A method for removing oxygen anions and carbonate ions from chloride molten salts
By leveraging the synergistic effect of heavy metal chlorides and reducing agents, oxygen anions and carbonate ions are converted into heavy metal oxide precipitates and generate elemental metals. This solves the problem of low removal efficiency of oxygen anions and carbonate ions in chloride molten salts, achieving a highly efficient and environmentally friendly purification effect.
Patent Information
- Application Number
- CN202611130214.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-28
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies have low removal efficiency for oxygen anions and carbonate ions in chloride molten salts, and the use of highly toxic or corrosive gases leads to equipment corrosion and high exhaust gas treatment costs, posing a risk of secondary pollution.
By using heavy metal chlorides such as PbCl2 or BiCl3 in synergy with a reducing agent, oxygen anions and carbonate ions are converted into heavy metal oxide precipitates through a thermodynamic spontaneous reaction. Then, the metal elements are generated through high-temperature reduction. The three-phase separation is achieved by utilizing density differences, thus avoiding the use of highly toxic gases.
It achieves efficient removal of oxygen negative ions and carbonate ions, avoids equipment corrosion and secondary pollution, improves purification efficiency and economy, and reduces exhaust gas treatment costs.
Smart Images

Figure CN123105682A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of nuclear fuel reprocessing and high-temperature metallurgical technology, specifically relating to a method for removing oxygen anions and carbonate ions from chloride molten salt. Background Technology
[0002] In the reprocessing technologies of advanced nuclear energy systems (such as fast reactors), the electrolytic reduction technology of mixed oxide (MOX) spent fuel based on a chloride molten salt system is one of the core process routes for achieving efficient recovery and recycling of nuclear materials. This technology typically uses LiCl molten salt as the electrolyte to convert metal oxides (such as UO2, PuO2, etc.) in MOX fuel into elemental metals through electrochemical reduction, thereby achieving preliminary separation from fission products.
[0003] However, this electrolytic reduction process faces an inherent technical challenge: the continuous accumulation of oxygen ions and the uncontrollable formation of impurity carbonates. During the MOX electrolytic reduction process, as the metal oxide cathode is continuously reduced to elemental metal, lattice oxygen will be released as oxygen anions (O... 2- Li2O is continuously released and dissolved in the LiCl molten salt matrix. This process causes the molten salt system to gradually evolve from pure LiCl to a LiCl-Li2O mixed molten salt. As the Li2O concentration continues to increase, it not only reduces the current efficiency of the electrolytic cell but also increases the alkalinity of the molten salt, exacerbating the molten salt corrosion rate of nickel-based alloys and other anode materials and reactor components. Furthermore, under high-temperature operating conditions (typically 600–750 °C), the molten salt has a strong chemical affinity for CO2 and H2O in the air. Trace amounts of CO2 will react rapidly with Li2O in the molten salt, generating in situ the chemically stable Li2CO3 impurity. Li2CO3 has extremely low solubility in chloride molten salts and an extremely high decomposition temperature (>1300 °C). After formation, it exists in the molten salt as a solid suspension or sediment, affecting the fluidity of the molten salt and potentially adhering to the electrode surface, leading to an abnormal increase in cell voltage.
[0004] To remove the aforementioned oxygen anions and carbonate impurities, existing technologies primarily employ gas-solid phase chemical conversion methods. This involves introducing HCl gas, Cl2, or solid chlorinating agents such as NH4Cl into a molten salt system. Through a chemical reaction, the Li2O and Li2CO3 impurities corresponding to the oxygen anions and carbonate ions are converted into LiCl, while oxygen is carried away as H2O or CO2. Typical reactions of this method include: Li2O + 2HCl → 2LiCl + H2O↑, and Li2CO3 + 2HCl → 2LiCl + H2O↑ + CO2↑. However, this method has serious drawbacks. HCl and Cl2 are both highly toxic and corrosive gases that can cause irreversible damage to stainless steel pipelines, seals, and exhaust gas treatment systems at high temperatures. Furthermore, exhaust gas treatment costs are extremely high. Additionally, the gas-liquid / solid reaction is limited by gas-liquid mass transfer efficiency, resulting in slow reaction kinetics and a long treatment cycle.
