A method for preparing yttrium oxide coatings and its products
By reacting a gaseous precursor of yttrium acetylacetonate and yttrium triisopropoxy with the matrix under specific conditions, the problems of low adhesion, high carbon content, high porosity and high surface roughness of yttrium oxide coatings were solved, and low-energy-consumption and high-efficiency yttrium oxide coating preparation was achieved.
Patent Information
- Application Number
- CN202611148758.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-30
- Publication Date
- 2026-11-17
AI Technical Summary
In the prior art, when yttrium acetylacetonate or yttrium triisopropoxy is used alone to prepare yttrium oxide coatings, there are problems such as high reaction temperature, low reaction rate, high carbon content, high porosity, high surface roughness, and low adhesion to the substrate.
A mixed gaseous precursor of yttrium acetylacetonate and yttrium triisopropoxy was used, with a mass ratio of 1:(0.8~1.2). The precursor was contacted with the matrix at 800℃~950℃. The oxygen-containing gas in the mixed gas participated in the reaction, which diluted the vapor viscosity of yttrium acetylacetonate, promoted the adsorption and decomposition of yttrium triisopropoxy at the active sites, reduced the reaction temperature, increased the reaction rate, and promoted the oxidative breakage of the six-membered ring chelate structure through the local high temperature zone, thereby reducing carbon residue.
It improves the adhesion between the yttrium oxide coating and the substrate, reduces the carbon content, porosity and surface roughness of the yttrium oxide coating, reduces reaction energy consumption, and reduces the risk of cracking and peeling of the yttrium oxide coating.
Smart Images

Figure CN123105702A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of new materials technology, specifically to a method for preparing a yttrium oxide coating and the yttrium oxide coating obtained by the method. Background Technology
[0002] Yttrium oxide (Y₂O₃) is a rare earth oxide with excellent properties. It has a high melting point of 2410℃ and exhibits good high-temperature resistance, plasma corrosion resistance, high insulation, low thermal conductivity, and chemical stability. It is widely used in semiconductor, aerospace, energy, and metallurgical industries. Currently, the main methods for preparing yttrium oxide coatings include plasma spraying, physical vapor deposition (PVD), and chemical vapor deposition (CVD). Among these, chemical vapor deposition (CVD) technology has become the preferred method for preparing high-performance yttrium oxide coatings due to its advantages such as strong adhesion between the yttrium oxide coating and the substrate, good shape retention, ability to deposit coatings on complex-shaped parts, and good coating uniformity. In the methods for preparing yttrium oxide coatings by chemical vapor deposition (CVD), existing technologies typically use yttrium acetylacetonate or yttrium triisopropoxylate alone. However, when using yttrium acetylacetonate or yttrium triisopropoxylate alone to prepare yttrium oxide coatings, there are generally problems such as high reaction temperature, low reaction rate, high carbon content, high porosity, high surface roughness, and low adhesion between the yttrium oxide coating and the substrate. Summary of the Invention
[0003] The study found that the specific reasons for the above problems are as follows: For yttrium acetylacetonate (YA), on the one hand, YA has a large molecular weight and high vapor viscosity, which easily forms a thick boundary layer on the substrate surface, hindering the diffusion of reactive gases such as oxygen to the substrate surface, resulting in incomplete oxidation reaction and a low reaction rate; on the other hand, YA contains a stable six-membered ring chelate structure, which is not easily oxidized and broken in an oxygen atmosphere, thus requiring the reaction temperature to be increased to above 1000℃. However, excessively high reaction temperatures not only increase energy consumption but also reduce the adhesion between the resulting yttrium oxide coating and the substrate, thereby increasing the risk of cracking and peeling of the yttrium oxide coating; at the same time, the combined effect of the above two aspects makes YA easily undergo incomplete pyrolysis during the pyrolysis process, resulting in high carbon content, porosity, and surface roughness of the yttrium oxide coating; for triisopropoxy yttrium, due to the high metal-oxygen bond energy (Y–O) in triisopropoxy yttrium, and the three The isopropoxy group in yttrium isopropoxy exhibits significant steric hindrance (steric hindrance refers to the phenomenon where a large group in a molecule hinders a chemical reaction in space), which prevents the yttrium atoms in triisopropoxy yttrium from approaching the substrate surface. This hinders the adsorption and decomposition reactions of triisopropoxy yttrium on the substrate surface, resulting in a low reaction rate when using triisopropoxy yttrium alone to deposit yttrium oxide coatings. Therefore, to improve the reaction rate, the reaction temperature for depositing yttrium oxide coatings using triisopropoxy yttrium alone often needs to reach above 1000℃. However, excessively high reaction temperatures not only increase energy consumption but also reduce the adhesion between the obtained yttrium oxide coating and the substrate, thereby increasing the risk of cracking and peeling of the yttrium oxide coating. At the same time, triisopropoxy yttrium has a loose structure and is easily volatile, but the volatilization rate is unstable, and carbon soot residue is easily generated during pyrolysis. This results in a high carbon content, porosity, and surface roughness of the yttrium oxide coating prepared using triisopropoxy yttrium alone.
[0004] To address the problems encountered in existing technologies for depositing yttrium oxide using yttrium acetylacetonate or yttrium triisopropoxy as precursors, such as high reaction temperature, low reaction rate, high carbon content, porosity, surface roughness, and low adhesion between the yttrium oxide coating and the substrate, this invention provides a method for preparing a yttrium oxide coating. This method dilutes the vapor viscosity of yttrium acetylacetonate, increases the reaction rate, promotes the oxidative breakage of the six-membered ring chelate structure in yttrium acetylacetonate, lowers the reaction temperature, and improves the coating's overall performance. The method of this invention not only enhances the bonding strength with the substrate but also promotes the complete pyrolysis of yttrium acetylacetonate, reducing the carbon content, porosity, and surface roughness of the yttrium oxide coating. Simultaneously, the method reduces the activation energy required for YO bond cleavage in triisopropoxyyttrium and enables triisopropoxyyttrium to be adsorbed and decomposed on the substrate surface without overcoming the steric hindrance of propoxyyttrium, thereby increasing the reaction rate, lowering the reaction temperature, and reducing carbon soot residue during the yttrium oxide coating deposition process, thus reducing the carbon content, porosity, and surface roughness of the yttrium oxide coating.
