Sequential Separation and Recovery Method of Lithium and Boron in High-Calcium Chloride Brine
By controlling the evaporation endpoint and using selective separation methods, the problem of low lithium and boron recovery rates in high-calcium chloride-type brines was solved, achieving sequential separation and efficient recovery of lithium and boron, thus improving product purity and recovery rate.
Patent Information
- Application Number
- CN202611038424.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-13
- Publication Date
- 2026-11-17
AI Technical Summary
In existing technologies for processing high-calcium chloride brine, lithium is easily lost due to entrainment in the high-viscosity liquid phase, boron resources are lost, and lithium-boron recovery routes interfere with each other, making it difficult to achieve high-yield recovery.
By controlling the evaporation endpoint, selective lithium extraction is performed on the brine within a physical property window where lithium is already enriched and viscosity has not increased dramatically. The tail liquid after lithium extraction is then treated with calcium and strontium removal and acidic nanofiltration, allowing boron to enter the nanofiltration permeate while magnesium remains on the concentrate side, thus entering different product routes.
This method enables sequential separation and high-yield recovery of lithium and boron, avoiding lithium entrainment loss in high-viscosity end brine, ensuring lithium product purity, and improving the recovery value of boron.
Smart Images

Figure CN123105684A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of comprehensive utilization of underground brine resources and hydrometallurgical separation technology. Specifically, it relates to a method for sequential separation and recovery of lithium and boron in brine with high calcium, high salt, and boron chloride content. Background Technology
[0002] Deep chloride-type brines typically exhibit low lithium concentration, high calcium content, moderate magnesium-to-lithium ratio, and boron as a byproduct in the form of boric acid or borate, making them important sources of lithium and boron resources. Currently, the development of these brines often follows the long-term salt field evaporation route, where lithium is extracted through precipitation or solvent extraction after the brine has evaporated to the final stage. However, the viscosity of the brine increases sharply in the later stages of evaporation, making lithium easily lost due to entrainment in the high-viscosity liquid phase, resulting in unreliable recovery rates. Simultaneously, boron in the final stage of evaporation can easily enter the solid phase with calcium-boron double salts or magnesium-boron salts, leading to boron resource loss.
[0003] Another process option is to add a large amount of alkali or calcium removal agent before lithium extraction, but this can easily lead to lithium loss and increase solid waste. If the end brine is directly acidified to precipitate boron or solvent extraction is used to extract boron, there are problems such as high reagent consumption, unstable product purity, and high environmental risks of organic phase.
[0004] The aforementioned processes, whether focusing on lithium extraction at the end of evaporation or extensive impurity removal at the beginning, fail to identify and control an evaporation endpoint window based on the coupled changes in viscosity, lithium concentration, and evaporation rate during the evaporation process. Within this window, lithium in the brine has accumulated to an adsorbable concentration, and the viscosity has not yet increased dramatically due to over-evaporation, maintaining good fluidity. This allows for selective extraction before significant lithium loss, while ensuring the tail liquid retains suitable fluidity for subsequent membrane separation and boron recovery. Therefore, a method is needed that can identify and control this evaporation window, enabling sequential separation to allow lithium and boron to enter different product routes and achieve high-yield recovery of each. Summary of the Invention
[0005] This invention provides a method for the sequential separation and recovery of lithium and boron in high-calcium chloride-type brine. The method involves determining and controlling the evaporation endpoint to selectively extract lithium from the brine within a physical property window where lithium is already enriched but viscosity has not yet increased dramatically. The tail liquid after lithium extraction undergoes calcium and strontium removal and acidic nanofiltration, allowing boron to enter the nanofiltration permeate while magnesium remains on the nanofiltration concentrate side. Thus, lithium and boron enter different product routes, achieving sequential separation and high-yield recovery of each.
[0006] Specifically, the method of the present invention includes the following steps: The chloride-type brine containing lithium, boron, calcium, and magnesium is evaporated, and the evaporation endpoint is controlled so that the lithium ion concentration in the liquid phase reaches 150~500 mg / L and the viscosity is not higher than 10 mPa·s, thus obtaining enriched brine. The enriched brine was adsorbed, eluted, and desorbed using a lithium-selective adsorbent to obtain a lithium-rich desorbent and an adsorption tail liquid. The lithium-rich desorbate was subjected to boron removal, nanofiltration to remove divalent impurities, concentration and lithium precipitation in sequence to obtain lithium salt products; The adsorption tail liquid is subjected to calcium and strontium removal treatment to obtain a low-calcium, strontium, and boron-rich solution. After adjusting the pH of the low-calcium strontium-rich boron solution to 2.8-4.8, nanofiltration is performed, allowing boron to enter the nanofiltration permeate while magnesium remains on the nanofiltration concentrate side. The nanofiltration permeate is concentrated and crystallized to obtain a boron product.