[0005] Therefore, developing a chloride molten salt purification process that combines high efficiency in impurity removal, non-corrosive system, no secondary pollution, and easy product separation is of great practical significance. Summary of the Invention
[0006] To address the shortcomings of existing technologies, this invention provides a method for removing oxygen anions and carbonate ions from chloride molten salts, thereby solving the technical problems of low impurity removal efficiency, severe equipment corrosion, high tail gas treatment costs, and secondary pollution in existing technologies. Specifically, this is achieved through the following techniques.
[0007] This invention provides a method for removing oxygen anions and carbonate ions from chloride molten salts, comprising the following steps:
[0008] A deoxygenation reaction is carried out by adding heavy metal chlorides to an initial chloride molten salt containing oxygen anions and / or carbonate ions;
[0009] A reducing agent is added to initiate a reduction reaction;
[0010] The gaseous and liquid byproducts are fractionated and discharged to obtain the purified chloride molten salt.
[0011] Furthermore, the chloride molten salt is selected from one or more of LiCl, NaCl, KCl, RbCl, CsCl, MgCl2, CaCl2, SrCl2, and BaCl2 molten salts;
[0012] Furthermore, the chloride molten salt is selected from LiCl molten salt.
[0013] Furthermore, the oxygen anion exists in one or more of the following forms: Li₂O, Na₂O, K₂O, Rb₂O, Cs₂O, MgO, CaO, SrO, and BaO; and the carbonate ion exists in one or more of the following forms: Li₂CO₃, Na₂CO₃, K₂CO₃, Rb₂CO₃, Cs₂CO₃, MgCO₃, CaCO₃, SrCO₃, and BaCO₃.
[0014] Furthermore, the oxygen anion exists in the form of Li2O, and the carbonate ion exists in the form of Li2CO3.
[0015] Furthermore, the heavy metal chloride is selected from one or both of PbCl2 and BiCl3.
[0016] Furthermore, the molar amount of the added heavy metal chloride is 95% to 98% of the theoretical molar amount required for complete reaction with the oxygen anion and / or carbonate ion.
[0017] Furthermore, the reducing agent is selected from at least one of gaseous reducing agents and carbon-based solid reducing agents; the gaseous reducing agent is selected from one or more of H2-Ar mixed gas, pure hydrogen, and methane (CH4); the carbon-based solid reducing agent is selected from one or more of graphite powder, coke, carbon black, activated carbon, and anthracite powder.
[0018] Furthermore, the molar amount of the reducing agent added is 105% to 110% of the theoretical molar amount required for complete reaction with the products in the deoxygenation reaction.
[0019] Furthermore, the reaction temperatures of the deoxygenation reaction and the reduction reaction must be higher than both the melting point of the chloride molten salt and the melting point of the product in the reduction reaction;
[0020] Furthermore, the reaction temperature for the deoxygenation and reduction reactions is 650–850 °C.
[0021] The method for removing oxygen anions and carbonate ions from chloride molten salt provided by this invention is based on the synergistic effect of low-melting-point heavy metal chlorides and reducing gases or carbon-based solid reducing agents to achieve in-situ purification of molten salt and recycling of precipitants.
[0022] This method is based on a thermodynamic spontaneous reaction precipitation transformation mechanism. It utilizes the strong chemical affinity between PbCl2 or BiCl3 and dissolved oxygen anions and carbonate ions in the molten salt to convert both oxide and carbonate impurities into heavy metal oxides (e.g., PbO, Bi2O3), releasing CO2 gas in the process. Because heavy metal oxides such as PbO and Bi2O3 have extremely high lattice energy and extremely low solubility in chloride molten salts, they precipitate as insoluble heavy metal oxides. This precipitation transformation reaction can rapidly break the metal-O bonding network (e.g., Li-O) in the original chloride molten salt, completely converting oxygen impurities from a liquid-phase dissolved state to a easily separable solid-phase state.