[0005] To achieve the above objectives, the present invention provides a method for preparing a yttrium oxide coating, comprising: mixing a first gaseous precursor, a second gaseous precursor, and an oxygen-containing gas to form a mixed gas, wherein the mixed gas makes a first contact with a substrate, the first gaseous precursor comprising yttrium acetylacetone, the second gaseous precursor comprising yttrium triisopropoxy, the mass ratio of the first gaseous precursor to the second gaseous precursor being 1:(0.8~1.2), and the conditions for the first contact including a temperature of 800℃~950℃.
[0006] By employing the above technical solution, the present invention has at least the following advantages compared with the prior art: This invention utilizes triisopropoxyyttrium to dilute the vapor viscosity of yttrium acetylacetonate, improving oxygen diffusion efficiency, thereby increasing the reaction rate and reducing the reaction temperature. This is beneficial for reducing energy consumption and enhancing the adhesion between the yttrium oxide coating and the substrate, reducing the risk of cracking and peeling. Furthermore, yttrium acetylacetonate preferentially undergoes partial pyrolysis at 800°C to form active sites, allowing triisopropoxyyttrium to preferentially adsorb onto these sites without overcoming the steric hindrance of isopropoxy groups. The localized activation environment provided by these active sites reduces the activation energy required for YO bond breaking, further increasing the reaction rate and lowering the reaction temperature. Simultaneously, the localized high-temperature region and numerous free radicals generated by the preferential oxidation of triisopropoxyyttrium adsorbed on the active sites can contribute to the six-membered ring chelation structure in yttrium acetylacetonate. The fracture provides heat energy and accelerates its oxidative fracture, allowing it to be fully oxidized into carbon dioxide and water, reducing carbon residue. The six-membered ring structure of yttrium acetylacetonate provides a complete lattice framework for the growth of the yttrium oxide coating, compensating for the loose structure of triisopropoxyyttrium, thereby reducing the carbon content, porosity, and surface roughness of the yttrium oxide coating. Furthermore, the mixing of the two precursors increases the system disorder (entropy increase effect), further lowering the reaction temperature and accelerating the reaction rate. Moreover, this invention specifically controls the mass ratio of the two precursors at 1:(0.8~1.2), which is beneficial for improving the dilution effect and ensuring a uniform gas phase concentration distribution. Controlling the deposition temperature at 800℃~950℃ is beneficial for forming an appropriate number of active sites and improving the adhesion between the yttrium oxide coating and the substrate.
[0007] Other features and advantages of the present invention will be described in detail in the following detailed description section.
[0008] The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of the various ranges, the endpoint values of the various ranges and individual point values, and individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein. Attached Figure Description
[0009] Figure 1 This is a schematic diagram showing the positional relationship between the yttrium oxide coating and the substrate obtained in an embodiment of the present invention. Detailed Implementation
[0010] The following provides a detailed description of specific embodiments of the present invention. It should be understood that the specific embodiments described herein are for illustrative and explanatory purposes only and are not intended to limit the invention. Unless otherwise specified herein, data ranges include endpoints.
[0011] It should be noted that the numerical designations such as "first" and "second" in this disclosure are only used to distinguish different substances or methods of use, and do not represent a difference in order.
[0012] This invention provides a method for preparing a yttrium oxide coating, comprising: mixing a first gaseous precursor, a second gaseous precursor, and an oxygen-containing gas to form a mixed gas, wherein the mixed gas makes a first contact with a substrate, the first gaseous precursor comprising yttrium acetylacetonate, the second gaseous precursor comprising yttrium triisopropoxy, the mass ratio of the first gaseous precursor to the second gaseous precursor being 1:(0.8~1.2) (e.g., 1:0.8, 1:0.9, 1:1, 1:1.1, or 1:1.2), and the conditions for the first contact including a temperature of 800℃~950℃ (e.g., 800℃, 810℃, 820℃, 830℃, 840℃, 850℃, 860℃, 870℃, 880℃, 890℃, 900℃, 910℃, 920℃, 930℃, 940℃, or 950℃).