[0007] Preferably, the evaporation rate corresponding to the evaporation endpoint is 80%~96%, and the pH of the enriched brine is 3.0~8.0. This precisely defines the boundary conditions of the evaporation window, avoiding premature entry leading to insufficient lithium concentration and delayed entry leading to a sharp increase in viscosity. This ensures more reliably that the brine enters the adsorption process while maintaining both good fluidity and lithium enrichment, thus supporting stable control of the core window.
[0008] Preferably, the lithium-selective adsorbent is one or more of aluminum-based layered lithium adsorbents, titanium-based lithium ion sieves, and manganese-based lithium ion sieves. Therefore, by limiting the type of adsorbent, the selectivity for lithium ions is improved, the co-adsorption of calcium and magnesium ions is reduced, thereby ensuring the purity of the lithium-rich desorption solution and reducing the load on subsequent membrane separation.
[0009] Preferably, the adsorption temperature is 10~80℃, the flow rate is 1~10 BV / h, and the adsorption time is 0.5~5h. This optimizes the adsorption mass transfer kinetics, improves the lithium adsorption load and efficiency per cycle, and makes the process more suitable for continuous industrial operation.
[0010] Preferably, the rinsing time is 5-60 minutes, and the desorption time is 0.5-4 hours. This effectively removes the high-calcium and magnesium halides entrained in the bed, increasing the relative lithium content in the desorbate and reducing the introduction of impurities into the lithium production line.
[0011] Preferably, the boron removal is performed using a boron-specific chelating resin to reduce the B2O3 content in the lithium-rich desorption solution to no more than 5 mg / L. This deeply removes boron from the lithium-rich desorption solution, preventing it from entering subsequent lithium products and ensuring that the lithium salt products meet battery-grade purity requirements.
[0012] Preferably, the operating pressure for nanofiltration to remove divalent impurities is 20-40 bar, and for Ca... 2+ Mg 2+ or Sr 2+The retention rate is no less than 90%. This enhances the membrane separation and retention effect of divalent metal ions, avoids the co-precipitation of calcium, magnesium, and strontium with lithium during subsequent concentration and lithium precipitation, and further improves the purity of lithium products.
[0013] Preferably, the calcium and strontium removal treatment involves heating the adsorption tail liquid to 40-90°C, adding sodium sulfate, ammonium sulfate, or a combination thereof, with the amount of precipitant added being 0.8-1.5 times the theoretical amount, and reacting for 0.2-4 hours followed by solid-liquid separation. This efficiently precipitates and removes calcium and strontium ions, preventing membrane fouling and excessively high osmotic pressure during subsequent acidic nanofiltration, thus ensuring stable operation of the membrane system.
[0014] Preferably, the low-calcium, strontium-rich, boron-rich solution is adjusted to a pH of 2.8–4.8, the nanofiltration operation pressure is 30–40 bar, the single-stage water recovery rate is 40%–70%, and the nanofiltration is effective against Mg. 2+ The rejection rate is no less than 95%, and the rejection rate for boron is no more than 20%. This optimizes the operating boundary of acidic nanofiltration, allowing boron to efficiently permeate through the nanofiltration membrane in the form of electrically neutral boric acid molecules, while magnesium is effectively retained due to its hydration radius and membrane charge repulsion. This significantly improves the selective separation efficiency of boron permeation and magnesium rejection, further enhancing the magnesium-boron separation effect.
[0015] Preferably, the concentration and lithium precipitation process includes: concentrating the permeate after nanofiltration to remove divalent impurities through one or more stages of reverse osmosis, then evaporating and concentrating it to a lithium ion concentration of 10-30 g / L, adding sodium carbonate or sodium bicarbonate, precipitating lithium carbonate at 85-100°C, and then washing, drying, and carbonizing and recrystallizing. This converts the purified lithium-rich solution into battery-grade lithium carbonate product, and further improves the purity of the lithium product through carbonization and recrystallization.