[0023] Taking Li₂O as an example, its reaction with PbCl₂ and BiCl₃ proceeds according to the following reaction equation:
[0024] Li₂O + PbCl₂ → 2LiCl + PbO↓;
[0025] 3Li2O+2BiCl3→6LiCl+Bi2O3↓;
[0026] For the carbonate impurity Li₂CO₃, its reaction with PbCl₂ and BiCl₃ proceeds according to the following reaction equation:
[0027] Li2CO3+PbCl2→2LiCl+PbO↓+CO2↑;
[0028] 3Li2CO3+2BiCl3→6LiCl+Bi2O3↓+3CO2↑;
[0029] Based on this, the present invention further introduces a reducing agent to perform deep reduction treatment on the separated heavy metal oxide precipitate. The reducing agent can be a gas-phase reducing agent or a carbon-based solid reducing agent.
[0030] When H2 is used as a reducing agent, PbO and Bi2O3 are reduced to metallic Pb and Bi, and the reaction proceeds according to the following reaction equation:
[0031] PbO + H2 → Pb + H2O↑;
[0032] Bi₂O₃ + 3H₂ → 2Bi + 3H₂O↑;
[0033] When CH4 is used as a reducing agent, the reactions of PbO and Bi2O3 with CH4 proceed according to the following reaction equation:
[0034] 4PbO+CH4→4Pb+CO2↑+2H2O↑;
[0035] 4Bi2O3+3CH4→8Bi+3CO2↑+6H2O↑;
[0036] When carbon-based solid reducing agents are used, solid carbon undergoes a reduction reaction with heavy metal oxides at a high temperature of 650~850℃. The reactions of PbO and Bi2O3 with carbon proceed according to the following reaction equations:
[0037] 2PbO + C → 2Pb + CO2↑;
[0038] 2Bi₂O₃ + 3C → 4Bi + 3CO₂↑;
[0039] The byproducts of the above reactions (H2O and CO2) are all high-temperature gaseous molecules that can rapidly escape from the molten salt system, maintaining the absolute purity of the system. The bubbling effect of the generated H2O and CO2 gases also acts as a physical stirrer for the molten salt system, promoting the uniform distribution and mass transfer of reactants and products.
[0040] Another key advantage of this invention lies in utilizing the significant density difference between reactants and products to achieve natural spatial isolation and physical separation. In a high-temperature molten salt environment, the gaseous byproducts (H2O, CO2) layer has an extremely low density and naturally escapes from the top of the molten salt; the pure chloride LiCl molten salt matrix layer has a moderate density (~1.50 g / cm³). 3 The liquid phase remains the main body of the molten salt; while the reduced elemental metals Pb or Bi have a much higher density than the molten salt (Pb: ~10.60 g / cm³). 3 Bi: ~10.0 g / cm³ 3 The precipitate naturally settles to the bottom of the reactor and collects into an independent liquid metal layer, thereby achieving complete physical isolation and efficient separation from the chloride molten salt. Simultaneously, this invention uses a precipitant added in a slightly smaller amount than the theoretical stoichiometric ratio required for complete reaction with oxides or carbonates; that is, the amount of precipitant added is 95%–98% of the theoretical amount. This ensures that while oxygen impurities in the molten salt are fully removed, excessive heavy metal chloride residues are absolutely avoided in the purified molten salt, thus guaranteeing the purity of the purified product and preventing the introduction of new heavy metal ion contamination.
[0041] Compared with the prior art, the advantages of the present invention are:
[0042] 1. In this invention, heavy metal chlorides PbCl2 or BiCl3 react with dissolved oxygen anions (O3) in the molten salt. 2- The precipitation reaction between the two is a thermodynamically spontaneous ion exchange reaction. The reaction rate is fast and the conversion is complete. It can achieve efficient removal of oxygen impurities and carbonate impurities in molten salt in a short time, which significantly improves the impurity removal efficiency.