[0013] In this invention, the first gaseous precursor comprises yttrium acetylacetonate, and the second gaseous precursor comprises yttrium triisopropoxy. The invention mixes the first and second gaseous precursors with an oxygen-containing gas and brings them into initial contact with the substrate. Firstly, yttrium triisopropoxy dilutes the originally high vapor viscosity of yttrium acetylacetonate, thinning the thick edge layer formed by the high vapor viscosity, and improving the diffusion efficiency of oxygen to the substrate surface. This increases the reaction rate while lowering the required reaction temperature. The lower reaction temperature not only reduces the energy consumption required for the reaction but also improves the adhesion between the yttrium oxide coating and the substrate, thereby reducing the risk of cracking and peeling of the yttrium oxide coating. Furthermore, compared to triisopropoxyyttrium, yttrium acetylacetonate preferentially undergoes partial pyrolysis at 800℃, releasing highly reactive yttrium-containing intermediates. These intermediates preferentially form active sites on the matrix surface. These active sites have a higher chemical affinity for the yttrium atoms in triisopropoxyyttrium, allowing triisopropoxyyttrium to preferentially adsorb onto the active sites without overcoming the steric hindrance of the isopropoxy group. Subsequent decomposition reactions then occur at these active sites. Moreover, the local activation environment provided by these active sites reduces the activation energy required for YO bond breaking, thereby increasing the reaction rate and lowering the required reaction temperature. Simultaneously, the triisopropoxyyttrium adsorbed on the active sites… The isopropoxy group in the yttrium isopropoxy structure is rich in CH bonds. In an oxygen-containing atmosphere, it preferentially oxidizes compared to the C / C bond-rich six-membered ring chelate structure in yttrium acetylacetone, releasing more heat. This creates a localized high-temperature zone in the reaction chamber, generating a large number of free radicals (e.g., ·OH, ·O). This localized high-temperature zone provides the necessary heat energy for the breakage of the six-membered ring chelate structure in yttrium acetylacetone, further reducing the required reaction temperature. Simultaneously, the free radicals can abstract H or O from the six-membered ring chelate structure in yttrium acetylacetone to accelerate its oxidative breakage, allowing the resulting fragments to be completely oxidized to carbon dioxide and water by oxygen. This promotes the complete pyrolysis of yttrium acetylacetone, reducing or even eliminating carbon residue, thereby lowering the oxygen content. The carbon content, porosity, and surface roughness of the yttrium oxide coating are reduced. Furthermore, the stable six-membered ring chelate structure in yttrium acetylacetonate provides a complete lattice framework for the growth of the yttrium oxide coating, guiding the orderly incorporation of yttrium species generated by the decomposition of triisopropoxyyttrium into the lattice. This compensates for the defect of soot residue easily generated due to the loose structure of triisopropoxyyttrium, thereby reducing the carbon content, porosity, and surface roughness of the prepared yttrium oxide coating. In addition, the mixing of triisopropoxyyttrium and yttrium acetylacetonate increases the disorder of the system (entropy increase effect), making it easier for triisopropoxyyttrium and yttrium acetylacetonate to obtain sufficient energy distribution to cross the energy barrier, thereby further reducing the reaction temperature required for the reaction and further accelerating the reaction rate.
[0014] This invention controls the mass ratio of the first gaseous precursor to the second gaseous precursor within the aforementioned range. This improves the dilution effect of triisopropoxyyttrium on the vapor viscosity of yttrium acetylacetonate, thereby better reducing the thick edge layer formed by the high vapor viscosity of yttrium acetylacetonate, further improving the diffusion efficiency of oxygen to the substrate surface, increasing the reaction rate, and lowering the reaction temperature required for the reaction. Simultaneously, the aforementioned range allows for a more uniform concentration distribution of the two precursors in the gas phase, which helps reduce the carbon content, porosity, and surface roughness of the resulting yttrium oxide coating. A mass ratio that is too high or too low is detrimental to the uniform concentration distribution of the two precursors in the gas phase, thus hindering the reduction of the carbon content, porosity, and surface roughness of the resulting yttrium oxide coating.
[0015] In this invention, the temperature of the first contact is controlled at 800℃~950℃. Yttrium acetylacetonate can undergo partial pyrolysis to generate active sites on the substrate surface, allowing triisopropoxy yttrium to complete subsequent decomposition reactions at these active sites. Simultaneously, the triisopropoxy yttrium adsorbed on the active sites will preferentially oxidize, releasing a large amount of heat and generating a large number of free radicals. This heat and free radicals can moderately break the six-membered ring chelate structure of yttrium acetylacetonate and fully oxidize it, thereby reducing the carbon content, porosity, and surface roughness of the obtained yttrium oxide coating. Moreover, the above temperature range improves the adhesion between the obtained yttrium oxide coating and the substrate, which helps to reduce the risk of cracking and peeling of the yttrium oxide coating. When the temperature of the first contact is below 800°C, the pyrolysis of yttrium acetylacetonate and yttrium triisopropoxy is insufficient, which is not conducive to reducing the carbon content, porosity and surface roughness of the obtained yttrium oxide coating. When the temperature of the first contact is above 950°C, it will not only increase the energy consumption required for the reaction, but also be not conducive to improving the bonding force between the obtained yttrium oxide coating and the substrate, and not conducive to reducing the risk of cracking and peeling of the yttrium oxide coating.
[0016] In one example, the first gaseous precursor is obtained by heating a first solid precursor. When the first solid precursor is yttrium acetylacetonate solid, the temperature at which it is heated to form the yttrium acetylacetonate gaseous precursor is 160°C to 180°C (e.g., 160°C, 162°C, 164°C, 166°C, 168°C, 170°C, 172°C, 174°C, 176°C, 178°C, or 180°C).
[0017] In one example, the flow rate of the first gaseous precursor in the mixed gas is 0.3 g / h to 0.45 g / h (e.g., 0.3 g / h, 0.31 g / h, 0.32 g / h, 0.33 g / h, 0.34 g / h, 0.35 g / h, 0.36 g / h, 0.37 g / h, 0.38 g / h, 0.39 g / h, 0.40 g / h, 0.41 g / h, 0.42 g / h, 0.43 g / h, 0.44 g / h or 0.45 g / h).
[0018] In one example, the second gaseous precursor is obtained by heating a second solid precursor. When the second solid precursor is triisopropoxyyttrium solid, the temperature at which it is heated to triisopropoxyyttrium gaseous precursor is 170°C to 190°C (e.g., 170°C, 172°C, 174°C, 176°C, 178°C, 180°C, 182°C, 184°C, 186°C, 188°C, or 190°C).
[0019] In one example, the flow rate of the second gaseous precursor in the mixed gas is 0.2 g / h to 0.55 g / h (e.g., 0.2 g / h, 0.22 g / h, 0.24 g / h, 0.26 g / h, 0.28 g / h, 0.3 g / h, 0.32 g / h, 0.34 g / h, 0.36 g / h, 0.38 g / h, 0.4 g / h, 0.42 g / h, 0.44 g / h, 0.46 g / h, 0.48 g / h, 0.5 g / h, 0.52 g / h, or 0.55 g / h).
[0020] In one example, the sum of the flow rates of the first gaseous precursor and the second gaseous precursor is 0.5 g / h to 1.0 g / h (e.g., 0.5 g / h, 0.6 g / h, 0.7 g / h, 0.8 g / h, 0.9 g / h, or 1.0 g / h). Controlling the sum of the flow rates of the first and second gaseous precursors within this range ensures a moderate total amount of precursor entering the reaction chamber per unit time. This helps reduce or even avoid side reactions caused by excessively high precursor concentrations in the gas phase (excessive concentrations can trigger homogeneous nucleation in the gas phase), thereby further reducing the carbon content, porosity, and surface roughness of the resulting yttrium oxide coating.