[0016] Beneficial effects: This invention controls the evaporation endpoint to preferentially extract lithium from brine within a specific physical property window where the lithium ion concentration reaches 150~500mg / L and the viscosity does not exceed 10mPa·s, avoiding lithium entrainment loss in the high-viscosity end brine. At the same time, the tail liquid after lithium extraction still has good fluidity and boron recovery value. After calcium and strontium removal and acidic nanofiltration (pH 2.8~4.8), boron permeates through the nanofiltration membrane in the form of electrically neutral boric acid molecules while magnesium is retained, thereby forming high-purity lithium salt products and boron products respectively, realizing the sequential diversion and synergistic recovery of lithium and boron product lines. Attached Figure Description
[0017] The above and other aspects, features, and advantages of embodiments of the present invention will become clearer from the following description taken in conjunction with the accompanying drawings, in which: Figure 1 This is a schematic diagram of the overall material flow for the lithium and boron product lines of the present invention, used to illustrate the overall material balance and diversion architecture of the entire process. Figure 2 This is a schematic diagram showing the relationship between the viscosity, pH, density, refractive index and evaporation rate of the brine in this invention, used to illustrate the abrupt changes in physical properties during evaporation and the location of the optimal extraction window; Figure 3 This is a flowchart of the adsorption-washing-desorption operation of the present invention, used to illustrate the cyclic operation steps of fixed bed adsorption for lithium extraction; Figure 4 This is a flow chart of the lithium-rich liquid NF / RO purification process of the present invention, used to illustrate the purification and concentration route from lithium-rich desorbent to battery-grade lithium carbonate in the lithium product line; Figure 5 The flowchart of the lithium extraction tail liquid calcium and strontium removal-acidic NF boron-magnesium interception-concentration crystallization process of the present invention is used to demonstrate the full membrane recovery process of boron product line. Detailed Implementation
[0018] Hereinafter, specific embodiments of the present invention will be described in detail with reference to the accompanying drawings. However, the present invention can be implemented in many different forms, and should not be construed as limited to the specific embodiments set forth herein. Rather, these embodiments are provided to explain the principles of the invention and its practical application, thereby enabling others skilled in the art to understand the various embodiments of the invention and various modifications suitable for particular intended applications.
[0019] For ease of understanding, some of the terms used in this embodiment are explained as follows: Bed volume (BV): refers to the total volume of the adsorbent filling the bed. The flow rate unit BV / h indicates how many bed volumes are equivalent to the volume of liquid flowing through the adsorption bed per hour. For example, 1 BV / h means that the volume of liquid flowing through the bed per hour is exactly equal to one bed volume.
[0020] Theoretical quantity: refers to the molar amount of precipitant required to completely precipitate calcium and strontium ions in a solution according to stoichiometric ratio.
[0021] Lithium extraction tail liquid: refers to the tail liquid obtained after adsorption lithium extraction and subsequent electro-oxidation pretreatment to remove organic impurities.
[0022] Adsorption qualified solution: refers to the qualified liquid after preliminary treatment of lithium-rich desorption solution.
[0023] Precipitating agents: These are reagents used to precipitate calcium and strontium ions as sulfates, including sodium sulfate, ammonium sulfate, or combinations thereof.
[0024] As described in the background section, existing technologies for treating high-calcium chloride-type brine often employ long-term evaporation to the end of the brine before lithium extraction, or involve adding large amounts of alkali to remove calcium at the beginning. These approaches fail to recognize the specific physical property window during evaporation that combines good fluidity with lithium enrichment. The consequences are: lithium is lost due to entrainment in the high-viscosity end brine; boron is lost through co-precipitation with calcium and magnesium double salts; and lithium and boron recovery routes interfere with each other.
[0025] To address the aforementioned technical problems, the overall technical concept of this invention is as follows: During the evaporation process of high-calcium chloride brine, viscosity, lithium concentration, and evaporation rate exhibit a coupled and abrupt relationship. Based on this, an evaporation endpoint window is determined and controlled. Within this window, the lithium-ion concentration of the brine reaches an adsorbable level, while the viscosity has not yet increased dramatically. This allows for selective lithium extraction. The tail liquid after lithium extraction still possesses good flowability, suitable for subsequent membrane separation treatment, and the boron within it has recovery value. The tail liquid undergoes calcium and strontium removal treatment followed by acidic nanofiltration. In acidic nanofiltration, boron permeates through the nanofiltration membrane in the form of electrically neutral boric acid molecules, while magnesium is retained. Lithium and boron are thus introduced into different product routes, achieving sequential diversion and high-yield recovery of each.
[0026] The overall technical concept described above will be explained in detail below.