[0043] 2. This invention eliminates the need to introduce highly toxic or corrosive reagents into the molten salt system, avoids damage to reactor components caused by high-temperature corrosive gases, and eliminates the burden of treating highly toxic exhaust gases and emission risks. The entire purification process has good environmental friendliness and operational safety.
[0044] 3. The byproducts of this invention achieve complete physical isolation and efficient separation from the purified chloride molten salt, and the entire process does not generate any secondary impurities;
[0045] 4. This invention converts heavy metal chlorides into heavy metal elements through precipitation conversion, achieving efficient recovery and recycling of valuable metal resources in the precipitant, avoiding waste of metal resources, and improving the economy and sustainability of the entire process. Attached Figure Description
[0046] Figure 1 This is a schematic diagram of a chloride molten salt purification reactor and its three-phase physical stratification isolation state provided in Examples 1-5. Figure 1 1 is the top exhaust outlet (water vapor / CO2); 2 is the reducing gas spray pipe; 3 is the pure molten salt layer (middle layer); 4 is the liquid metal heavy phase layer (bottom layer); 5 is the bottom heavy phase metal discharge port.
[0047] Figure 2 The image shows a physical diagram of a chloride molten salt purification reactor provided in Examples 1-5. Detailed Implementation
[0048] The technical solution of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0049] The present invention discloses a method for removing oxygen anions and carbonate ions from chloride molten salts, comprising the following steps:
[0050] S1. Preparation and melting of simulated waste salt: Prepare simulated waste salt containing oxygen anions and / or carbonate impurities, heat the simulated waste salt to completely melt it, and in the simulated waste salt, oxygen anions exist in the form of oxides and carbonates exist in the form of carbonates.
[0051] S2, In-situ Impurity Conversion: To the initial chloride molten salt system containing oxygen anions and / or carbonate impurities, add heavy metal chloride PbCl2 and / or BiCl3 purifying agents to carry out deoxygenation reaction, so that the oxides and / or carbonates in the system are converted into the corresponding chlorides, and the added heavy metal chlorides are converted into the corresponding intermediate heavy metal oxide precipitates.
[0052] S3, Deep gas phase reduction: A reducing agent is introduced into the molten salt system after step S1 to reduce the intermediate heavy metal oxide in situ to molten elemental heavy metal. In the reactor, a physical layered isolation structure is formed from top to bottom by relying on the density difference of each phase material: a gas phase by-product layer, a pure molten salt layer, and a liquid metal heavy phase layer.
[0053] S4. Three-phase stratification and separation: The gaseous byproducts at the top layer in step S2 are discharged from the top of the reactor, and the liquid heavy metal elements at the bottom layer are discharged from the bottom of the reactor, thereby achieving deep purification of chloride molten salt.
[0054] In some embodiments, the chloride molten salt may be selected from one or more of LiCl, NaCl, KCl, RbCl, CsCl, MgCl2, CaCl2, SrCl2, and BaCl2 molten salts.
[0055] In some embodiments, the oxide may be selected from one or more of Li2O, Na2O, K2O, Rb2O, Cs2O, MgO, CaO, SrO, and BaO, and the carbonate may be selected from one or more of Li2CO3, Na2CO3, K2CO3, Rb2CO3, Cs2CO3, MgCO3, CaCO3, SrCO3, and BaCO3.
[0056] In some embodiments, the molar amount of heavy metal chloride added can be 95% to 98% of the theoretical amount required for complete reaction with the oxide and / or carbonate.
[0057] In some embodiments, the reducing agent may be selected from one or more of the following: a mixture of 5% H2-Ar gas, pure hydrogen, methane, graphite powder, coke, carbon black, activated carbon, and anthracite powder.
[0058] In some embodiments, the molar amount of reducing agent added can be 105% to 110% of the theoretical molar amount required for complete reaction with the heavy metal oxides generated by the deoxidation reaction.