[0021] In one example, the oxygen-containing gas includes an inert gas and oxygen, and the inert gas includes at least one of argon and nitrogen.
[0022] In one example, the volume ratio of the inert gas to the oxygen is (5~8):1 (e.g., 5:1, 6:1, 7:1, or 8:1). Controlling the volume ratio of the inert gas to the oxygen within this range ensures a moderate oxygen partial pressure in the gas phase, which facilitates further and more complete oxidation of the first and second gaseous precursors. This, in turn, helps to further reduce the carbon content, porosity, and surface roughness of the resulting yttrium oxide coating. Conversely, if the volume ratio of the inert gas to the oxygen is too high, the oxygen partial pressure in the gas phase is insufficient, hindering the further and more complete oxidation of the first and second gaseous precursors. This can easily lead to carbon residue, which is detrimental to further reducing the carbon content, porosity, and surface roughness of the resulting yttrium oxide coating. When the volume ratio of the inert gas to the oxygen is too low, the yttrium oxide coating is prone to over-oxidation during the deposition process, which will generate a loose oxide layer or peroxide species on the surface of the yttrium oxide coating. This is not conducive to further reducing the carbon content, porosity and surface roughness of the obtained yttrium oxide coating.
[0023] In one example, the volume ratio of the inert gas to the oxygen is (6~7):1.
[0024] In one example, the flow rate of the oxygen-containing gas is 1.45 g / h to 2.2 g / h (e.g., 1.45 g / h, 1.5 g / h, 1.6 g / h, 1.7 g / h, 1.8 g / h, 1.9 g / h, 2 g / h or 2.2 g / h).
[0025] In one example, the flow rate of the mixed gas is 1.95 g / h to 3.2 g / h (e.g., 1.95 g / h, 2 g / h, 2.1 g / h, 2.2 g / h, 2.3 g / h, 2.4 g / h, 2.5 g / h, 2.6 g / h, 2.7 g / h, 2.8 g / h, 2.9 g / h, 3 g / h, 3.1 g / h, or 3.2 g / h). In one instance, the temperature of the first contact is 850°C to 900°C.
[0026] In one instance, the temperature of the first contact varies from -1°C to 1°C (e.g., -1°C, 0°C, or 1°C).
[0027] In one example, the first contact takes place in a reaction chamber, with the substrate located in the reaction chamber, and the first gaseous precursor and the second gaseous precursor each introduced into the reaction chamber independently.
[0028] In one instance, the duration of the first contact is 0.25h to 5h (e.g., 0.25h, 0.5h, 1h, 1.5h, 2h, 2.5h, 3h, 3.5h, 4h, 4.5h or 5h).
[0029] In one example, the pressure of the first contact is 5 kPa to 15 kPa (e.g., 5 kPa, 6 kPa, 7 kPa, 8 kPa, 9 kPa, 10 kPa, 11 kPa, 12 kPa, 13 kPa, 14 kPa, or 15 kPa). Controlling the pressure of the first contact within this range allows the first and second gaseous precursors sufficient residence time on the substrate surface to complete adsorption, surface migration, and reaction processes, thereby further reducing the carbon content, porosity, and surface roughness of the resulting yttrium oxide coating. Simultaneously, this range helps prevent excessive collisions between the first and second gaseous precursors in the gas phase, further reducing or even avoiding particulate byproducts generated during homogeneous nucleation, thus further reducing the carbon content, porosity, and surface roughness of the resulting yttrium oxide coating. When the pressure at the first contact is below 5 kPa, the diffusion rate of the first gaseous precursor and the second gaseous precursor is too fast, which is not conducive to further reducing the carbon content, porosity and surface roughness of the yttrium oxide coating. When the pressure at the first contact is above 15 kPa, the diffusion of the first gaseous precursor and the second gaseous precursor is hindered, which is not conducive to further reducing the carbon content, porosity and surface roughness of the yttrium oxide coating.
[0030] In one instance, the pressure of the first contact is 8 kPa to 12 kPa.
[0031] In one example, the matrix may be selected from one or more of graphite, silicon carbide, and high-temperature alloys.
[0032] In one instance, the substrate was pretreated prior to the first contact.
[0033] According to one specific embodiment, when the substrate is graphite, the substrate pretreatment includes the following steps: (1) Cleaning: Place the graphite substrate in acetone and ultrasonically clean it for 10 to 20 minutes (e.g., 10, 11, 12, 13, 14, 15, 16, 17, 18, 19 or 20 minutes) to remove surface oil; then place it in anhydrous ethanol and ultrasonically clean it for 5 to 15 minutes (e.g., 5, 6, 7, 8, 9, 10, 11, 12, 13, 14 or 15 minutes) to remove residual acetone; finally, at room temperature, purge the surface of the graphite substrate with 99.9% pure nitrogen for 7 to 9 minutes (e.g., 7, 8 or 9 minutes) to dry it. (2) Etching: Place the graphite substrate treated in step (1) into the reaction chamber, introduce hydrogen gas at a flow rate of 60 sccm to 100 sccm (e.g., 60 sccm, 65 sccm, 70 sccm, 75 sccm, 80 sccm, 85 sccm, 90 sccm, 95 sccm or 100 sccm), heat to 1400℃ to 1800℃ (e.g., 1400℃, 1500℃, 1600℃, 1700℃ or 1800℃), and hold at that temperature for 1.5 hours to 2.5 hours (e.g., 1.5 hours, 1.6 hours, 1.7 hours, 1.8 hours, 1.9 hours, 2 hours, 2.1 hours, 2.2 hours, 2.3 hours, 2.4 hours or 2.5 hours) to perform high-temperature hydrogen etching to remove the oxide layer and loose carbon particles on the surface of the graphite substrate. Cool to room temperature and remove the graphite substrate. (3) Activation: Place the graphite substrate treated in step (2) in dilute nitric acid with a mass fraction of 4%~6% (e.g., 4%, 5% or 6%) and soak for 4 minutes to 6 minutes (e.g., 4 minutes, 5 minutes or 6 minutes). After taking it out, rinse it with deionized water until neutral. Finally, at room temperature, blow the surface of the graphite substrate with nitrogen gas of 99.9% purity for 7 minutes to 9 minutes (e.g., 7 minutes, 8 minutes or 9 minutes) to dry it, thus completing the pretreatment of the graphite substrate.