[0027] This invention provides a method for the sequential separation and recovery of lithium and boron in high-calcium chloride-type brine. The overall material flow is as follows: Figure 1 As shown, the original brine is evaporated to obtain lithium-rich brine. After pretreatment, it enters the adsorption process. After adsorption, it is divided into two routes: the lithium-rich desorption solution is treated with resin boron removal and membrane system to obtain lithium carbonate product; the adsorption tail liquid is treated with membrane method to extract boron and then enters the subsequent salt recovery or is returned to the evaporation system. The boron extracted by resin boron removal is also included in the borax product route.
[0028] The method for sequential separation and recovery of lithium and boron in high-calcium chloride brine provided by this invention specifically includes the following steps: Step 1: Evaporate the chloride-type brine containing lithium, boron, calcium, and magnesium, and control the evaporation endpoint so that the lithium ion concentration in the liquid phase reaches 150~500 mg / L and the viscosity is not higher than 10 mPa·s, to obtain lithium-rich brine.
[0029] Step 2: The enriched brine is adsorbed, eluted and desorbed using a lithium selective adsorbent to obtain lithium-rich desorbed solution and adsorption tail liquid.
[0030] Step 3: The lithium-rich desorption solution is subjected to boron removal, nanofiltration to remove divalent impurities, concentration and lithium precipitation treatment in sequence to obtain lithium salt products.
[0031] Step 4: Remove calcium and strontium from the adsorption tail liquid to obtain a low-calcium, strontium-rich boron solution.
[0032] Step 5: Adjust the pH of the low-calcium strontium-rich boron solution to 2.8-4.8 and then perform nanofiltration, so that boron enters the nanofiltration permeate while magnesium remains on the nanofiltration concentrate side.
[0033] Step 6: Concentrate and crystallize the nanofiltration permeate to obtain the boron product.
[0034] The preferred methods for concentration and lithium precipitation treatment include: concentrating the permeate after nanofiltration to remove divalent impurities through one or more stages of reverse osmosis, and then evaporating and concentrating it to a lithium ion concentration of 10-30 g / L; adding sodium carbonate or sodium bicarbonate to the concentrate to precipitate lithium carbonate at 85-100°C; and washing, drying and carbonizing the precipitate for recrystallization.
[0035] Figure 2 The relationship between the physical properties of a high-calcium chloride brine and the evaporation rate during isothermal evaporation is shown. Figure 2 In (a), as the evaporation rate increases from 0% to approximately 90%, the pH of the brine slowly decreases from approximately 7.0 to approximately 6.0, and the density increases from approximately 1.05 g / cm³. 3 It gradually increased to approximately 1.25 g / cm³. 3 When the evaporation rate exceeds 90%, the pH drops sharply to 1.0-1.5, and the density rises sharply to 1.55 g / cm³. 3 above. Figure 2 In (b), the refractive index slowly increases from about 1.36 to about 1.40 (at 90% evaporation rate) as the evaporation rate increases, and then rises sharply to 1.47; the viscosity remains basically at 2~4 mPa·s before 90% evaporation rate, and then soars exponentially to over 25 mPa·s after 90%. Figure 2 The optimal extraction point is marked in the range of 90% to 95% evaporation rate. This range is the physical property window where lithium is enriched and the viscosity is not out of control.
[0036] Therefore, the present invention preferably sets the evaporation rate corresponding to the evaporation endpoint at 80%~96%, and the pH of the enriched brine is preferably 3.0~8.0. If the evaporation rate is too low, the lithium ion concentration will not reach 150mg / L, the volume of brine treated per unit lithium amount by the adsorbent will be too large, resulting in poor economic efficiency; if the evaporation rate is too high (>96%), then... Figure 2 The viscosity abrupt change region shown indicates a sharp deterioration in brine fluidity, increased adsorption-mass transfer resistance, and a significant increase in lithium entrainment loss at the solid-liquid interface. The pH range of 3.0–8.0 corresponds to the natural acid-base fluctuation range of the brine during evaporation. This range avoids both the damage to the adsorbent structure caused by strong acidity and lithium entrainment caused by calcium and magnesium hydroxide precipitation under alkaline conditions. Further optimization is achieved with an evaporation rate of 85%–95% and a pH of 3.5–6.5 to balance lithium enrichment and operational feasibility within the aforementioned window.
[0037] Figure 3This is a flow chart of the adsorption-elution-desorption operation. The adsorbent is packed into a fixed bed or multi-column continuous adsorption system. The adsorbent is first activated with pure water for 60-90 minutes to restore its adsorption activity, and then the evaporated and enriched brine is passed through for adsorption.