[0059] In some embodiments, the reaction temperature for the deoxygenation and reduction reactions can be 650–850 °C.
[0060] Example 1 (using LiCl-Li2O molten salt system, PbCl2 and H2 for purification)
[0061] This embodiment provides a method for removing oxides and carbonates from chloride molten salts, including the following steps:
[0062] S1. Preparation and melting of simulated waste salt: In a glove box filled with high-purity argon, 96 g of anhydrous LiCl reagent was weighed as the base salt, and 4.0 g of high-purity Li2O powder was added to prepare simulated waste salt with a Li2O mass fraction of 4.0%. The mixed salt was placed in a high-purity alumina crucible and then placed in a stainless steel reactor, heated to 700 ℃ to completely melt it.
[0063] S2. In-situ impurity conversion: Weigh 35.2 g of anhydrous PbCl2 powder (95% of the theoretical stoichiometry) and slowly add it to the molten salt through the feed tube. React at a constant temperature of 700 ℃ for 30 minutes to induce a metathesis reaction in the system, generating yellow PbO suspension, some of which partially settles at the bottom.
[0064] S3. Deep gas phase reduction: Maintain a constant temperature of 700 ℃, insert the corundum inlet pipe into the lower part of the molten salt, and continuously introduce 5% H2-Ar mixed reducing gas into the system at a flow rate of 200 mL / min to reduce the PbO in the lower part. Continue bubbling reduction for 300 minutes, and the generated H2O (gas) is discharged from the tail gas port at the top of the reactor along with the carrier gas.
[0065] S4. Three-phase stratification and separation: After the reaction is completed, let it stand for 15 minutes to achieve complete gravity sedimentation and stratification. The generated liquid metal Pb is deposited at the bottom of the crucible.
[0066] Example 2 (using LiCl-Li2O molten salt system, BiCl3 and H2 for purification)
[0067] This embodiment provides a method for removing oxides and carbonates from chloride molten salts, including the following steps:
[0068] S1. Preparation and melting of simulated waste salt: In a glove box filled with high-purity argon, 96.5 g of anhydrous LiCl reagent was weighed as the base salt, and 3.5 g of high-purity Li2O powder was added to prepare simulated waste salt with a Li2O mass fraction of 3.5%. The mixed salt was placed in a high-purity alumina crucible and then placed in a stainless steel reactor, heated to 700 ℃ to completely melt it.
[0069] S2. In-situ impurity conversion: Weigh 23.3 g of anhydrous BiCl3 powder (95% of the theoretical stoichiometry) and slowly add it to the molten salt through the feed tube. React at a constant temperature of 700 ℃ for 40 minutes to induce a metathesis reaction in the system, resulting in the formation of Bi2O3 suspension, some of which undergoes bottom sedimentation.
[0070] S3, Deep gas phase reduction: Maintain a constant temperature of 700 ℃, insert the corundum inlet pipe into the lower part of the molten salt, and continuously introduce 5% H2-Ar mixed reducing gas into the system at a flow rate of 150 mL / min. Continue bubbling reduction for 360 minutes, and the generated H2O (gas) is discharged from the tail gas port at the top of the reactor along with the carrier gas.
[0071] S4. Three-phase stratification and separation: After the reaction is completed, let it stand for 25 minutes to achieve complete gravity sedimentation and stratification. The generated liquid metal Bi is deposited at the bottom of the crucible.
[0072] Example 3 (using LiCl-KCl-Li2O-Li2CO3 molten salt system, PbCl2 and H2 for purification)
[0073] This embodiment provides a method for removing oxides and carbonates from chloride molten salts, including the following steps:
[0074] S1. Preparation and Melting of Simulated Waste Salt: In a glove box filled with high-purity argon, 34.9 g of anhydrous LiCl and 61.6 g of KCl reagent were weighed as the eutectic matrix salt. 2.0 g of high-purity Li₂O powder and 1.5 g of high-purity Li₂CO₃ powder were added to simulate complex aged waste salt that had absorbed CO₂ from the air, thus preparing a simulated waste salt with a Li₂O mass fraction of 2.0% and a Li₂CO₃ mass fraction of 1.5%. The mixed salt was placed in a high-purity alumina crucible and then placed in a stainless steel reactor, heated to 600 ℃ to completely melt it.