[0034] According to another specific embodiment of the present invention, when the substrate is silicon carbide, the pretreatment of the substrate includes the following steps: (1) Cleaning: The silicon carbide substrate is ultrasonically cleaned with acetone and anhydrous ethanol for 5 to 15 minutes (e.g., 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes, 10 minutes, 11 minutes, 12 minutes, 13 minutes, 14 minutes or 15 minutes) to remove oil and impurities from the surface of the silicon carbide substrate. After cleaning, the surface of the silicon carbide substrate is dried by blowing with 99.9% pure nitrogen gas at room temperature for 7 to 9 minutes (e.g., 7 minutes, 8 minutes or 9 minutes).
[0035] (2) Oxidation activation: The silicon carbide substrate treated in step (1) is placed in a muffle furnace and heated to 700℃~900℃ in an air atmosphere (e.g., 700℃, 750℃, 800℃, 850℃ or 900℃) and held for 0.5 hours to 2 hours (e.g., 0.5 hours, 1 hour, 1.5 hours or 2 hours) to form a thin silicon dioxide transition layer on the surface of the silicon carbide substrate. After oxidation is completed, the substrate is cooled to room temperature and removed.
[0036] (3) Reduction: Place the silicon carbide substrate treated in step (2) in a reaction chamber, introduce hydrogen gas at a flow rate of 40 sccm to 80 sccm (e.g., 40 sccm, 45 sccm, 50 sccm, 55 sccm, 60 sccm, 65 sccm, 70 sccm, 75 sccm or 80 sccm), heat to 800℃ to 1000℃ (e.g., 800℃, 850℃, 900℃, 950℃ or 1000℃), and keep warm for 0.5 hours to 2 hours (0.5 hours, 0.6 hours, 0.7 hours, 0.8 hours, 1 hour, 1.2 hours, 1.4 hours, 1.6 hours, 1.8 hours or 2 hours) to remove excess silicon dioxide from the surface of the silicon carbide substrate; after reduction, cool to room temperature to complete the pretreatment of the silicon carbide substrate.
[0037] According to another specific embodiment of the present invention, when the matrix is a high-temperature alloy, the pretreatment of the matrix includes the following steps: (1) Cleaning: Place the high-temperature alloy substrate in acetone and ultrasonically clean for 10 to 20 minutes (e.g., 10, 11, 12, 13, 14, 15, 16, 17, 18, 19 or 20 minutes) to remove surface oil stains; then place the high-temperature alloy substrate in deionized water and ultrasonically clean for 5 to 15 minutes (e.g., 5, 6, 7, 8, 9, 10, 11, 12, 13, 14 or 15 minutes) to remove residual acetone; finally, at room temperature, purge the surface of the high-temperature alloy substrate with nitrogen gas of 99.9% purity for 7 to 9 minutes (e.g., 7, 8 or 9 minutes) to dry it.
[0038] (2) Remove oxide layer: Place the high-temperature alloy substrate treated in step (1) in a hydrochloric acid solution with a mass fraction of 5% to 15% (e.g., 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14% or 15%) and soak for 5 to 15 minutes (e.g., 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes, 10 minutes, 11 minutes, 12 minutes, 13 minutes, 14 minutes or 15 minutes) to remove the surface oxide layer; after removal, rinse with deionized water until neutral, and then blow dry the surface of the high-temperature alloy substrate with nitrogen gas of 99.9% purity for 7 to 9 minutes (e.g., 7 minutes, 8 minutes or 9 minutes) at room temperature.
[0039] (3) Passivation: The high-temperature alloy substrate treated in step (2) is placed in a chromic acid solution with a mass fraction of 1% to 5% (e.g., 1%, 2%, 3%, 4% or 5%) and immersed for 2 to 5 minutes (e.g., 2 minutes, 3 minutes, 4 minutes or 5 minutes) to form a passivation film on the substrate surface; after removal, it is rinsed with deionized water and then the surface of the high-temperature alloy substrate is dried by blowing with nitrogen gas of 99.9% purity for 7 to 9 minutes (e.g., 7 minutes, 8 minutes or 9 minutes) at room temperature to complete the pretreatment of the high-temperature alloy substrate.
[0040] According to one specific embodiment of the present invention, the reaction chamber is evacuated before the mixed gas is introduced. Specifically, the reaction chamber is evacuated to 10 °C using a vacuum system. -4 kPa~10 -2 kPa (e.g., 10 kPa) -4 kPa, 10 -3 kPa or 10 - 2 (kPa) removes residual air, water vapor and other impurities from the reaction chamber, providing a clean reaction environment for subsequent deposition reactions.
[0041] According to a specific embodiment of the present invention, before introducing the mixed gas, the pretreated matrix is placed in the reaction chamber, the reaction chamber is heated to 800℃~950℃, the temperature control accuracy is controlled within ±1℃, and the temperature is maintained for 20 minutes~40 minutes to make the temperature of each part of the matrix uniform.
[0042] According to a specific embodiment of the present invention, before introducing the mixed gas, the gas flow control system is activated to introduce oxygen-containing gas, wherein the volume ratio of inert gas to oxygen in the oxygen-containing gas is (5~8):1, the flow rate of the oxygen-containing gas is 1.45g / h~2.2g / h, and the introduction time is 5 minutes~15 minutes, so as to replace the gas in the reaction chamber and eliminate the residual vacuum.