[0038] The preferred lithium-selective adsorbent is one or more of aluminum-based layered lithium adsorbents, titanium-based lithium ion sieves, and manganese-based lithium ion sieves. These adsorbents all exhibit lithium-ion memory effect. In a high-calcium-magnesium background, ordinary ion exchange resins struggle to distinguish Li. + With Ca 2+ / Mg 2+ The latter two have high charge density and hydration radius similar to Li. + When lithium is close to its surroundings, significant co-adsorption occurs. This leads to an increase in calcium and magnesium impurities in the desorption solution, increasing the load on subsequent membrane separation. Aluminum-based layered lithium adsorbents, on the other hand, possess lattice-matched sites, which facilitate the adsorption of lithium. + Its selectivity is much higher than that of calcium and magnesium. This ensures the purity of the lithium-rich desorption solution and reduces the pressure of subsequent nanofiltration for impurity removal.
[0039] The preferred adsorption temperature is 10–80℃, the preferred flow rate is 1–10 BV / h, and the preferred adsorption time is 0.5–5 h. The adsorption process is jointly controlled by liquid film diffusion and intraparticle diffusion. Increasing the temperature reduces the viscosity of the brine and increases the lithium-ion diffusion coefficient. A flow rate of 1–10 BV / h balances the mass transfer driving force and bed pressure drop. If the flow rate is too low, the throughput is insufficient; if the flow rate is too high, the contact time is insufficient, and the adsorption front breaks through prematurely. An adsorption time of 0.5–5 h ensures that mass transfer within the particles reaches equilibrium, maximizing the lithium adsorption load per cycle. This parameter range balances the economy and operational stability of industrial continuous processing.
[0040] The preferred rinsing time is 5–60 min, and the preferred desorption time is 0.5–4 h. After adsorption, a large amount of high-calcium magnesium brine remains in the bed gaps and on the surface of the adsorbent. If rinsing is insufficient (<<5 min), the residual brine will directly enter the desorption solution, diluting the lithium concentration and introducing impurities. If rinsing is excessive (>60 min), the adsorbed lithium may desorb prematurely, reducing the yield. The desorption time of 0.5–4 h corresponds to the desorption kinetics of lithium ions within the adsorbent particles. Insufficient time results in incomplete desorption; excessive time reduces equipment turnover. A preferred rinsing time of 10–30 min and desorption time of 1.5–3 h achieve the best balance between impurity removal and lithium yield.
[0041] Finally, the bed is topped with delithiation brine for 5-20 minutes to remove any remaining desorption liquid, preparing it for the next cycle. The adsorption tail liquid is then used as boron-rich tail liquid in the subsequent boron extraction process.
[0042] Figure 4This is a flow chart for the purification of lithium-rich NF / RO solution. The qualified adsorption solution (i.e., lithium-rich desorption solution) is first subjected to a boron-specific chelating resin for deep boron removal, reducing the B2O3 content to no more than 5 mg / L. More preferably, the B2O3 content is reduced to no more than 1 mg / L. The desorbed boron then enters the boron extraction section.
[0043] Boron removal is preferably achieved using a boron-specific chelating resin. This reduces the B2O3 content in the lithium-rich desorption solution to no more than 5 mg / L. Even trace amounts of boron in the lithium-rich desorption solution can be significantly amplified during subsequent concentration due to the enrichment effect. If boron enters the lithium precipitation stage, it will co-crystallize with lithium carbonate or coat the particle surface, leading to excessive boron content in battery-grade lithium carbonate products. The boron-specific chelating resin has a specific coordination ability for boric acid molecules, selectively capturing boron in a high-salt environment and reducing it to below 5 mg / L. This blocks the migration of boron to the lithium product line, ensuring the purity of lithium salts.
[0044] After boron removal, the feed solution undergoes microfiltration or ultrafiltration pretreatment before entering a primary NF nanofiltration system, operating within the general nanofiltration operating pressure range of 20–40 bar, allowing Ca to be removed. 2+ Mg 2+ 、Sr 2+ The divalent ion rejection rate is not less than 90%, preferably not less than 94%. The nanofiltration membrane's ion rejection follows the Donnan effect and sieving effect. An operating pressure of 20–40 bar provides sufficient transmembrane driving force, allowing solvent permeation while divalent ions are enriched on the concentrate side. Ca 2+ Mg 2+ 、Sr 2+ The hydration radius of these ions is relatively large, and they carry a divalent positive charge, making them more susceptible to electrostatic repulsion from the negative charge on the membrane surface. If the rejection rate is below 90%, a large number of divalent ions will enter the permeate side, competing with lithium for precipitation during subsequent concentration and evaporation, potentially leading to excessive levels of calcium, magnesium, and strontium impurities in the lithium carbonate product. These pressure and rejection rate parameters ensure that divalent impurities are effectively isolated from the lithium product line.