[0075] S2. In-situ impurity conversion: Weigh 23.0 g of anhydrous PbCl2 powder (95% of the theoretical stoichiometry) and slowly add it to the molten salt through the feed tube. React at a constant temperature of 600 ℃ for 30 minutes to induce a metathesis reaction in the system, converting Li2CO3. Obvious bubbles (CO2) are observed escaping from the crucible, while yellow PbO suspension is generated and some parts settle at the bottom.
[0076] S3. Deep gas phase reduction: Maintain a constant temperature of 600 ℃. After the release of CO2 bubbles has basically stopped, insert the corundum inlet pipe into the lower part of the molten salt and continuously introduce 5% H2-Ar mixed reducing gas into the system at a flow rate of 200 mL / min. Continue bubbling reduction for 200 minutes. The generated H2O (gas) is discharged from the tail gas port at the top of the reactor along with the carrier gas.
[0077] S4. Three-phase stratification and separation: After the reaction is completed, let it stand for 15 minutes to achieve complete gravity sedimentation and stratification. The generated liquid metal Pb is deposited at the bottom of the crucible, forming a very clear phase interface with the upper transparent LiCl-KCl composite molten salt.
[0078] Example 4 (using LiCl-KCl-Li2O-Li2CO3 molten salt system, BiCl3 and H2 for purification)
[0079] This embodiment provides a method for removing oxides and carbonates from chloride molten salts, including the following steps:
[0080] S1. Preparation and Melting of Simulated Waste Salt: In a glove box filled with high-purity argon, 43.5 g of anhydrous LiCl and 53.0 g of KCl reagent were weighed as the eutectic matrix salt. 2.5 g of high-purity Li₂O powder and 1.0 g of high-purity Li₂CO₃ powder were added to simulate complex aged waste salt that had absorbed CO₂ from the air, thus preparing a simulated waste salt with a Li₂O mass fraction of 2.5% and a Li₂CO₃ mass fraction of 1.0%. The mixed salt was placed in a high-purity alumina crucible and then placed in a stainless steel reactor, heated to 600 ℃ to completely melt it.
[0081] S2. In-situ impurity conversion: Weigh 20.0 g of anhydrous BiCl3 powder (98% of the theoretical stoichiometric ratio) and slowly add it to the molten salt through the feed tube. React at a constant temperature of 600 ℃ for 45 minutes to allow a metathesis reaction to occur in the system, converting Li2CO3. Obvious bubbles (CO2) are observed escaping from the crucible, and Li2O is converted into Bi2O3 particles.
[0082] S3. Deep gas phase reduction: Maintain a constant temperature of 600 ℃. After the release of CO2 bubbles has basically stopped, insert the corundum inlet pipe into the lower part of the molten salt and continuously introduce 5% H2-Ar mixed reducing gas into the system at a flow rate of 200 mL / min. Continue bubbling reduction for 230 minutes. The generated H2O (gas) is discharged from the tail gas port at the top of the reactor along with the carrier gas.
[0083] S4. Three-phase stratification and separation: After the reaction is completed, let it stand for 15 minutes to achieve complete gravity sedimentation and stratification. The generated liquid metal Bi is deposited at the bottom of the crucible, forming a very clear phase interface with the upper transparent LiCl-KCl composite molten salt.