[0043] In one example, after the first contact, while stopping the flow of the first and second gaseous precursors, oxygen-containing gas continues to be introduced at a constant flow rate to cool the reaction chamber to room temperature. The cooling rate does not exceed 10°C / min (e.g., 1°C / min, 2°C / min, 3°C / min, 4°C / min, 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min, or 10°C / min). This slow cooling method further reduces thermal stress caused by excessively rapid cooling, thereby further improving the adhesion between the yttrium oxide coating and the substrate, and further reducing the risk of cracking and peeling of the yttrium oxide coating.
[0044] In one example, the first contact takes place in a reaction chamber, with the substrate located in the reaction chamber, and the first gaseous precursor and the second gaseous precursor each introduced into the reaction chamber independently.
[0045] According to a specific embodiment of the present invention, after deposition and cooling are completed, the obtained yttrium oxide coating undergoes post-treatment, specifically including the following steps: (1) After the reaction chamber has cooled to room temperature, turn off the gas flow control system and vacuum system, open the reaction chamber, and take out the sample with the yttrium oxide coating deposited on it. (2) Place the obtained sample in a muffle furnace and heat it in an air atmosphere to 500°C to 700°C (e.g., 500°C, 550°C, 600°C, 650°C or 700°C) and hold it for 0.5 hours to 2 hours (e.g., 0.5 hours, 1 hour, 1.5 hours or 2 hours) to remove the small amount of organic impurities and carbon residue remaining on the coating surface; (3) Wipe the surface of the sample treated in step (2) with anhydrous ethanol to remove the dust attached to the surface, and the final yttrium oxide coating product is obtained.
[0046] The present invention also provides a yttrium oxide coating prepared by the above method.
[0047] In one example, a schematic diagram illustrating the positional relationship between the yttrium oxide coating prepared by the method described above and the substrate is shown below. Figure 1 As shown.
[0048] In one example, the carbon content of the yttrium oxide coating is ≤0.2wt% (e.g., 0.01wt%, 0.03wt%, 0.05wt%, 0.08wt%, 0.09wt%, 0.11wt%, 0.12wt%, 0.13wt%, 0.14wt%, 0.15wt%, 0.16wt%, 0.17wt%, 0.18wt%, 0.19wt%, 0.2wt%).
[0049] In one example, the porosity of the yttrium oxide coating is ≤2.5% (e.g., 0.1%, 0.3%, 0.5%, 0.7%, 0.9%, 1.1%, 1.3%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%).
[0050] In one example, the surface roughness of the yttrium oxide coating is ≤0.4 μm (e.g., 0.1 μm, 0.15 μm, 0.2 μm, 0.25 μm, 0.3 μm, 0.35 μm or 0.4 μm).
[0051] In one example, the yttrium oxide coating is located on the surface of the substrate, and the bonding strength between the yttrium oxide coating and the substrate is ≥55 MPa (e.g., 55 MPa, 56 MPa, 57 MPa, 58 MPa, 59 MPa, 60 MPa, 61 MPa, 62 MPa, 63 MPa, 64 MPa, 65 MPa, 66 MPa or 67 MPa).
[0052] The present invention will be described in detail below through embodiments. The embodiments described herein are only a part of the embodiments of the present invention, and not all of them. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without inventive effort are within the scope of protection of the present invention.
[0053] Example 1 (1) Matrix pretreatment Before the first contact, the substrate was pretreated by immersing the graphite substrate in acetone and ultrasonically cleaning it for 15 minutes. Then, the graphite substrate was immersed in anhydrous ethanol and ultrasonically cleaned for 10 minutes. Finally, the surface of the graphite substrate was dried by purging with 99.9% pure nitrogen for 8 minutes at room temperature. The cleaned graphite substrate was then placed in a reaction chamber, hydrogen gas was introduced at a flow rate of 80 sccm, and the temperature was raised to 1600℃ and maintained for 2 hours. After cooling to room temperature, the graphite substrate was removed. The removed graphite substrate was then immersed in 5% dilute nitric acid for 5 minutes, rinsed with deionized water until neutral, and then dried by purging with 99.9% pure nitrogen for 8 minutes at room temperature, resulting in the pretreated graphite substrate.
[0054] (2) Precursor preparation Weigh out the first solid precursor (yttrium acetylacetone solid) and the second solid precursor (yttrium triisopropoxy solid), and load them into two separate precursor evaporation furnaces. After sealing the evaporation furnaces, evaporate them to a vacuum level of 10⁻ using a vacuum system. 3 The first solid precursor (yttrium acetylacetone solid) is heated to 170°C in an evaporation furnace to obtain the first gaseous precursor (yttrium acetylacetone). The second solid precursor (yttrium triisopropoxy solid) is heated to 180°C in an evaporation furnace to obtain the second gaseous precursor (yttrium triisopropoxy). The mixture is kept at this temperature for 30 minutes and then set aside for later use.