[0045] The concentrate from the first-stage NF (Non-Fluorescence) filtration enters the second-stage NF nanofiltration system for further lithium recovery. The second-stage concentrate is returned to the salt pan. The first-stage NF permeate (feed solution) enters the first-stage reverse osmosis concentration system, followed by the second-stage reverse osmosis concentration system, and the desalinated water is reused. The reverse osmosis concentration ratio is preferably 3 to 15 times, more preferably 5 to 10 times.
[0046] The adsorption tail liquid is heated to 40-90℃, preferably 60-80℃. Sodium sulfate, ammonium sulfate, or a combination thereof are added as precipitants to precipitate the Ca... 2+ and Sr 2+ Precipitate in the form of sulfate. The amount of precipitant added is 0.8 to 1.5 times the theoretical amount. After the precipitation reaction is carried out for 0.2 to 4 hours, solid-liquid separation is performed to obtain a low-calcium, strontium-rich boron solution.
[0047] CaSO4 and SrSO4 are sparingly soluble salts. Increasing the temperature to 40-90℃ increases the crystal nucleation rate, promotes precipitation aging, and improves solid-liquid separation efficiency. If the precipitant dosage is less than 0.8 times the theoretical amount, calcium and strontium removal will be incomplete; if the dosage is more than 1.5 times, excessive sulfate ions will be introduced, increasing the load on subsequent nanofiltration desalination and potentially causing CaSO4 scaling on the membrane surface. A precipitation reaction time of 0.2-4 hours ensures that the precipitate crystals grow to a filterable size. The combination of the above-mentioned temperature, precipitant type and dosage, and reaction time creates low-hardness, low-scaling-prone feed water conditions for subsequent acidic nanofiltration while efficiently removing calcium and strontium.
[0048] Figure 5 The flow chart for calcium and strontium removal from lithium extraction tailings – acidic NF permeation for boron removal and magnesium interception – concentration and crystallization. Sodium sulfate solution is added to the lithium extraction tailings for stepwise removal of calcium and strontium, producing a mixture of strontium sulfate and gypsum slag. The gypsum slag washing liquid is returned for diluting the filtrate to reduce osmotic pressure. Subsequently, a scale inhibitor is added to the diluted filtrate, and the pH is acidified to 2.8–4.8. The acidified filtrate enters a nanofiltration system, where the nanofiltration membrane retains magnesium ions and residual sulfate, while boron permeates through the membrane in an electrically neutral molecular form into the permeate side.
[0049] The low-calcium, strontium-rich, boron-rich solution was adjusted to a pH of 2.8–4.8. The optimal operating pressure for this acidic nanofiltration process was 30–40 bar, with a single-stage water recovery rate of 40%–70%. Under these conditions, nanofiltration effectively reduced Mg2+ levels. 2+ The rejection rate is not less than 95%, and the rejection rate for boron is not higher than 20%.
[0050] The mechanism of the above selective separation is as follows: Boron has a pKa of 9.16, and at pH 2.8–4.8, boron mainly exists in the form of electrically neutral boric acid molecules (H3BO3); Mg 2+ It exists entirely in an ionic state. Nanofiltration membranes are typically negatively charged, and their Donan repulsion of electrically neutral molecules is negligible. Furthermore, electrically neutral boric acid molecules are small and easily permeate through the pores of nanofiltration membranes. In contrast, Mg... 2+ Positively charged, it is efficiently retained due to the combined effects of the negative charge on the membrane surface (Downan repulsion) and the size sieving effect.
[0051] An operating pressure of 30–40 bar provides sufficient transmembrane driving force; a single-stage water recovery rate of 40%–70% balances permeate flow and concentrate recirculation efficiency. Mg 2+ The retention rate is ≥95% to ensure that the concentrate side is rich in magnesium while the product water side is low in magnesium; the boron retention rate is ≤20% to ensure that boron enters the product water side efficiently.
[0052] The concentrate from the first-stage nanofiltration enters the second-stage NF nanofiltration for further treatment, producing a magnesium-rich solution. The nanofiltration permeate (i.e., boron-rich permeate) enters the subsequent concentration and crystallization stage. When using 2-4 stages in series or concentrate recycling, the cumulative boron recovery rate is not less than 80%, preferably not less than 90%.
