acid.
[0041] Example 3: Same as Example 1, except that: 70% of the filtrate from the third slurry filtration is returned to the dihydrate dissolution tank as a dissolving acid, and 30% is circulated to the hemihydrate acid hydrolysis tank as a phosphorus and fluorine mixed acid.
[0042] Example 4: Same as Example 1, except that 80% of the filtrate from the third slurry filtration is returned to the dihydrate dissolution tank as a dissolving acid, and 20% is circulated to the hemihydrate acid hydrolysis tank as a phosphorus and fluorine mixed acid.
[0043] Example 5: Same as Example 1, except that 90% of the filtrate from the third slurry filtration is returned to the dihydrate dissolution tank as a dissolving acid, and 10% is circulated to the hemihydrate acid hydrolysis tank as a phosphorus-fluorine mixed acid.
[0044] Example 6: Same as Example 1, except that: all the filtrate from the third slurry filtration is used as a dissolving acid and returned to the dihydrate dissolving tank.
[0045] The morphology of the hemihydrate phosphogypsum and dihydrate gypsum prepared in the above examples was observed using scanning electron microscopy. (See [link to relevant documentation]). Figure 2 , Figure 3 As shown in Table 1, the strength properties of hemihydrate phosphogypsum were tested according to the requirements of the national standard GB / T 9776-2022 "Building Gypsum". The chemical composition of dihydrate gypsum was tested according to the requirements of the national standard GB / T 23456-2025 "Phosphogypsum". The results are shown in Table 2.
[0046] Table 1. Strength properties of hemihydrate phosphogypsum
[0047] Table 2. Chemical composition of gypsum dihydrate
[0048] The second filtrate from the third slurry filtration is fluorine-containing filtrate acid (phosphoric and fluorine mixed acid + dissolution back acid). In Example 6, the fluorine-containing filtrate acid was not introduced into the hemihydrate acidolysis reaction process, but was entirely recycled back to the dihydrate dissolution tank as dissolution back acid for the hydration and recrystallization of hemihydrate phosphogypsum into dihydrate gypsum. In Examples 1-5, however, a portion of the fluorine-containing filtrate acid was introduced into the hemihydrate acidolysis reaction process as phosphoric and fluorine mixed acid.
[0049] See Figure 2 The morphology of hemihydrate phosphogypsum shown is as follows: the hemihydrate phosphogypsum in Examples 1-5 exhibits spheroidal crystals, while the microstructure of hemihydrate phosphogypsum in Example 6 exhibits irregular flaky polycrystals. This indicates that after introducing fluorinated filtrate acid into the hemihydrate acid hydrolysis reaction process, fluorine will be adsorbed on the (400) crystal surface of the hemihydrate phosphogypsum crystal nucleus, thereby controlling the original flaky polycrystals into spheroidal polycrystals with higher crystallinity and smoother and flatter surfaces. In addition, the fluorosilicic acid ions in the introduced fluorinated filtrate acid will also react with sulfuric acid to form silicon tetrafluoride gas, which can be absorbed to form fluorosilicic acid products, ensuring the stability of the liquid phase indicators in the hemihydrate process, so that the hemihydrate phosphogypsum can maintain good gel strength.
[0050] from Figure 3 As can be seen, the gypsum dihydrate in Examples 1-5 has a regular hexagonal morphology with a smooth and flat crystal surface, while the gypsum dihydrate in Example 6 has an irregular blocky morphology. This is because F ions in the liquid phase have extremely strong electronegativity. When the mass ratio of phosphoric acid and fluorine mixed acid in the second filtrate is 10-50% (Examples 1-5), the enrichment of F content in the second acid liquid phase is more suitable, and F may be completely adsorbed on the (111) crystal face. At this time, the gypsum dihydrate has a regular hexagonal morphology with a smooth and flat crystal surface. When the mass ratio of phosphoric acid and fluorine mixed acid in the second filtrate exceeds 50%, the F content in the liquid phase of the second acid solution is too high. After F is completely adsorbed on the (111) crystal surface of the gypsum dihydrate crystal, it may also be adsorbed on the (120) crystal surface and the (110) crystal surface, and the adsorption is uneven, which seriously interferes with the normal growth of each crystal surface, resulting in defects on the crystal surface, blurred crystal surface outline, and significant changes in the crystal form of gypsum dihydrate, presenting an irregular blocky morphology, and greatly reducing the filtration and washing performance of gypsum dihydrate.