[0055] (3) CVD deposition process The pretreated matrix was placed on the sample holder in the reaction chamber, and its position was adjusted so that the matrix surface was perpendicular to the airflow direction within the reaction chamber. The reaction chamber was then sealed, and a vacuum was applied to the reaction chamber before introducing the mixed gas. The vacuum system was used to evacuate the reaction chamber to 10 °C. -3kPa, activate the temperature control system to heat the reaction chamber to 875℃ with a temperature control accuracy of ±1℃, hold for 30 minutes to ensure uniform substrate temperature distribution, activate the pressure control system to adjust the reaction pressure to 10kPa, activate the gas flow control system to introduce oxygen-containing gas (oxygen-containing gas includes inert gas (argon) and oxygen, with a volume ratio of inert gas (argon) to oxygen of 6:1 and a flow rate of 1.71g / h), introduce for 10 minutes, open the gas valve of the precursor evaporator to introduce the first gaseous precursor (yttrium acetylacetone) and the second gaseous precursor ( The volatile gases of triisopropoxyyttrium are independently introduced into the reaction chamber. The flow rate of the first gaseous precursor (yttrium acetylacetonate) is 0.4 g / h, and the flow rate of the second gaseous precursor (yttrium triisopropoxyyttrium) is 0.3 g / h (the mass ratio of the first gaseous precursor to the second gaseous precursor is controlled at 1:1 by separately controlling the introduction time of the first and second gaseous precursors). The sum of the flow rates of the first and second gaseous precursors (yttrium acetylacetonate and yttrium triisopropoxyyttrium) is 0.7 g / h, and the flow rate of the mixed gas is 2.41 g / h. The mixed gas is brought into first contact with the matrix at a temperature of 875°C, with a temperature variation range of -1°C to 1°C, for 3 hours, and at a pressure of 10 kPa. After the first contact, the heating switch and gas valve of the precursor evaporator are turned off. While stopping the introduction of the first gaseous precursor (yttrium acetylacetone) and the second gaseous precursor (yttrium triisopropoxy), oxygen-containing gas (argon and oxygen) is introduced at a constant flow rate to cool the reaction chamber to room temperature at a cooling rate of 5°C / min.
[0056] (4) Post-processing After the reaction chamber cools to room temperature, the gas flow control system and vacuum system are turned off, the reaction chamber is opened, the sample with the yttrium oxide coating is taken out, the obtained sample is placed in a muffle furnace, heated to 600°C in an air atmosphere, held for 1 hour, and the sample surface is wiped with anhydrous ethanol to obtain the final yttrium oxide coating product.
[0057] Example 2 group This embodiment illustrates the effect of changing the mass ratio of the first gaseous precursor to the second gaseous precursor on the yttrium oxide coating.
[0058] Example 2a Referring to Example 1, the difference is that the mass ratio of the first gaseous precursor (yttrium acetylacetonate) to the second gaseous precursor (yttrium triisopropoxy) is controlled to be 1:0.8.
[0059] Example 2b Referring to Example 1, the difference is that the mass ratio of the first gaseous precursor (yttrium acetylacetonate) to the second gaseous precursor (yttrium triisopropoxy) is controlled to be 1:1.2.
[0060] Example 3 Group This embodiment illustrates the effect of the sum of the flow rates of the first gaseous precursor and the second gaseous precursor on the yttrium oxide coating.
[0061] Example 3a Referring to Example 1, except that the flow rate of the first gaseous precursor (yttrium acetylacetonate) is 0.3 g / h, the flow rate of the second gaseous precursor (yttrium triisopropoxy) is 0.2 g / h, and the sum of the flow rates of the first gaseous precursor (yttrium acetylacetonate) and the second gaseous precursor (yttrium triisopropoxy) is 0.5 g / h.
[0062] Example 3b Referring to Example 1, except that the flow rate of the first gaseous precursor (yttrium acetylacetonate) is 0.45 g / h, the flow rate of the second gaseous precursor (yttrium triisopropoxy) is 0.55 g / h, and the sum of the flow rates of the first gaseous precursor (yttrium acetylacetonate) and the second gaseous precursor (yttrium triisopropoxy) is 1 g / h.
[0063] Example 4 group This embodiment illustrates the effect of changing the temperature of the first contact on the yttrium oxide coating.
[0064] Example 4a Referring to Example 1, except that the temperature of the first contact is 800°C.
[0065] Example 4b Referring to Example 1, except that the temperature of the first contact is 950°C.
[0066] Example 5 group This embodiment illustrates the effect of changing the pressure at the first contact point on the yttrium oxide coating.
[0067] Example 5a Referring to Example 1, except that the pressure of the first contact is 5 kPa.
[0068] Example 5b Referring to Example 1, except that the pressure of the first contact is 15 kPa.
[0069] Example 6 This embodiment illustrates the effect of changing the volume ratio of inert gas to oxygen on yttrium oxide coatings.
[0070] Example 6a Referring to Example 1, the difference is that the volume ratio of inert gas to oxygen is 5:1.
[0071] Example 6b Referring to Example 1, the difference is that the volume ratio of inert gas to oxygen is 8:1.
[0072] Comparative Example 1a Referring to Example 1, the only difference is that the precursor is the first gaseous precursor (yttrium acetylacetonate).
[0073] Comparative Example 1b Referring to Example 1, the only difference is that the precursor is the second gaseous precursor (triisopropoxyyttrium).
[0074] Comparative Example 2a Referring to Example 1, the difference is that the mass ratio of the first gaseous precursor (yttrium acetylacetonate) to the second gaseous precursor (yttrium triisopropoxy) is 1:0.5.
[0075] Comparative Example 2b Referring to Example 1, the difference is that the mass ratio of the first gaseous precursor (yttrium acetylacetonate) to the second gaseous precursor (yttrium triisopropoxy) is 1:2.
[0076] Comparative Example 3a Referring to Example 1, the difference is that the temperature of the first contact is 780°C.
[0077] Comparative Example 3b Referring to Example 1, the difference is that the temperature of the first contact is 970°C.
[0078] Test case The yttrium oxide coatings prepared by the examples and comparative examples were subjected to the following tests, and the test results are shown in Table 1: 1. Carbon content test Select yttrium oxide coatings with smooth surfaces, free of oil, oxide scale, and surface contaminants, and with a test area size of not less than 10 mm × 10 mm as test samples. Start the GDMS instrument and evacuate to 10 °C. -6The process involves passing high-purity argon gas as the discharge gas, adjusting the argon pressure, discharge current, and sputtering power to a stable state, calibrating the instrument's mass number and sensitivity, and performing quantitative calibration using matrix-matched standard materials or relative sensitivity factor (RSF). The sample is then placed in a dedicated sample holder and positioned in a glow discharge ion source for 5-10 minutes of pre-sputtering to remove adsorbed contaminants and oxide layers from the coating surface. Formal sputtering and detection are then initiated, continuously acquiring ion signal intensities corresponding to different mass-to-charge ratios, recording the ion counts of each isotope, correcting for mass spectrometry interferences (including oxides and double-charged ions) using software, calculating the concentration of each element based on the calibration curve, and generating a test report after testing. This report includes qualitative results, quantitative concentrations, detection limits, and elemental depth distribution curves for each element in the coating. The carbon content is calculated using the difference method, and the results are recorded in Table 1.