[0053] The nanofiltration permeate is concentrated through reverse osmosis, electrodialysis, MVR, or solar evaporation in salt fields to achieve a B2O3 concentration of 30–120 g / L, preferably 50–100 g / L. Borax, boric acid, or boron-rich salt products are then obtained through cooling crystallization, evaporation crystallization, or seed crystallization.
[0054] like Figure 5 As shown, the above concentration process can be carried out in multiple stages: first, the solution is pre-concentrated by reverse osmosis, and the resulting freshwater is reused; then, the concentrate is precipitated by sun-drying in salt fields to obtain halite, and further concentrated by MVR; subsequently, sodium salt is removed by hot filtration to produce halite; alkali is added to the filtrate for cooling and crystallization, and after drying and packaging, borax is obtained. The crystallization mother liquor is returned to the evaporation system.
[0055] Li in nanofiltration product water + The concentration is typically only several hundred to several thousand mg / L. This lithium-rich solution needs to be concentrated 3 to 15 times, preferably 5 to 10 times, by one or more stages of reverse osmosis to reduce the energy consumption of subsequent evaporation. It is then concentrated by MVR (mechanical vapor recompression) to a lithium-ion concentration of 10 to 30 g / L. Sodium carbonate or sodium bicarbonate is added to this concentrate, and lithium carbonate is precipitated at 60 to 100°C. During this process, the reduced solubility of lithium carbonate at high temperatures and the common ion effect promote complete precipitation. However, the lithium carbonate precipitated in the first stage may contain trace amounts of sodium and potassium ions. Therefore, carbonation and recrystallization are used to convert these ions into lithium bicarbonate for further decomposition and lattice purification. This combined route achieves the coupling of low-energy concentration and high-purity product preparation.
[0056] Example 1: Pre-adsorption lithium extraction and lithium-rich liquid refining Take a deep, high-calcium chloride brine and evaporate it isothermally at approximately 25°C until Li + The brine concentration is approximately 200–430 mg / L, with a viscosity below 5 mPa·s and an evaporation rate between 85% and 95%. This brine is passed into a fixed bed packed with an aluminum-based layered lithium adsorbent at a flow rate controlled at approximately 4–7 BV / h. The flow rate is switched over approximately 1–3 h based on the breakthrough curve. Subsequently, it is rinsed with pure water for approximately 10–30 min and then hydrolyzed for approximately 1.5–3 h to obtain a lithium-rich desorbent.
[0057] After treatment with a boron-specific chelating resin, the B2O3 in the lithium-rich desorbate was reduced to trace levels. It then underwent microfiltration / ultrafiltration pretreatment, two-stage nanofiltration, and reverse osmosis concentration. Nanofiltration operated at approximately 20–40 bar, achieving a rejection rate of over 90% for divalent ions such as calcium, magnesium, and strontium. Reverse osmosis further concentrated the lithium solution by approximately 5–10 times. The concentrated solution was then evaporated to Li₂ using an MVR (Medium-Voltage Reduction) system. + After adding approximately 10-30 g / L of sodium carbonate, lithium is precipitated, and then battery-grade lithium carbonate is obtained through carbonization and recrystallization.
[0058] Example 2: Full-membrane recovery of boron from lithium extraction tailings The adsorption tail liquid obtained in Example 1 was used as a boron-rich tail liquid, containing g / L levels of B2O3 and a relatively high concentration of Ca. 2+ Mg 2+ and Sr 2+ First, heat the tailings liquid to 60-80℃, then add sodium sulfate at 0.9-1.3 times the theoretical amount required for calcium and strontium precipitation. After stirring and reacting, filter to allow the Ca... 2+ 、Sr 2+ Significantly reduced. The filtrate was adjusted to a pH of 3.3–4.2 before entering the nanofiltration membrane system. Because boron exists primarily as electrically neutral boric acid molecules within this pH range, it easily permeates the nanofiltration membrane; while Mg… 2+ The boron is mainly retained due to the influence of hydration radius and membrane charge repulsion. The recovery rate of single-stage nanofiltration water is controlled at about 50%~65%, while the cumulative boron recovery rate reaches over 90% when three stages are connected in series. The permeate is then concentrated to about 50~100 g / L of B2O3 through reverse osmosis, salt field solar evaporation, or MVR, and then cooled for crystallization. Borax or boron-rich products are obtained.