[0084] Example 5 (using KCl-LiCl-NaCl-Li2O-Li2CO3 molten salt system, PbCl2 and CH4 for purification)
[0085] This embodiment provides a method for removing oxides and carbonates from chloride molten salts, including the following steps:
[0086] S1. Preparation and Melting of Simulated Waste Salt: In a glove box filled with high-purity argon, 40.6 g of anhydrous LiCl, 8.9 g of KCl, and 46.0 g of NaCl reagents were weighed as a ternary composite matrix salt. 3.0 g of high-purity Li₂O powder and 1.5 g of high-purity Li₂CO₃ powder were added to prepare a simulated waste salt with a Li₂O mass fraction of 3.0% and a Li₂CO₃ mass fraction of 1.5%. The mixed salt was placed in a high-purity alumina crucible and then placed in a stainless steel reactor, heated to 720 °C to completely melt it.
[0087] S2, In-situ Impurity Conversion: Weigh 31.8 g of anhydrous PbCl2 powder (95% of the theoretical stoichiometry) and slowly add it to the molten salt through a feeding tube. React at a constant temperature of 720 °C for 40 minutes. The system releases CO2 and generates enriched PbO heavy phase suspension and precipitate in situ.
[0088] S3. Deep gas phase reduction: Maintain a constant temperature of 720 ℃. After the release of CO2 bubbles has basically stopped, insert the corundum inlet pipe into the lower part of the molten salt and continuously introduce high-purity CH4 gas into the system at a flow rate of 100 mL / min (for safety, mix in an appropriate amount of Ar as a carrier gas). Continue bubbling reduction for 7 minutes. The generated CO2 and water vapor are rapidly bubbled out from the tail gas port at the top of the reactor as gaseous byproducts.
[0089] S4. Three-phase stratification and separation: After the reaction is completed, let it stand for 15 minutes to achieve complete gravity sedimentation and stratification. The generated liquid metal Pb is deposited at the bottom of the crucible, forming a very clear phase interface with the upper transparent composite matrix molten salt.
[0090] The chloride molten salt purification reactor and the three-phase physical stratification isolation state in Examples 1-5 are as follows: Figure 1 As shown, where, Figure 1 1 is the top exhaust outlet (water vapor / CO2); 2 is the reducing gas spray pipe; 3 is the pure molten salt layer (middle layer); 4 is the liquid metal heavy phase layer (bottom layer); 5 is the bottom heavy phase metal discharge port.
[0091] The chloride molten salt purification reactors in Examples 1-5 are as follows: Figure 2 As shown.
[0092] Experimental Example: Impurity Removal Rate Test of the Reaction Systems in Examples 1-5
[0093] Samples were taken from the upper chloride molten salts after precipitation conversion and reduction treatment in Examples 1-5. After cooling, the samples were completely dissolved in deionized water. A portion of the solution was titrated with standard HCl solution to determine the concentration of residual oxygen anions in the molten salt. Another portion of the solution was titrated with ion chromatography to determine the concentration of residual carbonate ions, so as to calculate the removal rate of oxygen anions and carbonate ions in each example. At the same time, the above solutions were analyzed by inductively coupled plasma mass spectrometry (ICP-MS) to detect the concentration of residual heavy metal ions (Pb ions or Bi ions). The test results are shown in Table 1.
[0094] Table 1. Removal rates of oxygen anions and carbonate ions and residual heavy metal content in the reaction systems of Examples 1-5.
[0095] Example Oxygen ion removal rate (%) Carbonate removal rate (%) Heavy metal residue Example 1 92.2 — Pb not detected Example 2 91.5 — Bi was not detected. Example 3 89.8 99.9 Pb not detected Example 4 97.5 98.5 Bi was not detected. Example 5 93.1 99.3 Pb not detected
[0096] As shown in Table 1, the oxygen anion removal rate of the method of the present invention in different molten salt systems was above 89% in all examples. Example 4 achieved a removal rate of over 97% at 600 °C, possibly because the amount of BiCl3 added in Example 4 was 98% of the theoretical amount, providing more sufficient precipitant to capture dissolved oxygen anions in the molten salt. For Examples 3-5, which added lithium carbonate impurities, the carbonate removal rate was above 98.5%, confirming that the method of the present invention also has excellent removal effect on carbonate impurities. Example 5 used low-cost methane gas instead of high-purity hydrogen as a reducing agent, achieving good removal results for both oxygen anions and carbonate ions, verifying the feasibility and effectiveness of methane replacing hydrogen, and providing a low-cost reducing agent solution for industrial-scale applications. No heavy metal ion residues corresponding to the precipitant were detected in the purified molten salt of all examples, proving that the precipitant addition strategy of slightly lower than the theoretical stoichiometric ratio used in the present invention can effectively avoid secondary contamination of the purified molten salt by heavy metal ions.