[0079] 2. Porosity test Select the magnification (preferably 500x to 5000x) based on the sample coating thickness and pore size, adjust the light source intensity and contrast to ensure that the pores and coating substrate can be clearly distinguished, select multiple representative test areas (surface observation or cross-sectional observation), and acquire microscopic images of the coating. At least 5 to 10 images should be acquired for each sample, covering different test locations. Use image processing software to process the microscopic images, including noise reduction, threshold segmentation, and pore identification. Automatically count the area, number, and average pore diameter of pores in the images, and calculate the ratio of the total pore area to the total area of the test area, which is the coating porosity. Record the results in Table 1.
[0080] 3. Surface roughness test Start the 3D profilometer, calibrate the lens focal length, scanning accuracy and motion platform, set the scanning parameters, the scanning range is 500 μm×500 μm~10 mm×10 mm, the sampling interval is 0.1μm~1μm, fix the sample on the motion platform, align it with the test area, start scanning, continuously collect the three-dimensional height data of the coating surface to form a three-dimensional surface morphology model, perform filtering and noise reduction and point cloud processing through software, calculate the surface roughness parameters, generate a surface roughness analysis report, repeat the test 3~5 times, take the average value as the final test result, and record the results in Table 1.
[0081] 4. Combined strength test Measure the width and thickness of the sample, place the sample on a fixture with a span of 4mm, open the software and connect it online, select the test method as bond strength, set the speed to 0.5mm / min, input the width and thickness of the sample, reset the force, displacement, time, and speed to zero, click start, and the bond strength calculation formula is as follows: In the formula: Rm is the bond strength; FM is the maximum load; A is the cross-sectional area. The results are recorded in Table 1.
[0082] Table 1 As can be seen from Table 1, by comparing the comparative examples and embodiments, firstly, the composite precursor composed of a first gaseous precursor (yttrium acetylacetonate) and a second gaseous precursor (yttrium triisopropoxy) in this invention solves the problems of unstable volatilization and high carbon residue compared to a single precursor. The yttrium oxide coating prepared by the method of this invention has higher adhesion to the substrate, and the prepared yttrium oxide coating has lower carbon content, lower porosity, and lower surface roughness, which can meet the application requirements of high-end fields such as semiconductors and aerospace.
[0083] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combining the various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.
Claims
1. A method for preparing a yttrium oxide coating, characterized in that, include: A first gaseous precursor, a second gaseous precursor, and an oxygen-containing gas are mixed to form a mixed gas. The mixed gas comes into first contact with a matrix. The first gaseous precursor includes yttrium acetylacetone, and the second gaseous precursor includes yttrium triisopropoxy. The mass ratio of the first gaseous precursor to the second gaseous precursor is 1:(0.8~1.2). The conditions for the first contact include a temperature of 800℃~950℃.
2. The method according to claim 1, characterized in that, The flow rate of the first gaseous precursor in the mixed gas is 0.3 g / h to 0.45 g / h; And / or, the flow rate of the second gaseous precursor in the mixed gas is 0.2 g / h to 0.55 g / h.
3. The method according to claim 1, characterized in that, The oxygen-containing gas includes an inert gas and oxygen, and the inert gas includes at least one of argon and nitrogen; And / or, the volume ratio of the inert gas to the oxygen is (5~8):1; And / or, the flow rate of the oxygen-containing gas is 1.45 g / h to 2.2 g / h.
4. The method according to claim 1, characterized in that, The flow rate of the mixed gas is 1.95 g / h to 3.2 g / h; and / or, the sum of the flow rates of the first gaseous precursor and the second gaseous precursor is 0.5 g / h to 1 g / h.
5. The method according to claim 1, characterized in that, The first contact time is 0.25h to 5h, and / or the pressure of the first contact is 5kPa to 15kPa, preferably 8kPa to 12kPa; And / or, the temperature of the first contact is 850°C to 900°C; And / or, the temperature variation range of the first contact is -1℃ to 1℃.
6. The method according to claim 1, characterized in that, The first gaseous precursor is obtained by heating the first solid precursor. When the first solid precursor is yttrium acetylacetone solid, the heating temperature is 160°C to 180°C. And / or, the second gaseous precursor is obtained by heating a second solid precursor, wherein when the second solid precursor is triisopropoxyyttrium solid, the heating temperature is 170°C to 190°C.
7. The method according to any one of claims 1 to 6, characterized in that, The first contact takes place in the reaction chamber, with the substrate located in the reaction chamber, and the first gaseous precursor and the second gaseous precursor are each introduced into the reaction chamber independently; And / or, the matrix may be selected from one or more of graphite, silicon carbide, and high-temperature alloys; And / or, pretreatment of the substrate prior to the first contact.
8. The method according to claim 7, characterized in that, Before introducing the mixed gas, the reaction chamber is evacuated; and / or, after the first contact is completed, while stopping the introduction of the first gaseous precursor and the second gaseous precursor, oxygen-containing gas is continued to be introduced at a constant flow rate to cool the reaction chamber to room temperature at a rate not exceeding 10°C / min.
9. A yttrium oxide coating, characterized in that, The yttrium oxide coating is prepared using the method described in any one of claims 1 to 8.
10. The yttrium oxide coating according to claim 9, characterized in that, The carbon content of the yttrium oxide coating is ≤0.2wt%; And / or, the porosity of the yttrium oxide coating is ≤2.5%; And / or, the surface roughness of the yttrium oxide coating is ≤0.4μm; And / or, the yttrium oxide coating is located on the surface of the substrate, and the bonding strength between the yttrium oxide coating and the substrate is ≥55MPa.