[0059] In summary, this invention achieves selective lithium extraction from brine within a specific physical property window—a lithium ion concentration of 150–500 mg / L and a viscosity not exceeding 10 mPa·s—by controlling the evaporation endpoint. This avoids lithium entrainment loss in the high-viscosity brine at the end of the extraction process. The tail liquid after lithium extraction still possesses good flowability and boron recovery value. This tail liquid is first treated to remove calcium and strontium, then treated by acidic nanofiltration (pH 2.8–4.8). During this process, boron permeates through the nanofiltration membrane in the form of electrically neutral boric acid molecules, while magnesium is retained. Thus, lithium and boron enter different product routes. This invention achieves sequential diversion and synergistic recovery of lithium and boron product lines, improving the recovery rates of both lithium and boron, and increasing the purity of the lithium product.
[0060] The optional embodiments of the present invention have been described in detail above with reference to the accompanying drawings. However, the embodiments of the present invention are not limited to the specific details in the above embodiments. Within the scope of the technical concept of the embodiments of the present invention, various simple modifications can be made to the technical solutions of the embodiments of the present invention, and these simple modifications all fall within the protection scope of the embodiments of the present invention.
Claims
1. A method for sequential separation and recovery of lithium and boron in high-calcium chloride-type brine, characterized in that, Includes the following steps: The chloride-type brine containing lithium, boron, calcium, and magnesium is evaporated, and the evaporation endpoint is controlled so that the lithium ion concentration in the liquid phase reaches 150~500 mg / L and the viscosity is not higher than 10 mPa·s, thus obtaining enriched brine. The enriched brine was adsorbed, eluted, and desorbed using a lithium-selective adsorbent to obtain a lithium-rich desorbent and an adsorption tail liquid. The lithium-rich desorbate was subjected to boron removal, nanofiltration to remove divalent impurities, concentration and lithium precipitation in sequence to obtain lithium salt products; The adsorption tail liquid is subjected to calcium and strontium removal treatment to obtain a low-calcium, strontium, and boron-rich solution. After adjusting the pH of the low-calcium strontium-rich boron solution to 2.8-4.8, nanofiltration is performed, allowing boron to enter the nanofiltration permeate while magnesium mainly remains on the nanofiltration concentrate side. The nanofiltration permeate is concentrated and crystallized to obtain a boron product.
2. The method according to claim 1, characterized in that, The evaporation rate corresponding to the evaporation endpoint is 80%~96%, and the pH of the enriched brine is 3.0~8.
0.
3. The method according to claim 1, characterized in that, The lithium selective adsorbent is one or more of the following: aluminum-based layered lithium adsorbent, titanium-based lithium ion sieve, and manganese-based lithium ion sieve.
4. The method according to claim 1, characterized in that, The adsorption temperature is 10~80℃, the flow rate is 1~10 BV / h, and the adsorption time is 0.5~5h.
5. The method according to claim 1, characterized in that, The rinsing time is 5-60 minutes, and the desorption time is 0.5-4 hours.
6. The method according to claim 1, characterized in that, The boron removal process involves treating the lithium-rich desorption solution with a boron-specific chelating resin to reduce the B2O3 content to no more than 5 mg / L.
7. The method according to claim 1, characterized in that, The operating pressure of the nanofiltration for removing divalent impurities is 20-40 bar, and the rejection rate of Ca 2+ , Mg 2+ , or Sr 2+ is not less than 90%.
8. The method according to claim 1, characterized in that, The calcium and strontium removal treatment is as follows: the adsorption tail liquid is heated to 40~90℃, sodium sulfate, ammonium sulfate or a combination thereof are added, the amount of precipitant added is 0.8~1.5 times the theoretical amount, and the solid and liquid are separated after reacting for 0.2~4 hours.
9. The method according to claim 1, characterized in that, The low-calcium, strontium-rich, boron-rich solution was adjusted to a pH of 2.8–4.
8. The nanofiltration operation pressure was 30–40 bar, and the single-stage water recovery rate was 40%–70%. Furthermore, the nanofiltration process was effective against Mg2+. 2+ The rejection rate is not less than 95%, and the rejection rate for boron is not higher than 20%.
10. The method according to claim 1, characterized in that, The concentration and lithium precipitation process includes: concentrating the permeate after nanofiltration to remove divalent impurities through one or more stages of reverse osmosis, then evaporating and concentrating it to a lithium ion concentration of 10-30 g / L, adding sodium carbonate or sodium bicarbonate, precipitating lithium carbonate at 85-100°C, and then washing, drying and carbonizing recrystallizing the permeate.