[0051] Referring to the composition data of gypsum dihydrate shown in Table 2, if all the fluoride-containing filtrate acid is recycled back to the dihydrate dissolution tank, the fluoride concentration in the second acid solution will increase significantly, inhibiting the hydration of hemihydrate phosphogypsum. This will prevent the crystal water content of the dihydrate gypsum from reaching 20%, and a crystal water content of 15.78% will cause the dihydrate gypsum product to clump. Furthermore, the fluoride content will result in excessively high levels of other impurities, making it impossible to achieve the desired purification of dihydrate gypsum. However, by separating a portion of the fluoride-containing filtrate acid and introducing it as a mixed phosphofluoride acid into the hemihydrate acidolysis reaction process, the fluoride content in the second acid solution is effectively reduced to a suitable range, making it easier to prepare a dihydrate gypsum product with low impurity content and high purity. Combining the strength performance data in Table 1 and the index data in Table 2, the mass percentage of the mixed phosphofluoride acid in the second filtrate should ideally be 20-40%.
[0052] In summary, fluorine plays a crucial role in the crystallization of gypsum dihydrate. If the fluorine concentration in the second acid solution is too high, it will delay the hydration of hemihydrate phosphogypsum, resulting in excessively high P and F impurity content in the gypsum dihydrate product. Therefore, it is necessary to return part of the mixed acid containing fluorosilicate ions, phosphoric acid and free sulfuric acid in the gypsum dihydrate slurry phase to the front-end hemihydrate acidolysis reaction process. At the same time, introducing fluorine-containing filtrate acid into the hemihydrate acidolysis reaction process has the following advantages: (1) Fluorine-containing acid can promote better crystallization of hemihydrate phosphogypsum, giving it better gelling properties. On the other hand, after its reaction with sulfuric acid, The formation of silicon tetrafluoride gas, after absorption, can form fluorosilicic acid products, while also ensuring the stability of liquid phase indicators, so that hemihydrate phosphogypsum can maintain good gel strength; (2) The introduction of fluorine-containing filtrate acid into the hemihydrate acid hydrolysis reaction process can reduce the sulfate concentration in the first acid solution. The low concentration of free sulfuric acid can promote the decomposition of phosphate concentrate, effectively avoiding the problem of excessive sulfate in the liquid phase encapsulating the ore and seriously affecting the phosphorus recovery rate caused by directly adding concentrated sulfuric acid; (3) The low concentration of phosphoric acid in the first acid solution is mixed with the high concentration of phosphoric acid in the hemihydrate system and then concentratedly produced from the product acid outlet, avoiding the waste of phosphoric acid.
[0053] The above are merely preferred embodiments of the present invention. It should be noted that the above preferred embodiments should not be considered as limitations on the present invention, and the scope of protection of the present invention should be determined by the scope defined in the claims. For those skilled in the art, any improvements and modifications made based on the core ideas of the present invention without departing from the spirit and scope of the present invention should be considered within the scope of protection of the present invention.