[0097] The above detailed embodiments describe the implementation of the present invention; however, the present invention is not limited to the specific details described in the above embodiments. Within the scope of the claims and technical concept of the present invention, various simple modifications and changes can be made to the technical solution of the present invention, and these simple modifications all fall within the protection scope of the present invention.
Claims
1. A method for removing oxygen anions and carbonate ions from chloride molten salt, characterized in that, Includes the following steps: A deoxygenation reaction is carried out by adding heavy metal chlorides to an initial chloride molten salt containing oxygen anions and / or carbonate ions; A reducing agent is added to initiate a reduction reaction; The gaseous and liquid byproducts are fractionated and discharged to obtain the purified chloride molten salt.
2. The method for removing oxygen anions and carbonate ions from chloride molten salt according to claim 1, characterized in that, The chloride molten salt is selected from one or more of the following: LiCl, NaCl, KCl, RbCl, CsCl, MgCl2, CaCl2, SrCl2, and BaCl2 molten salts.
3. The method for removing oxygen anions and carbonate ions from chloride molten salt according to claim 2, characterized in that, The chloride molten salt is selected from LiCl molten salt.
4. The method for removing oxygen anions and carbonate ions from chloride molten salt according to claim 1, characterized in that, The oxygen anion exists in one or more of the following forms: Li₂O, Na₂O, K₂O, Rb₂O, Cs₂O, MgO, CaO, SrO, and BaO. The carbonate ion exists in one or more of the following forms: Li₂CO₃, Na₂CO₃, K₂CO₃, Rb₂CO₃, Cs₂CO₃, MgCO₃, CaCO₃, SrCO₃, and BaCO₃.
5. The method for removing oxygen anions and carbonate ions from chloride molten salt according to claim 4, characterized in that, The oxygen anion exists in the form of Li2O, and the carbonate ion exists in the form of Li2CO3.
6. The method for removing oxygen anions and carbonate ions from chloride molten salt according to claim 1, characterized in that, The heavy metal chloride is selected from one or both of PbCl2 and BiCl3.
7. The method for removing oxygen anions and carbonate ions from chloride molten salt according to claim 1, characterized in that, The molar amount of the heavy metal chloride added is 95% to 98% of the theoretical molar amount required for complete reaction with the oxygen anion and / or carbonate ion.
8. The method for removing oxygen anions and carbonate ions from chloride molten salt according to claim 1, characterized in that, The reducing agent is selected from one or two of gaseous reducing agents and carbon-based solid reducing agents. The gaseous reducing agent is selected from one or more of H2-Ar mixed gas, pure hydrogen, and methane. The carbon-based solid reducing agent is selected from one or more of graphite powder, coke, carbon black, activated carbon, and anthracite powder.
9. The method for removing oxygen anions and carbonate ions from chloride molten salt according to claim 1, characterized in that, The amount of reducing agent added is 105% to 110% of the theoretical amount required for complete reaction with the heavy metal oxides generated by the deoxidation reaction.
10. The method for removing oxygen anions and carbonate ions from chloride molten salt according to claim 1, characterized in that, The reaction temperatures of the deoxygenation and reduction reactions must be higher than both the melting point of the chloride molten salt and the melting point of the product in the reduction reaction. Furthermore, the reaction temperature for the deoxygenation and reduction reactions is 650–850 °C.