Claims
1. A method for recovering phosphorus and fluorine and producing high-purity gypsum dihydrate as a byproduct via a hemihydrate-dihydrate process, characterized in that: The method includes the following steps: (1) Hemihydrate acid hydrolysis reaction process: Phosphate rock powder and first acid solution are mixed at a mass ratio of 1:(2.5~3.5), and acid hydrolysis reaction is carried out at a temperature of 95~105℃ to obtain first slurry and silicon tetrafluoride gas; the first acid solution includes concentrated sulfuric acid solution, phosphoric acid back acid and phosphoric acid mixed acid, and the SO3 concentration of the first acid solution is controlled at 0.5~2wt%; (2) Fluorine recovery process: The silicon tetrafluoride gas is introduced into the absorption tank and reacted with the absorbent to obtain a fluorosilicic acid solution; the absorbent includes water and dilute fluorosilicic acid solution; (3) First slurry treatment process: The first slurry is filtered and washed by a belt vacuum filter to obtain the first filtrate and the first filter cake. The first filtrate is divided into two parts: phosphoric acid back acid and product phosphoric acid. The phosphoric acid back acid is used as the first acid solution in the hemihydrate acid hydrolysis reaction process. (4) Hydration and recrystallization process: The first filter cake and the second acid solution are mixed at a mass ratio of 1:(2.5-4), and the first filter cake is dissolved in the second acid solution at a temperature of 60-75°C to obtain the second slurry; the second acid solution includes aluminum sulfate solution, concentrated sulfuric acid solution, fluoride solution and dissolution back acid, and the SO3 concentration, aluminum sulfate concentration and fluoride ion concentration of the second acid solution are controlled to be 0.5-5wt%; (5) Gypsum dihydrate crystal growth process: Add concentrated sulfuric acid solution to the second slurry, control the SO3 concentration in the liquid phase to 0.5-5wt%, and carry out crystal growth at a temperature of 60-75℃ until the crystal particle size d50≥80μm to obtain the third slurry; (6) Third slurry treatment process: The third slurry is filtered and washed by a belt vacuum filter to obtain the second filtrate and gypsum dihydrate filter cake. The second filtrate is divided into two parts: phosphorus and fluorine mixed acid and dissolution and return acid. The phosphorus and fluorine mixed acid is used as the first acid solution in the hemihydrate acid hydrolysis reaction process, and the dissolution and return acid is used as the second acid solution in the hydration and recrystallization process.
2. The method for recovering phosphorus and fluorine and producing high-purity gypsum dihydrate as a byproduct using a hemihydrate-dihydrate process according to claim 1, characterized in that: The first filtrate contains 10-40 wt% phosphoric acid reversion, with the remainder being the product phosphoric acid.
3. The method for recovering phosphorus and fluorine and producing high-purity gypsum dihydrate as a byproduct using a hemihydrate-dihydrate process according to claim 1, characterized in that: The second filtrate contains 20-40 wt% phosphorus-fluorine mixed acid, with the remainder being dissolved acid.
4. The method for recovering phosphorus and fluorine and producing high-purity gypsum dihydrate as a byproduct using a hemihydrate-dihydrate process according to claim 1, characterized in that: The phosphate rock powder has a P2O5 content of ≥27wt% and a fineness of ≥90% of 100 mesh.
5. The method for recovering phosphorus and fluorine and producing high-purity gypsum dihydrate as a byproduct using a hemihydrate-dihydrate process according to claim 1, characterized in that: The concentrated sulfuric acid solution contains ≥98% sulfuric acid by mass.
6. The method for recovering phosphorus and fluorine and producing high-purity gypsum dihydrate as a byproduct using a hemihydrate-dihydrate process according to claim 1, characterized in that: The content of fluorosilicic acid in the dilute fluorosilicic acid solution is ≤10wt%.
7. The method for recovering phosphorus and fluorine and producing high-purity gypsum dihydrate as a byproduct using a hemihydrate-dihydrate process according to claim 1, characterized in that: The fluorinated acid solution includes at least one of fluorosilicic acid, hydrofluoric acid, fluoroboric acid, fluoroantimonic acid, fluoroplatinic acid, fluorosulfonic acid, and fluorochloroic acid.
8. The method for recovering phosphorus and fluorine and producing high-purity gypsum dihydrate as a byproduct using a hemihydrate-dihydrate process according to claim 1, characterized in that: The acidolysis reaction time in the hemihydrate acidolysis reaction process is 2-3 hours, the dissolution time in the hydration recrystallization process is 2-3 hours, and the crystal growth time in the dihydrate gypsum crystal growth process is 1-2 hours.
9. The method for recovering phosphorus and fluorine and producing high-purity gypsum dihydrate as a byproduct using a hemihydrate-dihydrate process according to claim 1, characterized in that: The temperature at which the absorbent absorbs the silicon tetrafluoride gas is controlled between 30 and 50°C.
10. The method for recovering phosphorus and fluorine and producing high-purity gypsum dihydrate as a byproduct using a hemihydrate-dihydrate process according to claim 1, characterized in that: The washing program of the belt vacuum filter is 3-4 stages of countercurrent washing, the washing water is desalinated water, and the water content of the filter cake is <20wt%.